Alkaline cyanide-free zinc-nickel alloy electroplating brightener and preparation method thereof
By using a combination of vanillin, sodium propargyl sulfonate, modified alkyl glycosides and non-ionic surfactants in the electroplating brightener, the nickel content and brightness of the plating layer were improved, and the dispersion and covering properties in the electroplating solution were solved. Solving the problem of deficiencies, a high-performance zinc-nickel alloy coating was achieved.
Patent Information
- Application Number
- CN202410883131.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
AI Technical Summary
Existing electroplating brighteners have insufficient dispersion and coverage properties in the electroplating solution, resulting in rough and dark coatings. Increasing the brightener dose will reduce the current efficiency and coating bonding force, affecting the properties of the coating, and commonly used surfactants cannot improve the surface properties of the coating. good.
An alkaline cyanide-free zinc-nickel alloy electroplating brightener is used, including vanillin and sodium propargyl sulfonate as the main brightener, modified alkyl glycoside as the carrier, and the nonionic surfactant is composed of polymethylhydrogensiloxane and Butynediol diethoxy ether is synthesized to improve the gloss performance and viscosity of the coating through the solubilization effect of modified alkyl glycosides and the wetting and penetration effect of non-ionic surfactants.
It increases the nickel content and brightness of the coating, enhances the gloss performance, flatness and ductility of the coating, solves the problem of insufficient dispersion and coverage properties, reduces the usage of brightener, and improves the overall performance of the electroplating solution.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electroplating brighteners, and specifically discloses an alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. Background Art
[0002] Electroplating is the process of depositing metal or composite materials onto a solid surface using electrochemical methods. During electroplating, the coating material acts as the anode and the workpiece to be plated acts as the cathode. The coating is reduced on the surface of the workpiece to be plated to form a coating. The purpose of electroplating is to plate a metal coating on the substrate to change the surface properties of the substrate to achieve the purpose of enhancing corrosion resistance and aesthetic surface. Brightener is a multi-component mixed additive that can make the coating uniform, bright and smooth. It is generally composed of a variety of intermediates, such as sulfur-containing compounds such as acetylamine compounds, pyridine derivatives, propargyl alcohol derivatives and thiourea compounds. When used as an electroplating additive, it can effectively improve the brightness of the coating. Due to the insufficient dispersibility and covering properties of brighteners, when they are used in electroplating solutions, they often result in rough and dark coatings.
[0003] The invention patent with publication number CN102002739 B discloses a synthetic main brightener for preparing zinc plating brightener, the formula components are: salicylaldehyde 59-61%, formaldehyde 24-26%, 2.4-dichlorobenzaldehyde 14-16%, the formula components are configured according to proportion, added to a reaction kettle and mixed and stirred evenly, and then 50% alkali solution is added at a ratio of 350-400 ml / L, the pH value is adjusted to 6.3-6.7, heated to 75-85°C, and kept warm for 3-4 hours. Then cool to room temperature, filter with filter cloth, add the filtered precipitate material into a spin dryer for spin drying, and then add it into a dryer for drying to obtain a finished product. When used, it is prepared into a composite brightener with a high-temperature carrier for potassium salt zinc plating. The formula has fast polishing, no oxidation, good electroplating quality, high coating brightness, stable and long-lasting non-discoloration; the invention patent with publication number CN104514018A discloses a nickel plating brightener and an electroplating method, the nickel plating brightener includes saccharin with a content of 100-120g / L Sodium, 40-60g / L p-toluenesulfonamide, 45-60g / L hydroxypropanesulfonic acid pyridinium salt, 30-40g / L hydroxyethyl propargyl ether, 5-10g / L sodium propargyl sulfonate, 0.5-2g / L sodium vinyl sulfonate; the nickel plating brightener of the invention is a composite of a primary brightener, a secondary brightener and an auxiliary brightener compounded from an intermediate, which can reduce the porosity of the coating, improve the brightness of the coating, and enhance the dispersion ability and deep plating ability of the plating solution.
[0004] However, there are too many organic substances in the above-mentioned prior art formula, which may cause serious pollution and poor environmental protection. In addition, increasing the amount of brightener added may lead to low current efficiency and slow deposition speed, while affecting the bonding strength of the coating and ultimately affecting the properties of the coating. In addition, there are researchers in the prior art who have solved the above problems by adding surfactants. However, the brightener containing a single surfactant in the system has poor effect on improving the surface performance of the coating when added to the plating solution.
[0005] In view of this, it is particularly important to disclose an alkaline cyanide-free zinc-nickel alloy electroplating brightener in the present application. Summary of the invention
[0006] In view of the defects of the prior art, the alkaline cyanide-free zinc-nickel alloy electroplating brightener provided by the present invention has excellent dispersion and covering ability when used in the electroplating solution, increases the nickel content of the coating, and has high brightness and excellent performance of the coating.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] On one hand, the present invention provides an alkaline cyanide-free zinc-nickel alloy electroplating brightener, wherein each liter of the electroplating brightener comprises the following raw materials: 5 to 15 g of a main brightener, 4 to 7 g of an auxiliary brightener, 1 to 3 g of a carrier and 0.8 to 1.5 g of a non-ionic surfactant, and the solvent is deionized water; wherein the main brightener is a combination of vanillin and sodium propargyl sulfonate.
[0009] In some embodiments of the present invention, the mass ratio of vanillin to sodium propargyl sulfonate is 1:(3-5).
[0010] Preferably, the mass ratio of vanillin to sodium propargyl sulfonate is 1:4.
[0011] In some embodiments of the present invention, the carrier is a modified alkyl glycoside.
[0012] In some embodiments of the present invention, the preparation steps of the modified alkyl glycoside are as follows:
[0013] Add branched fatty alcohol and catalyst in the reactor in sequence, then add glucose in batches, react at 100-110° C. for 2-3 hours, cool to 50-60° C., adjust pH to 7-8, filter, evaporate, distill and freeze-dry to obtain the modified alkyl glycoside.
[0014] Preferably, the preparation steps of the modified alkyl glycoside are as follows:
[0015] Add branched fatty alcohol and catalyst into the reactor in sequence, then add glucose evenly three times, react at 105°C for 2.5h, cool to 55°C, add sodium hydroxide solution to quench the reaction and adjust the pH to 7, filter, evaporate, distill and freeze-dry to obtain the modified alkyl glycoside.
[0016] In some embodiments of the present invention, the branched fatty alcohol is isomeric dodecanol.
[0017] In some embodiments of the present invention, the molar ratio of the branched fatty alcohol to glucose is (3-6):1.
[0018] Preferably, the molar ratio of the branched fatty alcohol to glucose is 4.5:1.
[0019] Preferably, the glucose is D-(+) glucose.
[0020] Preferably, the catalyst is dodecylbenzenesulfonic acid, and the added amount is 1-5% of the molar amount of glucose.
[0021] Further preferably, the added amount of the catalyst is 3% of the molar amount of glucose.
[0022] The present invention prepares a modified alkyl glycoside compound as a carrier of a brightener, and the modification improves the cathode polarization of the plating solution and inhibits the occurrence of a replacement reaction. The lipophilic end of the modified alkyl glycoside effectively solubilizes the main brightener, increases the dispersibility of the brightener in the electroplating solution, accelerates the reduction reaction of vanillin in the main brightener to zinc-nickel ions, forms a stable complex by complexation, inhibits the deposition of impurities, and ensures the improvement of the gloss performance of the coating at a relatively low amount of brightener added; on the other hand, the modified alkyl glycoside also plays a certain thickening role, and when the brightener is added to the electroplating solution, the viscosity and fluidity of the system can be effectively improved, which is helpful to improve the performance of the zinc-nickel alloy coating.
[0023] In some embodiments of the present invention, the preparation steps of the nonionic surfactant are as follows:
[0024] An organic solvent is added to a reactor, and then polymethylhydrogensiloxane and butynediol diethoxy ether are added and stirred evenly, and a Speier catalyst is added, and the mixture is stirred under an inert atmosphere, and the temperature is raised to 80-90° C. and reacted for 6-7 hours. After the reaction is completed, the mixture is subjected to reduced pressure distillation and drying to obtain the nonionic surfactant.
[0025] Preferably, the preparation steps of the nonionic surfactant are as follows:
[0026] Add an organic solvent into the reactor, then add polymethylhydrogensiloxane and butynediol diethoxy ether and stir evenly, add a Speier catalyst, stir under an inert atmosphere, heat to 85° C., react for 7 hours, and after the reaction is completed, perform reduced pressure distillation and drying to obtain the nonionic surfactant.
[0027] In some embodiments of the present invention, the molar ratio of the polymethyl hydrogen siloxane to butynediol diethoxy ether is 1:(1-1.3).
[0028] Preferably, the molar ratio of the polymethyl hydrogen siloxane to butynediol diethoxy ether is 1:1.2.
[0029] Preferably, the organic solvent is isopropanol.
[0030] Preferably, the amount of the organic solvent added is 1 to 2 times the total mass of polymethylhydrogensiloxane and butynediol diethoxy ether.
[0031] Further preferably, the amount of the organic solvent added is 1.5 times the total mass of polymethyl hydrogen siloxane and butynediol diethoxy ether.
[0032] Preferably, the Speier catalyst is a 1-2 wt % isopropanol solution of chloroplatinic acid.
[0033] Further preferably, the Speier catalyst is a 2 wt % isopropanol solution of chloroplatinic acid.
[0034] Preferably, the added amount of the Speier catalyst is 0.010-0.012% of the total mass of polymethylhydrogensiloxane, butynediol diethoxy ether and the organic solvent.
[0035] Further preferably, the added amount of the Speier catalyst is 0.011% of the total mass of polymethylhydrogensiloxane, butynediol diethoxy ether and the organic solvent.
[0036] The applicant prepares a nonionic surfactant by using specific polymethylhydrogensiloxane and butynediol diethoxy ether. By adjusting the reaction ratio, the nonionic surfactant can form stable micelles at a relatively low reaction amount of butynediol diethoxy ether, play a wetting and penetrating role, carry other components in the brightener to the deep layer of the surface of the object to be plated, and play a role; at the same time, the surface tension reduction effect of the nonionic surfactant is greatly improved, and the gas-liquid interface spreading ability is enhanced. At this time, the defoaming ability of the acetylenic group and alcohol hydroxyl group still existing on the butynediol diethoxy ether is greatly improved, which promotes the brightener to play a better filling effect in the deep layer of the surface of the object to be plated, increases the deep plating and uniform plating performance of the electroplating solution system, and solves the problem of insufficient dispersion and covering filling ability of the commonly used brightener in the electroplating solution in the prior art; at the same time, the components in the brightener system play a relatively high synergistic effect under the penetration of the nonionic surfactant, and finally improve the comprehensive performance of the electroplating solution containing the brightener, especially the brightness, flatness and ductility of the coating are greatly improved.
[0037] In some embodiments of the present invention, the auxiliary brightener is sodium polydipropane disulfide sulfonate.
[0038] On the other hand, the present invention also provides a method for preparing an alkaline cyanide-free zinc-nickel alloy electroplating brightener, comprising the following steps: adding deionized water, a main brightener, an auxiliary brightener, a carrier and a non-ionic surfactant into a container in sequence, continuously adding deionized water during stirring until the main brightener, the auxiliary brightener, the carrier and the non-ionic surfactant are evenly dispersed, and then adding deionized water to the standard scale of the container to obtain the alkaline cyanide-free zinc-nickel alloy electroplating brightener.
[0039] Preferably, the preparation method of the alkaline cyanide-free zinc-nickel alloy electroplating brightener comprises the following steps: adding deionized water, a main brightener, an auxiliary brightener, a carrier and a non-ionic surfactant, which account for 1 / 5 to 1 / 3 of the total volume of the electroplating brightener, into a container in sequence, continuously adding deionized water during stirring until the main brightener, the auxiliary brightener, the carrier and the non-ionic surfactant are evenly dispersed, and then adding deionized water to the standard scale of the container to obtain the alkaline cyanide-free zinc-nickel alloy electroplating brightener.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] (1) The alkaline cyanide-free zinc-nickel alloy electroplating brightener provided by the present invention has excellent dispersion and covering ability when used in the electroplating solution, increases the nickel content of the coating, and has high coating brightness and excellent performance;
[0042] (2) The present invention synthesizes polymethylhydrogensiloxane and butynediol diethoxy ether to prepare a nonionic surfactant by hydrosilane reaction, controls the proportion of hydrophilic segments on the nonionic surfactant, so that it can quickly form stable micelles when used, exerts a wetting and penetrating effect, and carries other components in the brightener to the deep layer of the surface of the object to be plated that is difficult to penetrate and exerts its effect; at the same time, the surface tension reduction effect of the nonionic surfactant is greatly improved, the gas-liquid interface spreading ability is enhanced, and the brightener is promoted to exert a better filling effect in the deep layer of the surface of the object to be plated, thereby increasing the deep plating and uniform plating ability of the electroplating solution system containing the brightener, and solving the problem of insufficient dispersion and covering filling ability of the commonly used brightener in the electroplating solution in the prior art; at the same time, the components in the brightener system exert a high synergistic effect under the penetration of the nonionic surfactant, and finally improve the comprehensive performance of the electroplating solution containing the brightener, especially the brightness, flatness and ductility of the coating are greatly improved;
[0043] (3) The present invention prepares a modified alkyl glycoside compound as a carrier of a brightener, and the modification improves the cathode polarization of the plating solution and inhibits the occurrence of a replacement reaction. The lipophilic end of the modified alkyl glycoside effectively solubilizes the main brightener, increases the dispersibility of the brightener in the electroplating solution, accelerates the reduction reaction of the vanillin in the main brightener to the zinc-nickel ions, forms a stable complex by complexation, inhibits the deposition of impurities, and ensures that the gloss performance of the coating is improved at a relatively low amount of brightener added; on the other hand, the modified alkyl glycoside also plays a certain thickening role. When the brightener is added to the electroplating solution, it can effectively improve the viscosity and fluidity of the system, which helps to improve the performance of the zinc-nickel alloy coating. DETAILED DESCRIPTION
[0044] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0045] If not otherwise specified, the reagents used below can be easily obtained from commercial companies, among which D-(+) glucose was purchased from Shanghai MacLean Reagent Co., Ltd.; polyoxyethylene lauryl ether was purchased from Jiangsu Hai'an Petrochemical Plant; polymethylhydrogensiloxane was purchased from Shandong Nengju Chemical Co., Ltd.; sodium polydisulfide dipropane sulfonate was purchased from Wuhan Shu'er Biotechnology Co., Ltd.; and silicone surfactant was purchased from Hubei Longsheng Sihai New Materials Co., Ltd.
[0046] Preparation Example 1
[0047] The preparation steps of modified alkyl glycoside are as follows:
[0048] 4.5 mol of isomeric dodecanol and 0.03 mol of dodecylbenzene sulfonic acid were added to the reactor in sequence, and then 1 mol of D-(+) glucose was added evenly in three times. The mixture was reacted at 105°C for 2.5 hours, cooled to 55°C, and sodium hydroxide was added to adjust the pH to 7. The modified alkyl glycoside was obtained by filtration, evaporation, distillation and freeze-drying.
[0049] Preparation Example 2
[0050] The preparation steps of the modified alkyl glycoside are the same as those of Preparation Example 1, except that 2.5 mol of isomeric dodecanol is added.
[0051] Preparation Example 3
[0052] The preparation steps of the modified alkyl glycoside are the same as those of Preparation Example 1, except that 6.5 mol of isomeric dodecanol are added.
[0053] Preparation Example 4
[0054] The preparation steps of the modified alkyl glycoside are the same as those of Preparation Example 1, except that 1 mol of D-(+) glucose is added at one time.
[0055] Preparation Example 5
[0056] The preparation steps of nonionic surfactant are as follows:
[0057] Add 67.8 mL of isopropanol to the reactor, then add 0.1 mol of polymethylhydrogensiloxane and 0.12 mol of butynediol diethoxy ether and stir evenly, add 0.012 mL of 2 wt% chloroplatinic acid isopropanol solution, stir under nitrogen atmosphere, heat to 85 ° C, react for 7 hours, and after the reaction is completed, distill and dry under reduced pressure to obtain a non-ionic surfactant.
[0058] Preparation Example 6
[0059] The preparation steps of the nonionic surfactant are the same as those of Preparation Example 5, except that 0.09 mol of butynediol diethoxy ether is added.
[0060] Preparation Example 7
[0061] The preparation steps of the nonionic surfactant are the same as those of Preparation Example 5, except that 0.14 mol of butynediol diethoxy ether is added.
[0062] Unless otherwise specified, the auxiliary brightener used in the following examples and comparative examples is sodium polydipropane disulfide sulfonate.
[0063] Example 1
[0064] An alkaline cyanide-free zinc-nickel alloy electroplating brightener, wherein each liter of the electroplating brightener comprises the following raw materials: 2g of vanillin, 8g of sodium propargyl sulfonate, 5.5g of an auxiliary brightener, 2g of a modified alkyl polyglycoside and 1.2g of a nonionic surfactant;
[0065] The preparation method of the alkaline cyanide-free zinc-nickel alloy electroplating brightener of the present embodiment comprises the following steps: 250 mL of deionized water, vanillin, sodium propargyl sulfonate, sodium polydisulfide propane sulfonate, modified alkyl glucoside and nonionic surfactant are sequentially added into a container, deionized water is continuously added during stirring until the vanillin, sodium propargyl sulfonate, sodium polydisulfide propane sulfonate, modified alkyl glucoside and nonionic surfactant are uniformly dispersed, and deionized water is added to the standard scale of the container to adjust the volume to 1 L, so as to obtain the alkaline cyanide-free zinc-nickel alloy electroplating brightener;
[0066] The modified alkyl polyglycoside of this example is obtained from Preparation Example 1, and the nonionic surfactant is obtained from Preparation Example 5.
[0067] Example 2
[0068] An alkaline cyanide-free zinc-nickel alloy electroplating brightener, wherein each liter of the electroplating brightener comprises the following raw materials: 1g of vanillin, 4g of sodium propargyl sulfonate, 4g of auxiliary brightener, 1g of modified alkyl polyglycoside and 0.8g of nonionic surfactant, and the solvent is deionized water;
[0069] The preparation method of the alkaline cyanide-free zinc-nickel alloy electroplating brightener of the present embodiment comprises the following steps: 200 mL of deionized water, vanillin, sodium propargyl sulfonate, sodium polydisulfide propane sulfonate, modified alkyl glucoside and nonionic surfactant are sequentially added into a container, deionized water is continuously added during stirring until the vanillin, sodium propargyl sulfonate, sodium polydisulfide propane sulfonate, modified alkyl glucoside and nonionic surfactant are uniformly dispersed, and deionized water is added to the standard scale of the container to adjust the volume to 1 L, so as to obtain the alkaline cyanide-free zinc-nickel alloy electroplating brightener;
[0070] The modified alkyl polyglycoside of this example is obtained from Preparation Example 1, and the nonionic surfactant is obtained from Preparation Example 5.
[0071] Example 3
[0072] An alkaline cyanide-free zinc-nickel alloy electroplating brightener, wherein each liter of the electroplating brightener comprises the following raw materials: 3g of vanillin, 12g of sodium propargyl sulfonate, 7g of auxiliary brightener, 3g of modified alkyl polyglycoside and 1.5g of nonionic surfactant, and the solvent is deionized water;
[0073] The preparation method of the alkaline cyanide-free zinc-nickel alloy electroplating brightener of the present embodiment comprises the following steps: 333 mL of deionized water, vanillin, sodium propargyl sulfonate, sodium polydisulfide propane sulfonate, modified alkyl glucoside and nonionic surfactant are sequentially added into a container, deionized water is continuously added during stirring until the vanillin, sodium propargyl sulfonate, sodium polydisulfide propane sulfonate, modified alkyl glucoside and nonionic surfactant are uniformly dispersed, and deionized water is added to the standard scale of the container to adjust the volume to 1 L, so as to obtain the alkaline cyanide-free zinc-nickel alloy electroplating brightener;
[0074] The modified alkyl polyglycoside of this example is obtained from Preparation Example 1, and the nonionic surfactant is obtained from Preparation Example 5.
[0075] Example 4
[0076] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified alkyl glycoside used is obtained from Preparation Example 2.
[0077] Example 5
[0078] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified alkyl glycoside used is obtained from Preparation Example 3.
[0079] Example 6
[0080] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified alkyl glycoside used is obtained from Preparation Example 4.
[0081] Example 7
[0082] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the nonionic surfactant used is obtained from Preparation Example 6.
[0083] Example 8
[0084] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the nonionic surfactant used is obtained from Preparation Example 7.
[0085] Example 9
[0086] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that 3.3 g of vanillin and 6.7 g of sodium propargyl sulfonate are added.
[0087] Example 10
[0088] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that 1.5 g of vanillin and 8.5 g of sodium propargyl sulfonate are added.
[0089] Embodiment 11
[0090] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified alkyl glycoside is replaced by a carrier prepared by mixing 1.7 g of polyoxyethylene lauryl ether and 0.3 g of sodium benzoate.
[0091] Example 12
[0092] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that the nonionic surfactant used is an organosilicon surfactant.
[0093] Comparative Example 1
[0094] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that 10 g of vanillin is used to replace 2 g of vanillin and 8 g of sodium propargyl sulfonate.
[0095] Comparative Example 2
[0096] An alkaline cyanide-free zinc-nickel alloy electroplating brightener and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that 10 g of sodium propargyl sulfonate is used to replace 2 g of vanillin and 8 g of sodium propargyl sulfonate.
[0097] Performance Testing
[0098] The alkaline cyanide-free zinc-nickel alloy electroplating brightener obtained in the above-mentioned embodiments and comparative examples was taken, and an electroplating solution was prepared according to the formula (each liter of electroplating solution contained 9 g of zinc oxide, 1.5 g of nickel sulfate, 130 g of sodium hydroxide, 100 mL of a cylinder opening agent, 15 mL of a nickel supplement, 3.5 mL of the alkaline cyanide-free zinc-nickel alloy electroplating brightener obtained in each embodiment and comparative example, 1.75 mL of hexylbenzylamine salt, and the balance was deionized water). The zinc-nickel alloy was used as the anode, and the iron sheet to be electroplated was used as the cathode. The size of the iron sheet was 10 cm × 8 cm × 0.3 mm. Electroplating was performed, and the electroplating temperature was set to 23 ° C, and the current density was 2 A / dm 2 , the electroplating time is 18min, and the plated parts covered with zinc-nickel alloy coating are subjected to the following performance tests. The specific test results are shown in Table 1:
[0099] (1) Adhesion test: According to GB / T5270-2005 "Review of test methods for adhesion strength of electrodeposited and chemically deposited metal coatings on metal substrates", use a steel scratcher with a blade grinded to 30° to forcefully scratch 6 parallel lines with a spacing of 1 mm on the surface of the plated coating, and then scratch 6 parallel straight lines with the same spacing and perpendicular to them, with the depth required to reach the iron sheet. If there is no coating peeling between the lines, the adhesion is considered to be qualified;
[0100] (2) Dispersion performance test: According to the near-far cathode method specified in the mechanical industry standard JB / T7704.4-95 (the current density is specified as 2A / dm 2 ) to conduct dispersion performance test, the larger the dispersion performance value, the better the dispersion performance;
[0101] (3) Nickel content test of the coating: The nickel content of each plated part is tested using an XDL-B X-ray fluorescence thickness gauge;
[0102] (4) Brightness performance test: Under the condition of 50W fluorescent lamp illumination, the surface of the coating is 40cm away from the fluorescent lamp, and the brightness of the coating is tested by visual inspection. Example 1 of Chinese Patent Publication No. CN103184479A is selected as the blank group. Based on its surface brightness, the surface brightness of the plated parts covered with zinc-nickel alloy coatings obtained by using the alkaline cyanide-free zinc-nickel alloy electroplating brightener obtained in each embodiment of the present invention and the comparative example is evaluated as brighter, darker or the same, wherein the brighter evaluation is scored as 1 point, the darker evaluation is scored as -1 point, and the same evaluation is scored as 0 point. After evaluation by 10 persons aged 20-30 with a visual acuity of 5.0 and no color blindness, the average score of the groups other than the blank group is calculated and recorded.
[0103] Table 1
[0104] project Bonding strength / qualified Dispersion performance / % Nickel content of coating / wt% Brightness Example 1 qualified 90.90 13.91 1 Example 2 qualified 88.95 13.80 1 Example 3 qualified 90.57 13.85 1 Example 4 qualified 86.72 13.59 0.9 Example 5 qualified 86.73 13.41 0.9 Example 6 Failure 86.65 12.55 0.8 Example 7 qualified 83.63 13.08 0.9 Example 8 qualified 82.64 12.85 0.9 Example 9 qualified 86.45 12.73 0.8 Example 10 qualified 86.55 12.69 0.8 Embodiment 11 qualified 86.00 12.47 0.8 Example 12 Failure 79.61 12.13 0.2 Comparative Example 1 qualified 86.25 12.35 0.7 Comparative Example 2 qualified 85.98 12.28 0.5
[0105] It can be seen from Table 1 that the electroplating brighteners provided in Examples 1 to 3 of the present invention have excellent performance, good dispersion and covering ability in the electroplating solution, high nickel content in the coating, corrosion prevention, and high coating brightness.
[0106] In Examples 4 and 5, the preparation ratio of isomeric dodecanol and D-(+) glucose was changed. In Example 6, D-(+) glucose was added at one time during preparation. In Example 11, the carrier prepared by polyoxyethylene dodecyl ether and sodium benzoate was used to replace the modified alkyl glycoside preferably prepared in the present invention. Compared with Example 1, the electroplating brightener preferably prepared in the present invention using branched alkyl glycoside as a high-temperature carrier can improve the cathode polarization of the electroplating solution, inhibit the occurrence of the replacement reaction, and effectively improve the performance of the zinc-nickel alloy coating.
[0107] In Example 7 and Example 8, the addition ratio of polymethylhydrogensiloxane and butynediol diethoxy ether in the preparation process of the nonionic surfactant was changed. In Example 12, an equal amount of an organic silicon surfactant was added to replace the nonionic surfactant prepared by the present invention. Compared with Example 1, it can be shown that the nonionic surfactant preferably prepared by the present invention can quickly form stable micelles when used, exert a wetting and penetrating effect, and the defoaming ability is greatly improved, the dispersion and covering effect are enhanced, the brightness and elongation of the electroplating solution coating are improved, and the comprehensive performance is improved;
[0108] In Examples 9 and 10, the addition ratio of vanillin and sodium propargyl sulfonate in the main brightener was changed, which affected the accelerating effect of the modified alkyl polyglycoside on the reduction reaction of vanillin in the main brightener to zinc-plated nickel ions, resulting in decreased stability of the complex and deposition of impurities, thereby affecting the gloss performance of the coating.
[0109] Comparative Examples 1 and 2 respectively add vanillin and sodium propargyl sulfonate as the main brightener. Compared with Example 1, it can be shown that the main brightener obtained by the combination of vanillin and sodium propargyl sulfonate specifically selected by the present invention can play a good synergistic role in the electroplating brightener system.
[0110] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. An alkaline cyanide-free zinc-nickel alloy electroplating brightener, characterized in that: Each liter of the electroplating brightener contains the following raw materials: 5-15g of a main brightener, 4-7g of an auxiliary brightener, 1-3g of a carrier and 0.8-1.5g of a non-ionic surfactant, and the solvent is deionized water; wherein the main brightener is a combination of vanillin and sodium propargyl sulfonate.
2. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 1, characterized in that: The mass ratio of the vanillin to sodium propargyl sulfonate is 1:(3-5).
3. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 1, characterized in that: The carrier is modified alkyl glycoside.
4. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 3, characterized in that: The preparation steps of the modified alkyl glycoside are as follows: Add branched fatty alcohol and catalyst in the reactor in sequence, then add glucose in batches, react at 100-110° C. for 2-3 hours, cool to 50-60° C., adjust pH to 7-8, filter, evaporate, distill and freeze-dry to obtain the modified alkyl glycoside.
5. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 4, characterized in that: The branched chain fatty alcohol is isomeric dodecanol.
6. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 4, characterized in that: The molar ratio of the branched fatty alcohol to glucose is (3-6):
1.
7. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 1, characterized in that: The preparation steps of the nonionic surfactant are as follows: An organic solvent is added to a reactor, and then polymethylhydrogensiloxane and butynediol diethoxy ether are added and stirred evenly, and a Speier catalyst is added, and the mixture is stirred under an inert atmosphere, and the temperature is raised to 80-90° C. and reacted for 6-7 hours. After the reaction is completed, the mixture is subjected to reduced pressure distillation and drying to obtain the nonionic surfactant.
8. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 7, characterized in that: The molar ratio of the polymethyl hydrogen siloxane to butynediol diethoxy ether is 1:(1-1.3).
9. The alkaline cyanide-free zinc-nickel alloy electroplating brightener according to claim 1, characterized in that: The auxiliary brightener is sodium polydipropane disulfide sulfonate.
10. A method for preparing the alkaline cyanide-free zinc-nickel alloy electroplating brightener according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: adding deionized water, a main brightener, an auxiliary brightener, a carrier and a non-ionic surfactant into a container in sequence, continuously adding deionized water during stirring until the main brightener, the auxiliary brightener, the carrier and the non-ionic surfactant are evenly dispersed, and then adding deionized water to the standard scale of the container to obtain the alkaline cyanide-free zinc-nickel alloy electroplating brightener.