Metal mask plate and coating method thereof

By forming an insulating film layer with a thickness difference of greater than 10% to 40% for the upper and lower surfaces of the metal mask in the OLED production process, the problems of mask sagging and opening morphology deterioration are solved, and the quality of the mask is improved. The accuracy and quality of the packaging layer.

CN118726902APending Publication Date: 2024-10-01JIANGSU TOPTO MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410768074.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the OLED production process, the sagging and opening shape specifications of the metal mask are prone to deterioration when precision requirements increase, affecting the quality of the packaging layer.

Method used

Using the coating method of different surface insulating film layers, by forming insulating film layers on the upper and lower surfaces of the metal mask, ensure that the thickness of the insulating film layer on the lower surface is greater than the thickness of the insulating film layer on the upper surface, and the thickness difference is within 10% to 40%, and optimize the topography specifications of the mask by adjusting the coating rate and film material.

Benefits of technology

Significantly optimized the sagging/opening morphology specifications of the metal mask during and after coating, reducing deterioration and improving the accuracy of the mask and the quality of the packaging layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726902A_ABST
    Figure CN118726902A_ABST
Patent Text Reader

Abstract

The invention provides a metal mask plate and a coating method thereof, different surfaces of the metal mask plate are coated to form insulating film layers, and the coating method specifically comprises the following steps: forming an upper surface insulating film layer on the upper surface of the metal mask plate, and forming a lower surface insulating film layer on the lower surface of the metal mask plate; wherein the nominal thickness of the lower surface insulating film layer is larger than that of the upper surface insulating film layer, and the thickness difference is 10%-40% of the thickness of the upper surface insulating film layer; the metal mask plate is at least used for forming a packaging layer in an OLED production process. Compared with the prior art, according to the scheme, the deformation of sagging / opening morphology occurring in the film coating process and / or after film coating of the metal mask plate can be obviously optimized. And in an ideal state, the net surface sagging morphology of the metal mask plate can be reduced and degraded by 3%-5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of OLED, or more specifically AMOLED production technology, and in particular to a metal mask plate and a coating method thereof. Background Art

[0002] The vacuum evaporation process is the core process relied upon in the OLED production process. In the subsequent process of vacuum evaporation, a metal mask is also required for thin film packaging. The accuracy of the metal mask directly determines the accuracy of the packaging layer, which in turn affects the quality of the OLED panel products.

[0003] With the continuous iteration of production line generations, the OLED production process has continuously increased the accuracy and quality requirements of metal mask plates.

[0004] Under the premise of increasing precision requirements, the degradation of metal mask droop specifications and opening morphology has been noticed more and more. Summary of the invention

[0005] In order to solve the above problems existing in the prior art, an embodiment of the present disclosure provides a coating method of a metal mask plate.

[0006] The coating method of the metal mask provided in the embodiment of the present disclosure coats different surfaces of the metal mask to form an insulating film layer, specifically comprising:

[0007] An upper surface insulating film layer is formed on the upper surface of the metal mask plate.

[0008] forming a lower surface insulating film layer on the lower surface of the metal mask plate;

[0009] Wherein, the nominal thickness of the lower surface insulating film layer is greater than the nominal thickness of the upper surface insulating film layer, and the thickness difference is 10% to 40% of the thickness of the upper surface insulating film layer;

[0010] The metal mask is at least used to form a packaging layer in the OLED production process.

[0011] Compared with the prior art, the above solution can significantly optimize the deformation of the drooping / opening morphology that occurs during and / or after the metal mask coating process.

[0012] Optionally, the thickness difference is 10% to 30% of the thickness of the upper surface insulating film layer.

[0013] Optionally, the thickness difference is 20% of the thickness of the upper surface insulating film layer.

[0014] The aforementioned optional technical solution can reduce the degradation of the mesh drooping morphology of the metal mask by 3% to 5%.

[0015] Optionally, the nominal thickness of the upper surface insulating film layer is 2.0 μm, the thickness difference is 0.8 μm, and the nominal thickness of the lower surface insulating film layer is 2.8 μm. The droop specification and opening morphology of the metal mask before coating can be effectively optimized by 2% to 5%.

[0016] Optionally, an upper surface insulating film layer is formed on the upper surface of the metal mask plate at a first rate, and a lower surface insulating film layer is formed on the lower surface of the metal mask plate at a second rate;

[0017] The first rate is greater than the second rate.

[0018] Optionally, the first rate is 0.5 nm / min and the second rate is 0.2 nm / min.

[0019] The above-mentioned optional solution can effectively optimize the droop specification and opening morphology specification of the metal mask before coating by about 2% to 5%.

[0020] Optionally, the film layer material includes an insulating film layer of aluminum oxide, and an aluminum oxidation rate of the upper surface insulating film layer is lower than an aluminum oxidation rate of the lower surface insulating film layer.

[0021] Optionally, the aluminum-oxygen ratio in the upper surface insulating film layer is 2:3, and the aluminum-oxygen ratio in the lower surface insulating film layer is 4:7. The droop specification and opening morphology of the metal mask before coating can be effectively optimized by 2% to 3%.

[0022] Optionally, the film layer material formed includes one or more insulating film layers selected from aluminum oxide, zirconium oxide, aluminum nitride, and aluminum oxynitride, and the film layer materials of the upper surface insulating film layer and the lower surface insulating film layer are different.

[0023] Optionally, the film layer material of the upper surface insulating film layer includes aluminum oxide, and the film layer material of the lower surface insulating film layer includes aluminum oxynitride.

[0024] The droop specification and opening morphology of the metal mask before coating can be effectively optimized by 2% to 3%.

[0025] Optionally, the upper surface insulating film layer with a nominal thickness of 2.0 μm is formed by coating at a rate of 0.5 nm / min, and the lower surface insulating film layer with a nominal thickness of 2.8 μm is formed at a rate of 0.2 nm / min, wherein the material of the upper surface insulating film layer includes aluminum oxide, and the material of the lower surface insulating film layer includes aluminum nitride oxide. This solution can effectively optimize the droop specification and opening morphology specification of the metal mask before coating by about 5% to 15%.

[0026] The embodiment of the present disclosure further provides a metal mask plate having an insulating film layer, wherein the insulating film layer is formed by the coating method described in any one of the aforementioned technical solutions.

[0027] In summary, the coating method provided in the aforementioned technical solution or its preferred or optional solution can compensate for the degradation of the morphology specifications of the metal mask during / after coating to varying degrees. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure or the background technology, the drawings required for use in the embodiments of the present disclosure or the background technology will be described below.

[0029] Figure 1 is a schematic diagram of a CVD mask plate involved in an embodiment of the present disclosure;

[0030] Figure 2 It shows that the thickness of the insulating coating films on the upper and lower sides of the CVD mask plate in the embodiment is different;

[0031] Figure 3 The embodiment shows the selection of a detection point column of a mask plate shape detection method involved in the embodiment;

[0032] Figure 4 The three detection points corresponding to an opening on the mask plate are shown as an example;

[0033] Figure 5 It is a cross-sectional view (partial) of the tested CVD mask, and shows the morphological features corresponding to the positive and negative offset values ​​of the test points.

[0034] Note in the figure:

[0035] 1.CVD mask;

[0036] 10.Invar substrate;

[0037] 111. upper surface insulating film layer, 112. lower surface insulating film layer, 113. side surface insulating film layer, 114. opening inner insulating film layer;

[0038] 12. Mask plate opening;

[0039] In the figure, T1 and T2 indicate the different film thicknesses of the upper surface insulating film layer and the lower surface insulating film layer, and a, b, and c are three detection points in the same column but different rows. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0042] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0043] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0044] The present disclosure aims to optimize and improve the manufacturing process of metal mask plates. Explanatoryally, the metal mask plates in the present disclosure include mask plates used in OLED production lines (and subdivided AMOLED production lines). According to different applicable processes, the aforementioned mask plates are further subdivided into CVD mask plates (CVD Mask), open metal masks (OMM, Open Mask) and precision metal mask plates (FMM, Fine Metal Mask).

[0045] The metal mask referred to in the present disclosure especially includes the aforementioned CVD mask. In AMOLED production, CVD mask is generally used for thin film encapsulation (TFE, Thin Film Encapsulation) and Y-octa (YOUMOn-Cell Touch AMOLED) production in the back-end process of AMOLED, for example, using physical vapor deposition (such as magnetron sputtering) or chemical vapor deposition to form an encapsulation layer on the device. It can be seen that the accuracy of the CVD mask directly affects the quality of the encapsulation layer, and further determines the long-term stability of the device and the effect of isolating oxygen and moisture penetration, which has a great impact on the quality of the final product.

[0046] The main structure of the metal mask is the mesh surface, which is formed by making fixed openings on a whole sheet of raw material such as Invar36 (an iron-nickel alloy with an ultra-low expansion coefficient) through steps such as exposure and etching. During use, the metal mask plate uses the openings on the mesh surface to limit the film layer area formed by processes such as evaporation, magnetron sputtering, and chemical vapor deposition. The morphology of a typical CVD mask plate is as follows: Figure 1As shown, it should be understood that the number of openings on the mask grid is simplified in this figure.

[0047] In the process of thin film packaging using a mask, abnormal gas phase material deposition may occur at the position corresponding to the edge of the mesh opening, which affects the quality of the packaging layer formed around the above position, such as making the shape of the packaging layer irregular. This is caused by the degradation of the morphology specifications of the mesh opening. At the same time, the droop of the mask due to its own weight will also deteriorate the morphology specifications of the opening.

[0048] The inventors of the present application have discovered through research that the aforementioned degradation of the morphological specifications of the droop and openings is associated with the coating process of the metal mask plate. In other words, when the coating process of the metal mask plate is performed, the morphological specifications of the mask plate will change. Usually, such specifications change in the direction of degradation and may be further aggravated during the use of the mask plate due to environmental influences such as temperature.

[0049] For ease of understanding, the coating process of the metal mask plate is explained as follows in the present disclosure. The material of the mask plate, such as Invar36 (Invar steel, Invar alloy, ideal components include Ni 36% and Fe 64%), has good conductivity, which will cause the gas phase material to be mistakenly deposited on the mask plate during the process of forming the packaging layer. Therefore, the surface of the metal mask plate must be plated to form an insulating coating layer.

[0050] Without wishing to be bound by any theory, the inventors of the present application have conducted in-depth research on the coating process of the metal mask plate, aiming to compensate for the aforementioned degradation of the morphology specifications caused by the coating by improving the coating process, or to improve the deformation of the mask plate caused by its own weight, and ultimately improve the quality of the product packaging layer and enhance the reliability of the product.

[0051] In view of this, the present disclosure first provides an embodiment of a coating method, wherein the coating method coats different surfaces of a metal mask plate to form an insulating film layer, and specifically includes:

[0052] like Figure 2 As shown, an upper surface insulating film layer 111 is formed on the upper surface of the metal mask plate, and a lower surface insulating film layer 112 is formed on the lower surface of the metal mask plate.

[0053] It should be understood that the upper surface in the embodiment refers to the surface of the mask plate that should be on the upper side during use, and the same applies to the lower surface.

[0054] According to an embodiment of the present disclosure, different surfaces of the metal mask plate are respectively coated to form an insulating film layer. Specifically, the coating can be in a sequential order, for example, the upper surface is coated first and then the lower surface is coated, or the upper and lower surfaces are coated at the same time, but the coating parameters are different, so that the upper surface insulating film layer and the lower surface insulating film layer have different structures from each other.

[0055] It should be understood that the coating process involved in the embodiments of the present disclosure and the detection method involved in the following text are all carried out in a state where, for example, a CVD mask plate is stretched.

[0056] According to the embodiments of the present disclosure, the upper surface insulating film layer and the lower surface insulating film layer have different structures, which are specifically reflected in one or more of the following differences:

[0057] The film materials, film thickness and film forming rates are different.

[0058] Furthermore, the different film layer materials specifically include: different main compounds constituting the film layer, such as aluminum oxide and zirconium oxide; or different ratios of elements in the film layer, such as different ratios of aluminum and oxygen, different ratios of aluminum and zirconium, etc.

[0059] According to the embodiments of the present disclosure, in order to ensure the insulation performance of the mask plate, Figure 1 As shown, in addition to the upper and lower surfaces, the side walls of the mask and the inner walls of the mesh openings are also provided with insulating film layers, such as the side surface insulating film layer 113 and the inner opening insulating film layer 114. The composition thereof may be the same as or different from the film layers of the upper and lower surfaces.

[0060] According to the embodiment of the present disclosure, the film material, film thickness and film forming rate of the side surface insulating film layer 113 and the opening inner insulating film layer 114 can also be adjusted so that different film layers produce stress differences to improve the overall morphology of the mask plate and the opening morphology.

[0061] According to an embodiment of the present disclosure, in order to compensate for the morphology degradation at the mesh opening position, the coating parameters at the periphery / sidewall of the mesh opening, such as thickness, rate, and material, may be different from the coating parameters at other positions of the mask.

[0062] According to an embodiment of the present disclosure, the thickness of each insulating film layer (eg Figure 2 The T1 or T2 in FIG. 5 may be 1.0 μm to 5.0 μm, or may be 1.5 μm to 2.5 μm.

[0063] According to the embodiments of the present disclosure, the insulating film layer can be a compound film layer that meets the impedance requirements of the CVD mask, such as aluminum oxide Al2O3, aluminum oxide + aluminum nitride AlN covalently bonded, zirconium oxide ZrO2, etc. The aluminum oxide + aluminum nitride is covalently bonded, for example, a film layer with a total film thickness of 2μm, 1.5μm is aluminum oxide, 0.5μm is aluminum nitride, and the two film layers are plated separately.

[0064] The material of the insulating film layer in the embodiment of the present disclosure is not limited thereto, and may also be other film-forming materials having the characteristics of corrosion resistance, high impedance, and not easy to fall off.

[0065] According to the embodiments of the present disclosure, Figure 2 As shown, the nominal thickness T2 of the lower surface insulating film layer is greater than the nominal thickness T1 of the upper surface insulating film layer, and the thickness difference is 10% to 40% of the thickness of the upper surface insulating film layer.

[0066] In a typical embodiment, the metal mask is specifically used to form an encapsulation layer in an OLED production process.

[0067] In a typical embodiment, the metal mask is used to limit the film layer area formed by evaporation, magnetron sputtering or chemical vapor deposition process through the openings on the mesh surface.

[0068] Compared with the prior art, under the condition of forming a packaging layer, the above solution can significantly optimize the deformation of the drooping / opening morphology that occurs during and / or after the metal mask is coated.

[0069] According to an embodiment of the present disclosure, in a preferred embodiment, the difference in thickness between T2 and T1 is 10% to 30% of the thickness of the upper surface insulating film layer T1.

[0070] More preferably, the thickness difference is 20% of the thickness T1 of the upper surface insulating film layer.

[0071] The aforementioned embodiment can reduce the degradation of the mesh drooping morphology of the metal mask by 3% to 5%.

[0072] More preferably, the nominal thickness of the upper surface insulating film layer is T1 = 2.0 μm, the thickness difference is 0.8 μm, and the nominal thickness of the lower surface insulating film layer is T2 = 2.8 μm. The droop specification and opening morphology of the metal mask before coating can be effectively optimized by 2% to 5%.

[0073] Based on the above embodiments, the present disclosure further provides an embodiment in which the coating rates of the upper and lower surfaces are different. Specifically, an upper surface insulating film layer is formed on the upper surface of the metal mask plate at a first rate, and a lower surface insulating film layer is formed on the lower surface of the metal mask plate at a second rate; wherein the first rate is greater than the second rate.

[0074] According to an embodiment of the present disclosure, in a preferred embodiment, the first rate is 0.5 nm / min, the second rate is 0.2 nm / min, and in one embodiment, in addition to the difference in the aforementioned rates, the thickness of the lower surface insulating film layer is also greater than that of the upper surface insulating film layer.

[0075] The above preferred embodiment utilizes different film forming speeds to further achieve the technical effect of making the upper and lower surfaces have different film layer internal stresses, thereby affecting the morphological changes of the mesh surface and the openings brought about by the film layer.

[0076] The above preferred embodiment, under the premise of controlling the difference in thickness of the insulating layers on the upper and lower surfaces, can further effectively optimize the sagging specification and the opening morphology specification of the metal mask before coating by about 2% to 5%.

[0077] On the basis of the aforementioned embodiments, the present disclosure also provides an embodiment in which the upper and lower surface insulating film layers are composed of materials with different element ratios. More specifically, this can be achieved by controlling the oxidation rates of different surface film layers. For example, an insulating film layer is formed in which the film layer material includes aluminum oxide, and the aluminum oxidation rate of the upper surface insulating film layer is less than the aluminum oxidation rate of the lower surface insulating film layer.

[0078] The above-mentioned embodiment can also be applied to the insulating film layer whose main material is zirconium oxide. For example, the zirconium oxidation rate of the upper surface insulating film layer is smaller than the zirconium oxidation rate of the lower surface insulating film layer.

[0079] The above-mentioned embodiment can also be applied to the insulating film layer whose main material is aluminum nitride, for example, the aluminum nitridation rate of the upper surface insulating film layer is greater than or less than the aluminum nitridation rate of the lower surface insulating film layer.

[0080] Preferably, the ratio of aluminum to oxygen in different film layers is adjusted by oxidation rate, for example, the ratio of aluminum to oxygen in the upper surface insulating film layer is 2:3, and the ratio of aluminum to oxygen in the lower surface insulating film layer is 4:7. Based on the solution of adjusting the film thickness in the above embodiment, the droop specification and opening morphology of the metal mask before coating can be effectively optimized by 2% to 3%.

[0081] In the above-mentioned embodiment, the aluminum oxide film layer is formed by the reaction of pure aluminum with oxygen. By adjusting different ratios of aluminum and oxygen, the overall composition of the film layer is fine-tuned on the basis of generating the main reaction product AL2O3.

[0082] Preferably, the film layer material includes one or more insulating film layers selected from aluminum oxide, zirconium oxide, aluminum nitride, and aluminum oxynitride, and the film layer materials of the upper surface insulating film layer and the lower surface insulating film layer are different.

[0083] In a typical embodiment, the main components of the insulating film layers on different surfaces are different. It should be understood that the main components mentioned above refer to the components with a content greater than 90% by mass in the film layer material.

[0084] Preferably, the film material of the upper surface insulating film layer comprises aluminum oxide, and the film material of the lower surface insulating film layer comprises aluminum oxynitride. This preferred embodiment can effectively optimize the droop specification and opening morphology of the metal mask before coating by 2% to 3%.

[0085] Preferably, the aluminum oxynitride includes AlN x ·(Al2O3) 1-x (x=0.1-0.9) aluminum oxynitride; optionally, x is 0.5. Optionally, the aluminum oxynitride is a covalent combination of aluminum oxide and aluminum nitride.

[0086] The aforementioned embodiment or its preferred embodiment utilizes the differences in different film layer stresses formed by different film layer thicknesses / film layer materials / coating processes to optimize specification data. Since the double-sided film layer is coated separately, the different stresses of the front and back film layers can be used to affect the overall mesh surface morphology specifications, thereby compensating for the metal mask plate, especially the morphology degradation of the opening part.

[0087] In a typical embodiment, the coating thickness, film forming rate, and coating material of the upper and lower surfaces are controlled simultaneously, including: forming an upper surface insulating film layer with a nominal thickness of 2.0 μm at a rate of 0.5 nm / min, and forming a lower surface insulating film layer with a nominal thickness of 2.8 μm at a rate of 0.2 nm / min, wherein the material of the upper surface insulating film layer is aluminum oxide, and the material of the lower surface insulating film layer is aluminum nitride oxide. This solution can effectively optimize the droop specification and opening morphology specification of the metal mask before coating by about 5% to 15%.

[0088] For the opening morphology optimization effect of the aforementioned typical embodiment, an example of a detection method is provided as follows:

[0089] like Figure 3 ,and Figure 4 As shown in the figure, for each opening (Cell) on the metal mask plate, three test points a, b, and c are selected on its Y-axis side. At the same time, the X-axis position of the test point is selected to be 0.5mm away from the half-etching edge. Figure 4 As shown, the 01st column, the 03rd column, and the 05th column before and after the coating according to the parameters of the above typical embodiment are selected (such as Figure 3 The test values ​​(unit: μm) of each test point are compared as shown in Table 1 and Table 2.

[0090] Table 1 Morphology of each test point before coating

[0091] Number of lines 05 columns 03 columns 01 Column 1 -1 24.5 6.5 2 3 22.5 5 3 -1 20.5 4.5 4 0 20 5 5 -1 22.5 4 6 1 21.5 5.5 7 2 23 3.5 8 1 24 4 9 -1 24.5 5.5 10 -2 23.5 5.5 11 1 21 5 12 -1 23.5 5 13 1 25 5.5 14 1 27.5 5 15 1 21.5 5 16 -1 23 6 17 1 23.5 4 18 -2 23 5 19 2 26 6

[0092] Among them, the test value of each column / row is the height data of the test point in the vertical direction (perpendicular to the mask plane), such as Figure 5 As shown in the figure, the positive value is above the horizontal reference, and the negative value is below the horizontal reference. The different heights of each test point form the overall shape data of the mesh surface.

[0093] As shown in Table 1, the values ​​of each test point in column 03 are significantly higher than those in columns 01 and 05, which indicates that the mask has obvious flatness morphology defects. In addition, it does not meet the specific customization requirements of the product, that is, column 05 cannot be a negative number, and each test point is less than 50μm.

[0094] Table 2 Morphology of each test point after coating

[0095] Number of lines 05 columns 03 columns 01 Column 1 20 30 17 2 17 27.5 13 3 14 29 10.5 4 15 23.5 10 5 16 27 11 6 14 31.5 14 7 16 36.5 9.5 8 20 28.5 13.5 9 21 29 16 10 20 29.5 10.5 11 18 28.5 8 12 26 32.5 14.5 13 16 27.5 13 14 19 31.5 8 15 14 30.5 14.5 16 17 29 13.5 17 14 24 9.5 18 18 32.5 12.5 19 18 33 10

[0096] As can be seen from Table 2, through the coating parameters in the aforementioned embodiment, that is, the upper surface insulating film layer with a nominal thickness of 2.0 μm is formed by coating at a rate of 0.5 nm / min, and the lower surface insulating film layer with a nominal thickness of 2.8 μm is formed at a rate of 0.2 nm / min, wherein the material of the upper surface insulating film layer is aluminum oxide, and the material of the lower surface insulating film layer is aluminum nitride. After coating, the values ​​of the 01 column / 05 column are less different from the values ​​of the 03 column. The test shows that after coating with the parameters in the embodiment, the planar morphology degradation of the metal mask is significantly improved. Obviously, the morphology of the opening is also optimized, and the specific customization requirements of the product are met, that is, the 05 column cannot be a negative number, and the overall value is less than 50 μm.

[0097] For the above test, the applicant found that during the production process, the product was better when the test value of each test point was within the range of 0 to 50 μm, and it was not suitable to have too many negative values ​​or positive values ​​greater than 50 μm. The data in Table 1 had too many negative values. After the coating process in the above embodiment was used, the overall data was optimized to positive values. Although the values ​​in other columns increased to a certain extent, they were still controlled within 50 μm, meeting the requirements of good products.

[0098] In an optional embodiment, the aforementioned coating method may be applied to, but not limited to, the manufacturing process of a CVD mask plate, an open metal mask plate, or a precision metal mask plate.

[0099] The present disclosure provides an embodiment of a metal mask plate. The metal mask plate has an insulating film layer. The insulating film layer is formed by any of the embodiments of the aforementioned coating method.

[0100] The present disclosure provides an embodiment of a metal mask plate, in which the nominal thickness of the insulating film layer on the lower surface of the metal mask plate in the embodiment is greater than the nominal thickness of the insulating film layer on the upper surface, and the thickness difference is 10% to 40% of the thickness of the insulating film layer on the upper surface. Preferably, the thickness difference is 10% to 30% of the thickness of the insulating film layer on the upper surface. More preferably, the thickness difference is 20% of the thickness of the insulating film layer on the upper surface. The metal mask plate in this example is not prone to sagging or morphological degradation of the opening specifications under the use conditions. The use conditions in the embodiment are to use the openings on the mesh surface of the metal mask plate to limit the film layer area formed in the evaporation, magnetron sputtering or chemical vapor deposition process to form a desired encapsulation layer, for example.

[0101] The present disclosure provides an embodiment of a metal mask plate, wherein the nominal thickness of the insulating film layer on the upper surface of the metal mask plate is 2.0 μm, and the nominal thickness of the insulating film layer on the lower surface of the metal mask plate is 2.8 μm.

[0102] The present disclosure provides an embodiment of a metal mask plate, wherein the upper and lower surface insulating film layers of the metal mask plate are both formed by oxidation of pure aluminum, and the aluminum oxidation rate of the upper surface insulating film layer is lower than that of the lower surface insulating film layer.

[0103] The present disclosure provides an embodiment of a metal mask plate. In the embodiment, the aluminum-oxygen ratio in the upper surface insulating film layer of the metal mask plate is 2:3, and the aluminum-oxygen ratio in the lower surface insulating film layer is 4:7.

[0104] The present disclosure provides an embodiment of a metal mask, wherein the film material of the upper insulating film layer of the metal mask comprises aluminum oxide, and the film material of the lower insulating film layer comprises aluminum oxynitride. Preferably, the aluminum oxynitride comprises AlN x ·(Al2O3) 1-x The aluminum oxynitride is a covalent combination of aluminum oxide and aluminum nitride.

[0105] The present disclosure provides an embodiment of a metal mask plate, wherein the upper surface insulating film layer and the lower surface insulating film layer of the metal mask plate are formed at different film forming speeds, respectively. Preferably, the film forming rate of the upper surface insulating film layer is 0.5nm / min, and the film forming rate of the lower surface insulating film layer is 0.2nm / min.

[0106] In an embodiment, the metal mask may have one or more features of the aforementioned metal mask embodiments.

[0107] In an embodiment, the metal mask plate may have one or more features in other embodiments based on different film layer thicknesses.

[0108] In a typical embodiment, the nominal thickness of the insulating film layer on the upper surface of the metal mask is 2.0 μm, and the film forming rate is 0.5 nm / min; the nominal thickness of the insulating film layer on the lower surface is 2.8 μm, and the film forming rate is 0.2 nm / min. The main component of the upper surface insulating film layer is aluminum oxide, and the main component of the lower surface insulating film layer is aluminum nitride oxide. Under the working condition of manufacturing the OLED encapsulation layer, the upper and lower insulating film layers of the metal mask in this embodiment have a stress difference, and the sagging of the metal mask and / or the degradation of the opening morphology can be compensated by the stress difference.

[0109] The above description is only part of the specific implementation methods of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the embodiments of the present disclosure should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A method for coating a metal mask, characterized in that: Plating different surfaces of the metal mask plate to form insulating film layers respectively, including: forming an upper surface insulating film layer on the upper surface of the metal mask plate, forming a lower surface insulating film layer on the lower surface of the metal mask plate; Wherein, the nominal thickness of the lower surface insulating film layer is greater than the nominal thickness of the upper surface insulating film layer, and the thickness difference is 10% to 40% of the thickness of the upper surface insulating film layer; The metal mask is at least used to form a packaging layer in the OLED production process.

2. The coating method according to claim 1, characterized in that: The thickness difference is 20% of the thickness of the upper surface insulating film layer.

3. The coating method according to claim 1, characterized in that: The nominal thickness of the upper surface insulating film layer is 2.0 μm, the thickness difference is 0.8 μm, and the nominal thickness of the lower surface insulating film layer is 2.8 μm.

4. The coating method according to claim 1, characterized in that: forming an upper surface insulating film layer on the upper surface of the metal mask at a first rate, forming a lower surface insulating film layer on the lower surface of the metal mask at a second rate; The first rate is greater than the second rate.

5. The coating method according to claim 4, characterized in that: The first rate is 0.5 nm / min, and the second rate is 0.2 nm / min.

6. The coating method according to claim 1, characterized in that: The film layer material includes an insulating film layer of aluminum oxide, and the aluminum oxidation rate of the upper surface insulating film layer is lower than the aluminum oxidation rate of the lower surface insulating film layer.

7. The coating method according to claim 6, characterized in that: The aluminum-oxygen ratio in the upper surface insulating film layer is 2:3, and the aluminum-oxygen ratio in the lower surface insulating film layer is 4:

7.

8. The coating method according to claim 1, characterized in that: The film layer material includes one or more insulating film layers selected from aluminum oxide, zirconium oxide, aluminum nitride, and aluminum oxynitride, and the film layer materials of the upper surface insulating film layer and the lower surface insulating film layer are different.

9. The coating method according to claim 8, characterized in that: The film layer material of the upper surface insulating film layer includes aluminum oxide, and the film layer material of the lower surface insulating film layer includes aluminum oxynitride.

10. A metal mask, characterized in that: The metal mask has an insulating film layer, and the insulating film layer is formed by the coating method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Insulating treatment method of metal masking plate for flexible OLED (Organic Light Emitting Diode) package

    CN108034913A

  • Composite metal mask plate with function of improving stretching flatness

    CN113493892A

  • Spatially tunable deposition to compensate in wafer differential bending

    CN114258436A

  • Mask sheet for OLED deposition, The Mask assembly using thereof

    KR102591278B1