Tungsten-rhenium alloy high-temperature-resistant thermal-shock-resistant coating and preparation method thereof

Through the combination and optimization process of tungsten-rhenium alloy materials and nanomaterials, a high-temperature and thermal shock-resistant coating with high hardness and toughness is prepared, which solves the problems of porosity and peeling of existing coatings in high-temperature environments, and improves performance and lifespan while reducing costs.

CN118726892APending Publication Date: 2024-10-01ZHONGYUAN CRITICAL METAL LAB
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410730827.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing high-temperature and thermal shock-resistant coatings have pores and peeling phenomena during high-temperature combustion and airflow erosion, which affects their mechanical properties, thermal insulation properties, wear resistance and service life, and some coatings have poor thermal shock resistance. There are deficiencies.

Method used

Using tungsten-rhenium alloy material, the coating is prepared by combining boron nitride nanosheets and molybdenum disilicide with nanocrystalline tungsten-rhenium alloy powder, combined with polyphenylene sulfide and polypropylene, using ultrasonic treatment and atmospheric plasma spraying technology to form a high-performance coating. Hard and tough coating to enhance interfacial interaction and bonding.

Benefits of technology

It improves the density, high temperature resistance and thermal shock resistance of the coating, reduces porosity and risk of spalling, extends service life and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004880165000000101
    Figure BDA0004880165000000101
  • Figure BDA0004880165000000111
    Figure BDA0004880165000000111
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and particularly relates to a tungsten-rhenium alloy high-temperature-resistant and thermal-shock-resistant coating and a preparation method thereof.The preparation method comprises the following steps that S1, boron nitride nanosheets and molybdenum disilicide are added into N-methyl pyrrolidone, ultrasonic treatment is conducted, nanosheet dispersion liquid is obtained, nanocrystalline tungsten-rhenium alloy powder is soaked in the nanosheet dispersion liquid, and the nanocrystal tungsten-rhenium alloy powder is obtained; a pretreated tungsten-rhenium alloy matrix is obtained; s2, polyphenylene sulfide is added into absolute ethyl alcohol, then polypropylene and the pretreated tungsten-rhenium alloy matrix are added, and stirring is conducted till sticky slurry is formed; and S3, spraying the slurry to the surface of a metal or alloy matrix by adopting an atmospheric plasma spraying technology to form a coating, and carrying out heat treatment after spraying. The molecular chain structures of polyphenylene sulfide and polypropylene endow the coating with good toughness and mechanical strength, the structure and performance of the coating can be maintained at high temperature, and the thermal shock resistance of the coating in a high-temperature environment can be enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a tungsten-rhenium alloy high-temperature resistant and thermal shock resistant coating and a preparation method thereof. Background Art

[0002] In modern aerospace technology, the application of high temperature resistant and thermal shock resistant coatings is particularly important. With the rapid development of aerospace technology, various aircraft such as supersonic missiles and rockets are flying at high altitudes and high speeds. Their key components such as ultrasonic flame nozzles, rocket nozzles, missile nozzles, and supersonic missile nose cones will be subject to severe challenges in extreme temperature environments. These challenges include but are not limited to high temperature combustion, thermal shock, airflow scouring, and rapid switching between high and low temperatures. The mechanism of high temperature resistant and thermal shock resistant coatings is mainly to resist high temperature, thermal shock, and airflow scouring by forming a layer of material with special properties on the surface of the substrate. This type of coating is usually composed of high temperature resistant ceramic materials or intermetallic compounds, and has good high temperature resistance and thermal shock resistance. In a high temperature environment, the coating can form a dense oxide film, which can effectively isolate the direct thermal erosion of the high temperature gas on the substrate, thereby protecting the substrate from being melted or oxidized by high temperature. The scouring resistance of the coating is due to its high hardness and excellent wear resistance. During high altitude and high speed flight, the key components of the aircraft will be strongly scoured by high-speed airflow. High temperature and thermal shock resistant coatings can effectively resist the erosion of such airflows and maintain the integrity and stable performance of components through their high hardness and wear resistance. In addition, in high altitude and low temperature environments, the coating also needs to have good low temperature resistance. This requires that the coating material will not become brittle or its performance will not degrade under low temperature conditions to ensure the safe flight of the aircraft. When the aircraft returns to the atmosphere, it will experience rapid switching between high and low temperatures, which places higher requirements on the performance of the coating, requiring the coating to be able to withstand such rapid temperature changes without cracking or peeling.

[0003] In the prior art, the coating has pores and peeling poisoning phenomena during high-temperature combustion and airflow scouring, which affects the life of the coating. Porosity is a structural defect in the coating, which will affect the mechanical properties, thermal insulation properties, wear resistance and corrosion resistance of the coating. The pores inside the coating will form blind holes, while the pores on the surface of the coating may form open holes. If the pores run through the entire coating, through holes will be formed. The presence of pores will seriously affect the service life and performance of the coating. In addition, under high temperatures and extreme environments, the bonding force between the coating and the substrate will be affected, causing the coating to peel off or crack, affecting the service life and performance stability of the coating. At the same time, some high-temperature resistant and thermal shock resistant coatings may still be limited in certain specific properties. For example, zirconium dioxide series coatings exhibit good performance at high temperatures, but are not ideal in terms of thermal shock resistance. Summary of the invention

[0004] The object of the present invention is to provide a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating and a preparation method thereof in view of the deficiencies in the prior art.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a tungsten-rhenium alloy high-temperature resistant and thermal shock resistant coating comprises the following steps:

[0007] S1. Add boron nitride nanosheets and molybdenum disilicide to N-methylpyrrolidone, perform ultrasonic treatment using an ultrasonic processor to obtain a nanosheet dispersion, immerse the nanocrystalline tungsten-rhenium alloy powder in the nanosheet dispersion, stir at a speed of 400-600 rpm for 2-3 hours, let stand for 12-16 hours, filter, wash with deionized water for 3-5 times, and dry to constant weight to obtain a pretreated tungsten-rhenium alloy matrix;

[0008] S2, adding polyphenylene sulfide to anhydrous ethanol, and then adding polypropylene and the pretreated tungsten-rhenium alloy matrix, and using a high-speed stirrer to mix at a speed of 2000-3000 rpm to form a uniform and viscous slurry;

[0009] S3. Use atmospheric plasma spraying technology to spray the slurry onto the surface of the metal or alloy substrate to form a coating. After spraying, place it in a vacuum or argon atmosphere, heat treat it at 1250-1350℃, keep it warm for 3-4h, cool it down to 80℃, keep it warm for 1-2h, the cooling rate is 5-10℃ / min, and cool it to room temperature to obtain a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating.

[0010] Furthermore, in step S1, the amount ratio of boron nitride nanosheets, molybdenum disilicide and N-methylpyrrolidone is (5-8) g: (3-4) g: (100-120) mL, and the amount ratio of nanocrystalline tungsten-rhenium alloy powder and nanosheet dispersion is (2-6) g: (50-60) mL.

[0011] The nanocrystalline tungsten-rhenium alloy powder in step S1 is prepared by the following steps: uniformly mixing tungsten powder and rhenium powder in an agate mortar, grinding for 10-20 minutes, transferring to a ball mill, adding 10-20 hard alloy ball milling beads with a diameter of 5 mm, adding anhydrous ethanol, and ball milling at a speed of 300-400 rpm for 4-6 hours, changing the ball milling direction every 30 minutes, after the ball milling, taking out the powder and placing it in a ventilated place to dry naturally for 12-24 hours, sieving with a 200-mesh sieve, placing it in a tubular furnace, heating it to 800-900° C. at a rate of 5° C. / min in an argon atmosphere, keeping it warm for 2-4 hours, and cooling it to room temperature to obtain the nanocrystalline tungsten-rhenium alloy powder.

[0012] The frequency of the ultrasonic treatment in step S1 is 40-50 kHz, and the dispersion time of the ultrasonic treatment is 20-30 min.

[0013] In the step S2, the usage ratio of polyphenylene sulfide, anhydrous ethanol, polypropylene and pretreated tungsten-rhenium alloy substrate is (0.2-0.5) g: (100-200) mL: (12-18) g: (6-9) g.

[0014] The spraying power in step S2 is 45-55 kW, the gas flow rate of argon is 55-60 L / min, the gas flow rate of hydrogen is 12-18 L / min, and the coating thickness is 300-400 μm.

[0015] The usage ratio of the tungsten powder, rhenium powder and anhydrous ethanol is (10-15) g: (2-3) g: (30-50) mL.

[0016] The alloy matrix is ​​a tungsten-rhenium alloy, and the composition is W: 3.8-4.2%, Re: 0.35-0.45% and HFCs: 0.01%.

[0017] According to another aspect of the present invention, a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating prepared by the above preparation method is provided.

[0018] Beneficial effects of the present invention:

[0019] 1. In the technical solution of the present invention, boron nitride and molybdenum disilicide have low surface energy, which helps them to be evenly dispersed in N-methylpyrrolidone. At the same time, the low surface energy also promotes the wetting between the nanosheets and the tungsten-rhenium alloy powder, so that the nanosheets can be tightly attached to the powder surface. The interface area between the nanosheets and the tungsten-rhenium alloy powder is the key to the performance of the coating. The introduction of nanosheets increases the interface area, thereby enhancing the interface interactions such as van der Waals forces and hydrogen bonds, which helps to enhance the overall strength of the coating. The small size of the nanosheets allows the tiny gaps between the tungsten-rhenium alloy powders to be filled, reducing the porosity in the coating, which not only improves the density of the coating, but also reduces the heat conduction path, thereby improving the high temperature resistance of the coating.

[0020] 2. In the technical solution of the present invention, the molecular chain structure of polyphenylene sulfide and polypropylene gives the coating good toughness and mechanical strength. At high temperatures, the molecular chain can maintain a certain fluidity, thereby absorbing and dispersing thermal stress and reducing the risk of cracking of the coating. Polyphenylene sulfide and polypropylene have high thermal stability and can maintain their structure and performance at high temperatures, which helps to enhance the thermal shock resistance of the coating in high temperature environments. The interaction between polyphenylene sulfide and polypropylene and tungsten-rhenium alloy powder may form a composite structure, which enhances the internal bonding force of the coating at a microscopic level, making the coating more stable at high temperatures and reducing the risk of peeling and cracking. Polyphenylene sulfide and polypropylene have good interface compatibility with tungsten-rhenium alloy powder, which helps to reduce interface defects and improve the overall performance of the coating. At the same time, it reduces the cost of high-temperature resistant and thermal shock resistant coatings, which has certain economic benefits. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] The nanocrystalline tungsten-rhenium alloy powder is prepared by the following steps: 100 g of tungsten powder and 20 g of rhenium powder are uniformly mixed in an agate mortar, ground for 10 minutes, transferred to a ball mill, 10 hard alloy ball milling beads with a diameter of 5 mm are added, and then 300 mL of anhydrous ethanol is added, and the mixture is ball milled at a speed of 300 rpm for 4 hours, and the ball milling direction is changed every 30 minutes. After the ball milling is completed, the powder is taken out and placed in a ventilated place for natural drying for 12 hours, sieved with a 200-mesh screen, placed in a tubular furnace, and heated to 800° C. at a rate of 5° C. / min in an argon atmosphere, kept warm for 2 hours, and cooled to room temperature to obtain the nanocrystalline tungsten-rhenium alloy powder.

[0024] Example 2

[0025] The nanocrystalline tungsten-rhenium alloy powder is prepared by the following steps: 125 g of tungsten powder and 25 g of rhenium powder are uniformly mixed in an agate mortar, ground for 15 minutes, transferred to a ball mill, 15 hard alloy ball milling beads with a diameter of 5 mm are added, and then 400 mL of anhydrous ethanol is added, and the mixture is ball milled at a speed of 350 rpm for 5 hours, and the ball milling direction is changed every 30 minutes. After the ball milling is completed, the powder is taken out and placed in a ventilated place for natural drying for 18 hours, sieved with a 200-mesh screen, placed in a tubular furnace, and heated to 850° C. at a rate of 5° C. / min in an argon atmosphere, kept warm for 3 hours, and cooled to room temperature to obtain the nanocrystalline tungsten-rhenium alloy powder.

[0026] Example 3

[0027] The nanocrystalline tungsten-rhenium alloy powder is prepared by the following steps: 150 g of tungsten powder and 30 g of rhenium powder are uniformly mixed in an agate mortar, ground for 20 minutes, transferred to a ball mill, 20 hard alloy ball milling beads with a diameter of 5 mm are added, and then 500 mL of anhydrous ethanol is added, and the mixture is ball milled at a speed of 400 rpm for 6 hours, and the ball milling direction is changed every 30 minutes. After the ball milling is completed, the powder is taken out and placed in a ventilated place for natural drying for 24 hours, sieved with a 200-mesh screen, placed in a tubular furnace, heated to 900° C. at a rate of 5° C. / min in an argon atmosphere, kept warm for 4 hours, and cooled to room temperature to obtain the nanocrystalline tungsten-rhenium alloy powder.

[0028] Example 4

[0029] A method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating, characterized in that it comprises the following steps:

[0030] S1, adding 50g of boron nitride nanosheets and 30g of molybdenum disilicide to 1000mL of N-methylpyrrolidone, using an ultrasonic processor for ultrasonic treatment, the ultrasonic frequency is 40kHz, disperse for 20min, to obtain a nanosheet dispersion, immersing 20g of the nanocrystalline tungsten-rhenium alloy powder obtained in Example 1 in 500mL of the nanosheet dispersion, stirring at a speed of 400rpm for 2h, and then standing for 12h, filtering, washing with deionized water 3 times, and drying to constant weight to obtain a pretreated tungsten-rhenium alloy matrix;

[0031] S2, adding 2 g of polyphenylene sulfide to 1000 mL of anhydrous ethanol, and then adding 120 g of polypropylene and 60 g of pretreated tungsten-rhenium alloy matrix, and mixing at a speed of 2000 rpm using a high-speed stirrer to form a uniform and viscous slurry;

[0032] S3. Use atmospheric plasma spraying technology to spray the slurry onto the surface of the tungsten-rhenium alloy substrate to form a coating. The power is 45kW, the gas flow rate of argon is 55L / min, the gas flow rate of hydrogen is 12L / min, the feed rate is 25g / min, and the coating thickness is 300μm. After spraying, place it in a vacuum or argon atmosphere, heat treat at 1250℃, keep it warm for 3h, cool it down to 80℃, keep it warm for 1h, the cooling rate is 5℃ / min, and cool it to room temperature to obtain a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating.

[0033] Example 5

[0034] A method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating, characterized in that it comprises the following steps:

[0035] S1, adding 75g of boron nitride nanosheets and 35g of molybdenum disilicide to 1100mL of N-methylpyrrolidone, using an ultrasonic processor for ultrasonic treatment, the ultrasonic frequency is 45kHz, dispersed for 25min, to obtain a nanosheet dispersion, immersing 40g of the nanocrystalline tungsten-rhenium alloy powder obtained in Example 2 in 55mL of the nanosheet dispersion, stirring at a speed of 500rpm for 2.5h, and then standing for 14h, filtering, washing with deionized water 4 times, and drying to constant weight to obtain a pretreated tungsten-rhenium alloy matrix;

[0036] S2, adding 4 g of polyphenylene sulfide to 1500 mL of anhydrous ethanol, and then adding 150 g of polypropylene and 75 g of pretreated tungsten-rhenium alloy matrix, and mixing at a speed of 2500 rpm using a high-speed stirrer to form a uniform and viscous slurry;

[0037] S3. Use atmospheric plasma spraying technology to spray the slurry onto the surface of the tungsten-rhenium alloy substrate to form a coating. The power is 50kW, the gas flow rate of argon is 55L / min, the gas flow rate of hydrogen is 15L / min, the feed rate is 27g / min, and the coating thickness is 350μm. After spraying, place it in a vacuum or argon atmosphere, heat treat it at 1300℃, keep it warm for 3.5h, cool it down to 80℃, keep it warm for 1.5h, the cooling rate is 5℃ / min, and cool it to room temperature to obtain a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating.

[0038] Example 6

[0039] A method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating, characterized in that it comprises the following steps:

[0040] S1, adding 80g of boron nitride nanosheets and 40g of molybdenum disilicide to 1200mL of N-methylpyrrolidone, using an ultrasonic processor for ultrasonic treatment, the ultrasonic frequency is 50kHz, and the dispersion is carried out for 30min to obtain a nanosheet dispersion liquid, and 60g of the nanocrystalline tungsten-rhenium alloy powder prepared in Example 3 is immersed in 600mL of the nanosheet dispersion liquid, stirred at a speed of 600rpm for 3h, and then allowed to stand for 16h, filtered, washed with deionized water 5 times, and dried to constant weight to obtain a pretreated tungsten-rhenium alloy matrix;

[0041] S2, adding 5 g of polyphenylene sulfide to 2000 mL of anhydrous ethanol, and then adding 180 g of polypropylene and 90 g of pretreated tungsten-rhenium alloy matrix, and using a high-speed stirrer to mix at a speed of 3000 rpm to form a uniform and viscous slurry;

[0042] S3. Use atmospheric plasma spraying technology to spray the slurry onto the surface of the tungsten-rhenium alloy substrate to form a coating. The power is 55kW, the gas flow rate of argon is 60L / min, the gas flow rate of hydrogen is 18L / min, the feed rate is 30g / min, and the coating thickness is 400μm. After spraying, place it in a vacuum or argon atmosphere, heat treat at 1350℃, keep it warm for 4h, cool it down to 80℃, keep it warm for 2h, the cooling rate is 10℃ / min, and cool it to room temperature to obtain a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating.

[0043] Comparative Example 1

[0044] The difference between this comparative example and Example 4 is that polyethylene is used instead of polyphenylene sulfide, and the remaining steps are the same as those of Example 4, namely:

[0045] S1, adding 50g of boron nitride nanosheets and 30g of molybdenum disilicide to 1000mL of N-methylpyrrolidone, using an ultrasonic processor for ultrasonic treatment, the ultrasonic frequency is 40kHz, disperse for 20min, to obtain a nanosheet dispersion, immersing 20g of the nanocrystalline tungsten-rhenium alloy powder obtained in Example 1 in 500mL of the nanosheet dispersion, stirring at a speed of 400rpm for 2h, and then standing for 12h, filtering, washing with deionized water 3 times, and drying to constant weight to obtain a pretreated tungsten-rhenium alloy matrix;

[0046] S2, add 2g polyethylene into 1000mL anhydrous ethanol, then add 120g polypropylene and 60g pretreated tungsten-rhenium alloy matrix, and use a high-speed stirrer to mix at a speed of 2000rpm to form a uniform and viscous slurry;

[0047] S3. Use atmospheric plasma spraying technology to spray the slurry onto the surface of the tungsten-rhenium alloy substrate to form a coating. The power is 45kW, the gas flow rate of argon is 55L / min, the gas flow rate of hydrogen is 12L / min, the feed rate is 25g / min, and the coating thickness is 100μm. After spraying, place it in a vacuum or argon atmosphere, heat treat at 1250℃, keep it warm for 3h, cool it down to 80℃, keep it warm for 1h, cool it down at a rate of 5℃ / min, and cool it to room temperature.

[0048] Comparative Example 2

[0049] The difference between this comparative example and Example 5 is that in step S2, only the pretreated tungsten-rhenium alloy substrate is added to anhydrous ethanol, and the remaining steps are the same as those in Example 5, namely:

[0050] S1, adding 75g of boron nitride nanosheets and 35g of molybdenum disilicide to 1100mL of N-methylpyrrolidone, using an ultrasonic processor for ultrasonic treatment, the ultrasonic frequency is 45kHz, dispersed for 25min, to obtain a nanosheet dispersion, immersing 40g of the nanocrystalline tungsten-rhenium alloy powder obtained in Example 2 in 55mL of the nanosheet dispersion, stirring at a speed of 500rpm for 2.5h, and then standing for 14h, filtering, washing with deionized water 4 times, and drying to constant weight to obtain a pretreated tungsten-rhenium alloy matrix;

[0051] S2, adding 75g of the pretreated tungsten-rhenium alloy matrix into 1500mL of anhydrous ethanol, and mixing with a high-speed stirrer at a speed of 2500rpm until a uniform and viscous slurry is formed;

[0052] S3. Use atmospheric plasma spraying technology to spray the slurry onto the surface of the tungsten-rhenium alloy substrate to form a coating. The power is 50kW, the gas flow rate of argon is 55L / min, the gas flow rate of hydrogen is 15L / min, the feed rate is 27g / min, and the coating thickness is 150μm. After spraying, place it in a vacuum or argon atmosphere, heat treat it at 1300℃, keep it warm for 3.5h, cool it down to 80℃, keep it warm for 1.5h, cool it down at a rate of 5℃ / min, and cool it to room temperature.

[0053] The coating samples prepared in Examples 4-6 and Comparative Examples 1-2 were subjected to thermal shock tests. All coating samples were placed in a high-temperature furnace, heated to 2000°C, and kept warm for 5 minutes, and quickly cooled to liquid nitrogen. The above heating and quenching process was repeated 10 times to simulate the thermal shock environment of the spacecraft. The surface conditions of each sample after the thermal shock test were observed and recorded, including crack conditions, peeling conditions, and hardness retention rate, where hardness retention rate = (hardness value after treatment / initial hardness value) × 100%. The results are shown in Table 1:

[0054] Table 1. Thermal shock test results of Examples 4-6 and Comparative Examples 1-2

[0055]

[0056]

[0057] As can be seen from Table 1, Examples 4-6 did not show cracks after the thermal shock test, which may be due to the high melting point characteristics of the nanocrystalline tungsten-rhenium alloy powder, which enhances the high temperature resistance of the coating. The nanocrystalline structure also provides better thermal stability and deformation resistance, so it can effectively resist the thermal stress caused by rapid temperature changes and prevent the generation of cracks. In contrast, cracks appeared in the coatings of Comparative Examples 1 and 2, probably because their material composition and structure do not have the same high temperature resistance and deformation resistance, resulting in the inability to effectively cope with thermal stress under rapid thermal shock conditions, thereby generating cracks. The crack situation in Comparative Example 2 is the most serious, which may be related to the uneven stress distribution inside the coating or the poor compatibility between the materials.

[0058] The coatings of Examples 4 and 5 did not peel off, indicating that the bonding force between the coating and the substrate in the examples is strong and can effectively resist the peeling force during the thermal shock process. The slight peeling in Example 6 may be caused by a slight difference in coating thickness or material ratio. The coatings of Comparative Examples 1 and 2 peeled off significantly, which is probably because the bonding between the coating and the substrate is not strong enough, or the stress accumulation inside the coating causes the separation of the coating.

[0059] The high hardness retention rates of Examples 4-6 indicate that the mechanical properties of the coatings can be well maintained even under extreme thermal shock conditions. This is mainly due to the synergistic effect of nanocrystalline tungsten-rhenium alloy powder, boron nitride nanosheets, and molybdenum disilicide, which not only enhances the hardness of the coatings, but also improves their wear resistance and impact resistance. The lower hardness retention rates of Comparative Examples 1 and 2 indicate that the mechanical properties of these coatings are greatly affected during the thermal shock process, which may be related to the insufficient thermal shock resistance of the material or the instability of the coating structure.

[0060] In summary, the reason why the tungsten-rhenium alloy coatings prepared in Examples 4-6 performed well in the thermal shock test is that the addition of nanomaterials enhances the high temperature resistance, deformation resistance and mechanical properties of the coatings, while the optimized preparation process ensures a firm bond between the coatings and the substrate.

[0061] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0062] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a high temperature resistant and thermal shock resistant coating of tungsten-rhenium alloy, characterized in that: The following steps are involved: S1. Add boron nitride nanosheets and molybdenum disilicide to N-methylpyrrolidone, perform ultrasonic treatment using an ultrasonic processor to obtain a nanosheet dispersion, immerse the nanocrystalline tungsten-rhenium alloy powder in the nanosheet dispersion, stir at a speed of 400-600 rpm for 2-3 hours, and then stand for 12-16 hours to obtain a pre-treated dispersion; S2, adding polyphenylene sulfide to anhydrous ethanol, and then adding polypropylene and pre-treated dispersion, and using a high-speed stirrer to mix at a speed of 2000-3000 rpm to form a uniform and viscous slurry; S3. Use atmospheric plasma spraying technology to spray the slurry onto the surface of the alloy substrate to form a coating. After spraying, place it in a vacuum or argon atmosphere, heat treat it at 1250-1350℃, keep it warm for 3-4h, cool it down to 80℃, keep it warm for 1-2h, the cooling rate is 5-10℃ / min, and cool it to room temperature to obtain a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating.

2. The method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating according to claim 1, characterized in that: In step S1, the dosage ratio of boron nitride nanosheets, molybdenum disilicide and N-methylpyrrolidone is (5-8) g: (3-4) g: (100-120) mL.

3. The method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating according to claim 1, characterized in that: The nanocrystalline tungsten-rhenium alloy powder in step S1 is prepared by the following steps: tungsten powder and rhenium powder are uniformly mixed in an agate mortar, ground for 10-20 minutes, transferred to a ball mill, 10-20 hard alloy ball milling beads with a diameter of 5 mm are added, and then anhydrous ethanol is added, and the ball milling is performed at a speed of 300-400rpm for 4-6 hours, and the ball milling direction is changed every 30 minutes. After the ball milling is completed, the powder is taken out and placed in a ventilated place for natural drying for 12-24 hours, sieved with a 200-mesh screen, placed in a tubular furnace, and heated to 800-900°C at a rate of 5°C / min in an argon atmosphere, kept warm for 2-4 hours, and cooled to room temperature to obtain the nanocrystalline tungsten-rhenium alloy powder.

4. The method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating according to claim 1, characterized in that: The frequency of the ultrasonic treatment in step S1 is 40-50 kHz, and the dispersion time of the ultrasonic treatment is 20-30 min.

5. The method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating according to claim 1, characterized in that: In step S2, the usage ratio of polyphenylene sulfide, anhydrous ethanol, polypropylene and pretreated tungsten-rhenium alloy substrate is (0.2-0.5) g: (100-200) mL: (12-18) g: (6-9) g.

6. The method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating according to claim 1, characterized in that: In step S2, the spraying power is 45-55 kW, the gas flow rate of argon is 55-60 L / min, the gas flow rate of hydrogen is 12-18 L / min, and the coating thickness is 100-200 μm.

7. The method for preparing a tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating according to claim 3, characterized in that: The dosage ratio of tungsten powder, rhenium powder and anhydrous ethanol is (10-15) g: (2-3) g: (30-50) mL.

8. A tungsten-rhenium alloy high temperature resistant and thermal shock resistant coating obtained by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Tungsten-rhenium thermocouple oxidation resistant coating having high thermal shock resistance and application thereof

    CN108070850A

  • Method for preparing high-performance tungsten base metal parts

    CN109128163A

  • Tungsten-rhenium solid alloy powder with nanocrystalline structure as well as preparation method and application of tungsten-rhenium solid alloy powder

    CN114769602A

  • Preparation method of nano tungsten-rhenium pre-alloyed powder

    CN116021024A

  • Preparation method of high-uniformity nano tungsten-rhenium alloy powder

    CN117983821A