Isoquinoline micro-nanofiber membrane as well as preparation method and application thereof

By combining polymers with tetrastyrene-isoquinoline compounds, an isoquinoline micro-nanofiber membrane that can respond quickly under acid and alkali stimulation is prepared, which solves the problems of insufficient response speed and sensitivity in the existing technology and achieves for efficient applications in biomedical and environmental monitoring fields.

CN118727264AActive Publication Date: 2024-10-01WUYI UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410915081.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01
Estimated Expiration
2044-07-09

Smart Images

  • Figure CN118727264A_ABST
    Figure CN118727264A_ABST
Patent Text Reader

Abstract

The invention discloses an isoquinoline micro-nano fiber membrane as well as a preparation method and application thereof, the fiber membrane is prepared from a polymer and a tetraphenyl ethylene-isoquinoline compound, and the structural general formula of the tetraphenyl ethylene-isoquinoline compound is as follows: # imgabs0 # Ar represents isoquinoline. According to the scheme, the fiber membrane has strong fluorescence, the fluorescence color can present high-contrast change before and after acid-base fumigation, the response to acid and base is rapid, and the fiber membrane has wide application prospects in the fields of acid-base detection, environment monitoring and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field related to fluorescent materials, and in particular to an isoquinoline micro-nano fiber membrane and a preparation method and application thereof. Background Art

[0002] In the field of modern materials science, micro-nano fiber membranes have shown extensive application potential in many fields such as biomedicine and environmental protection due to their unique physical and chemical properties, such as surprisingly high specific surface area, excellent filtration performance and excellent biocompatibility. Especially in cutting-edge fields such as bioimaging and chemical sensing, micro-nano fiber membranes can achieve accurate detection, dynamic tracking and high-definition imaging of specific substances due to their fluorescent properties. This unique fluorescent property is achieved by cleverly introducing compounds or groups with fluorescent properties into the fiber membrane, which greatly expands its application range in bioimaging and chemical analysis.

[0003] However, with the rapid development of science and technology and the increasing requirements for material performance in the fields of biomedicine, environmental protection, energy storage, etc., the existing micro-nano fiber membranes have been unable to meet the growing demand in some aspects. Especially in application scenarios that require rapid response to acid-base stimulation, it is particularly important to develop a new type of nanofiber membrane with high sensitivity and rapid response to acid-base changes.

[0004] Therefore, in order to meet these growing demands, it is urgent to develop a new type of micro-nano fiber membrane. This membrane material not only inherits the advantages of traditional micro-nano fiber membranes, but also has a significant improvement in acid-base sensitivity, and can quickly and accurately respond to acid-base changes in the external environment, thus showing a broader application prospect in the fields of biomedicine, environmental monitoring, energy storage, etc. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides an isoquinoline micro-nano fiber membrane, which can not only generate fluorescence, but also respond quickly to acid-base stimulation and generate fluorescence of different colors.

[0006] The invention also provides a method for preparing the fiber membrane.

[0007] The present invention also proposes the application of the fiber membrane.

[0008] According to one aspect of the present invention, an isoquinoline micro-nano fiber membrane is provided. The raw materials for preparing the fiber membrane include a polymer and a tetraphenylethylene-isoquinoline compound. The structural formula of the tetraphenylethylene-isoquinoline compound is as follows:

[0009] Ar represents isoquinoline.

[0010] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the fiber membrane of the present invention has strong fluorescence, and its fluorescence color can show high contrast changes before and after acid and alkali fumigation, and it responds quickly to acid and alkali, and has broad application prospects in the fields of acid and alkali detection and environmental monitoring.

[0011] In some embodiments of the present invention, the structural formula of the tetraphenylethylene-isoquinoline compound is shown in one of the following formulas:

[0012]

[0013] In some embodiments of the present invention, the polymer includes at least one of cellulose acetate (CA), polystyrene (PS), polyvinyl alcohol (PVA) and polylactic acid (PLA). The compounds of the present invention have good fluorescence stability in different polymer matrices.

[0014] In some embodiments of the present invention, the mass ratio of the polymer to the tetraphenylethylene-isoquinoline compound is 1:0.01-0.1, such as 1:0.05.

[0015] In some embodiments of the present invention, the preparation raw material further includes a solvent, and the solvent is selected from a mixed solution of DMF (N,N-dimethylformamide) and DCM (dichloromethane).

[0016] In some embodiments of the present invention, the volume ratio of DMF to DCM is 1:1 to 3, such as 1:2.

[0017] In some embodiments of the present invention, the mass ratio of the tetraphenylethylene-isoquinoline compound to the solvent is 1:175-185, such as 1:179, 1:180, etc.

[0018] In some embodiments of the present invention, silicone oil paper is used as a grounding collector during the preparation of the fiber membrane.

[0019] According to another aspect of the present invention, a method for preparing the above-mentioned fiber membrane is provided, comprising the following steps:

[0020] Weigh tetraphenylethylene-isoquinoline compounds and polymers and dissolve them in a solvent to prepare an electrospinning solution, load the solution into a syringe, and extrude it through a spinneret at a speed of 0.8 to 1.2 mL / h (preferably 1.0 mL / h) to form filaments under the action of high-voltage static electricity; wherein the spinning voltage is 15 to 20 kV (preferably 17 kV), and the working distance is 11 to 15 cm (preferably 13 cm);

[0021] The general structural formula of the tetraphenylethylene-isoquinoline compound is as follows:

[0022] Ar represents isoquinoline.

[0023] In some embodiments of the present invention, silicone oil paper is used as a grounding collector during the preparation of the fiber membrane.

[0024] According to yet another aspect of the present invention, application of the fiber membrane in the field of detection or anti-counterfeiting is proposed.

[0025] In some embodiments of the present invention, the detection includes at least one of the following detection contents:

[0026] 1) Acidic substances;

[0027] 2) Alkaline substances.

[0028] In some embodiments of the present invention, the detection comprises the following steps: applying the detection content to the fiber membrane, irradiating the compound with an ultraviolet light source as an excitation light source, and observing fluorescence changes.

[0029] In some embodiments of the present invention, it is sufficient to apply it to the surface or inside of the product to be tested, without the need for complex operations such as photo-induced polymerization. The detection method of the present invention is easy to operate, has high detection efficiency, can realize batch fully automated detection, and has good industrial application prospects.

[0030] In some preferred embodiments of the present invention, the applying comprises at least one of coating, dipping, and fumigation. The coating, dipping, or fumigation operation allows the test content to be applied to the surface of the product to be tested, which is easy to operate.

[0031] In some preferred embodiments of the present invention, the wavelength of the ultraviolet light source is 320nm to 405nm; preferably 345nm to 385nm; more preferably 365nm.

[0032] According to the application of a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the compound of the present invention has strong fluorescence, and after being prepared into a fiber membrane, due to its larger specific surface area, it responds more quickly to external stimuli. The fiber membrane of the present invention responds quickly to acid and alkali, has good reversibility to acid fumigation, can be used repeatedly, and has good industrial application prospects.

[0033] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0035] Figure 1 This is a SEM image of the nanofiber membrane prepared in Example 1 of the present invention.

[0036] Figure 2 These are optical photographs and inverted fluorescence microscope photographs of the Iso-TPECN3Qu compound / PLA composite micro-nano fiber membranes with different contents prepared in Example 1 of the present invention: a) fluorescent lamp photograph; b) ultraviolet lamp photograph; c) inverted fluorescence microscope photograph.

[0037] Figure 3 This is the PL spectrum of the PLA-Iso-TPECN3Qu micro-nano fiber membrane prepared in Example 1 of the present invention under external stimulation. m represents the initial film; m-HCl represents the film after m-acid fumigation; m-HCl-NH3 represents the film after m-HCl film alkaline fumigation.

[0038] Figure 4 This is a fluorescence photograph (365 nm) of the PLA-Iso-TPECN3Qu micro-nano fiber membrane prepared in Example 1 of the present invention under external stimulation.

[0039] Figure 5 The fluorescence emission wavelength change and fluorescence photograph of the PLA-Iso-TPECN3Qu micro-nano fiber membrane prepared in Example 1 of the present invention after 10 cycles of acid-base stimulation.

[0040] Figure 6 It is a microstructure diagram of the PLA-ISO-TPECN4Qu fiber membrane prepared in Example 4 of the present invention at 1.50kX a) and 5.00kX b) times.

[0041] Figure 7 It is a microstructure diagram of the PLA-ISO-TPECN5Qu fiber membrane prepared in Example 5 of the present invention at 1.50kX a) and 5.00kX b) times.

[0042] Figure 8 It is a microstructure diagram of the PLA-ISO-TPECN8Qu fiber membrane prepared in Example 6 of the present invention at 1.50kX a) and 5.00kX b) times.

[0043] Fig. 9 It is a graph showing the acid-base stimulation test results of the fiber membranes prepared in Examples 4 to 6. DETAILED DESCRIPTION

[0044] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. The test methods used in the embodiments are conventional methods unless otherwise specified; the materials, reagents, etc. used, unless otherwise specified, can be reagents and materials obtained from commercial channels. Unless otherwise specified, the same parameter in each embodiment has the same value. The embodiments described below are exemplary and are only used to explain the present invention, and cannot be understood as limitations on the present invention.

[0045] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0046] The purchasing information of some raw materials used in the following examples and comparative example 1 is shown in Table 1 below:

[0047] Table 1

[0048]

[0049] The instrument information used in the following examples and comparative example 1 is shown in Table 2 below:

[0050] Table 2

[0051]

[0052] The methods and main parameter information used in the test characterization process are as follows:

[0053] Compound 1 H-NMR and 13 C-NMR was measured on a Bruker AVANCE NEO500 spectrometer with deuterated chloroform as solvent and tetramethylsilane (TMS) as internal standard to test the chemical structure of the compounds.

[0054] Fluorescence spectra and UV-visible absorption spectra are used to analyze the photophysical properties of compounds. The excitation and emission slits of the fluorescence spectrum for AIE performance testing are 10nm and 15nm, and the rest are 3nm and 5nm.

[0055] The X-ray diffractometer uses CuKα (λ=0.1541 nm) as the light source, with a test voltage of 40 kV and 40 mA, to characterize the aggregated structure of the compound.

[0056] The fluorescence quantum efficiency of the compounds was tested using a combined steady-state / transient fluorescence spectrometer and a calibrated integrating sphere.

[0057] Scanning electron microscopy was used to observe the microstructure of the fiber membrane with an operating voltage of 15 kV.

[0058] The specific synthesis process of TPECN is as follows (refer to Zhang X, Zhang X, Yang B, et al. Facile preparation of water dispersible red fluorescent organic nanoparticles and their cell imaging applications [J]. Tetrahedron, 2014, 70 (22): 3553-3559. Preparation):

[0059] 1-Bromo-1,2,2-triphenylethylene (1.74 g, 5.2 mmol) and 4-(cyanoethyl)phenylboronic acid (1.00 g, 6.2 mmol) were dissolved in a mixture of toluene (40 mL), Aliquat336 (methyl trioctylammonium chloride, 10 drops) and 2M aqueous potassium carbonate solution (10 ml). The mixture was stirred at room temperature under argon for 0.5 h, and Pd(PPh3)4 (0.010 g, 8.70*10 -3 mmol), heated to 90°C for 24h, poured the mixture into water and extracted with ethyl acetate three times. The organic layer was dried over anhydrous sodium sulfate. After the solvent was removed under reduced pressure, the residue was chromatographed on a silica gel column with petroleum ether / CH2Cl2 (volume ratio 3:1) as the eluent to obtain intermediate 1 (1.30 g, yield 68%).

[0060] The specific process of the preparation of tetraphenylethylene-isoquinoline compound Iso-TPECN3Qu is as follows: TPECN (1g, 2.6mmol) is added to a three-necked flask, and then 30mL of anhydrous ethanol is added, and dissolved under magnetic stirring. After fully dissolved, nitrogen is introduced, and isoquinoline-3-carboxaldehyde (0.41g, 2.6mmol) is added, and the temperature is raised to 80°C, and an appropriate amount of catalyst TBAH is added, and the reaction is carried out for 24h. After the reaction is completed, the filter is sucked and the filter residue is collected, and it is repeatedly washed with ethanol for 3 times to obtain a light yellow solid powder (1.3g, 80%). 1H NMR (500MHz, CDCl3) δ9.33 (s, 1H), 8.23 ​​(s, 1H), 8.01 (dd, J = 8.3, 1.2Hz, 1H), 7.91 (dd,J=8.3,1.1Hz,1H),7.78–7.64(m,3H),7.56–7.50(m,2H),7.17–7.02(m,17H). 13 C NMR (500MHz, CDCl3) δ152.68,146.13,145.33,143.44,143.38,143.27,142.09,140.58,139.92,135.81,132.23,132.05,131.39,1 31.32,131.04,128.69,128.56,127.93,127.85,127.80,127.71,127.52,126.87,126.72,126.67,125.55,121.81,117.83,113.30.

[0061] Synthesis of ISO-TPECN4Qu: TPECN (1 g, 2.6 mmol) and isoquinoline-4-carboxaldehyde (0.4086 g, 2.6 mmol) were added under nitrogen. After they were fully dissolved, an appropriate amount of catalyst tetrabutylammonium hydroxide (0.49 g, 0.0019 mmol) was added to the reaction solution. After the reaction was completed, vacuum filtration was performed. During this process, the mixture was rinsed three times with ethanol. After the filtration was completed, the filter residue was dried in an oven to obtain 1.30 g of yellow solid powder (yield was 83%).

[0062] 1 H NMR(500MHz, CDCl3)δ9.31(s,1H),8.97(d,J=1.1Hz,1H),8.09–8.02(m,2H),7.93(dd,J=8.4,1.0Hz,1H),7 .79(ddd,J=8.3,6.9,1.3Hz,1H),7.70(ddd,J=8.1,6.9,1.1Hz,1H),7.56–7.50(m,2H),7.22–7.02(m,17H). 13C NMR (500MHz, CDCl3) δ154.37,145.91,143.44,143.35,143.04,142.37,139.85,135.87,133.99,132.30,131.48,131.4 5,131.41,128.69,128.16,128.10,128.04,128.01,127.85,127.04,126.90,126.86,125.74,122.89,117.21,117.13.C 38 H 27 ESI+HRMS m / z calculated for N2: 511.2183 [M+H], found: 511.2183 [M+H].

[0063] Synthesis of ISO-TPECN5Qu: The method is similar to the above-mentioned synthesis of ISO-TPECN4Qu, wherein the raw material added is isoquinoline-5-carboxaldehyde, the isomer of isoquinoline-4-carboxaldehyde, and 1.20 g of light yellow solid is obtained with a yield of 71%.

[0064] 1 H NMR (500MHz, CDCl3) δ9.31 (d, J = 0.9Hz, 1H), 8.61 (d, J = 6.0Hz, 1H), 8.30 (dd, J = 7.3, 1. 1Hz,1H),8.12–8.04(m,2H),7.79–7.68(m,2H),7.55–7.49(m,2H),7.18–7.03(m,17H). 13 C NMR (500MHz, CDCl3) δ153.47,145.89,144.15,143.45,143.35,142.38,139.84,137.20,134.44,132.32,131.59,131.47,131.46,131. 40,130.98,130.42,130.10,128.71,128.09,128.01,127.85,127.23,127.03,126.90,126.86,125.67,117.47,116.48,116.32,1.16.C 38 H 27 ESI+HRMS m / z calculated for N2: 512.2181 [M+H], found: 512.2181 [M+H].

[0065] Synthesis of ISO-TPECN8Qu: The method is similar to the above-mentioned synthesis of ISO-TPECN4Qu, wherein the raw material added is isoquinoline-8-carboxaldehyde, the isomer of isoquinoline-4-carboxaldehyde, and 1.10 g of light yellow solid is obtained with a yield of 78%.

[0066] 1 H NMR (500MHz, CDCl3) δ9.44(d,J=1.0Hz,1H),8.64(d,J=5.6Hz,1H),8.26(s,1H),8.10(dd,J=7.2,1.1Hz,1H),7.91 (d,J=8.3Hz,1H),7.77(dd,J=8.3,7.2Hz,1H),7.72(dd,J=5.8,0.9Hz,1H),7.56–7.51(m,2H),7.21–7.02(m,17H). 13 C NMR (500MHz, CDCl3) δ148.53,145.99,144.02,143.45,143.43,143.33,142.41,139.85,137.20,136.17,132.35,132.17,131.48,13 1.45,131.41,130.23,129.01,128.19,128.10,128.02,127.84,127.08,126.90,126.85,126.59,125.71,121.17,117.37,117.07.C 38 H 27 ESI+HRMS m / z calculated for N2: 511.2177 [M+H], found: 511.2177 [M+H].

[0067] Example 1

[0068] In this example, an isoquinoline fiber membrane was prepared. 0.05g of tetraphenylethylene-isoquinoline compound Iso-TPECN3Qu and 1g of polymer (PLA) were weighed and dissolved in 8.95g of DMF / DCM (v / v=1 / 2) mixed solution to prepare an electrospinning solution. Then, the solution was loaded into a 10mL syringe and extruded from a spinneret at a speed of 1mL / h to form a filament under the action of high-voltage electrostatics. Among them, the spinning voltage was 17kV, the working distance was 13cm, and silicone oil paper was used as a grounding collector.

[0069] Example 2

[0070] In this example, an isoquinoline fiber membrane was prepared. 0.05g of tetraphenylethylene-isoquinoline compound Iso-TPECN3Qu and 1g of polymer (CA) were weighed and dissolved in 8.95g of DMF / DCM (v / v=1 / 2) mixed solution to prepare an electrospinning solution. Then, the solution was loaded into a 10mL syringe and extruded from a spinneret at a speed of 1mL / h to form a filament under the action of high-voltage electrostatics. Among them, the spinning voltage was 17kV, the working distance was 13cm, and silicone oil paper was used as a grounding collector.

[0071] Example 3

[0072] In this example, an isoquinoline fiber membrane was prepared. 0.05g of tetraphenylethylene-isoquinoline compound Iso-TPECN3Qu and 1g of polymer (polystyrene (PS)) were weighed and dissolved in 8.95g of DMF / DCM (v / v=1 / 2) mixed solution to prepare an electrospinning solution. Then, the solution was loaded into a 10mL syringe and extruded from a spinneret at a speed of 1mL / h to form a filament under the action of high-voltage electrostatics. Among them, the spinning voltage was 17kV, the working distance was 13cm, and silicone oil paper was used as a grounding collector.

[0073] Example 4

[0074] In this example, an isoquinoline fiber membrane is prepared, which is different from Example 1 in that the tetraphenylethylene-isoquinoline compound is Iso-TPECN4Qu.

[0075] Example 5

[0076] In this example, an isoquinoline fiber membrane is prepared, which is different from Example 1 in that the tetraphenylethylene-isoquinoline compound is Iso-TPECN5Qu.

[0077] Example 6

[0078] In this example, an isoquinoline fiber membrane is prepared, which is different from Example 1 in that the tetraphenylethylene-isoquinoline compound is Iso-TPECN8Qu.

[0079] Comparative Example 1

[0080] This example provides a fluorescent material, which is 0.05 g of an isoquinoline compound Iso-TPECN3Qu.

[0081] Comparative Example 2

[0082] This example provides a fluorescent material, which is 0.05 g of an isoquinoline compound Iso-TPECN4Qu.

[0083] Comparative Example 3

[0084] This example provides a fluorescent material, which is 0.05 g of an isoquinoline compound Iso-TPECN5Qu.

[0085] Comparative Example 4

[0086] This example provides a fluorescent material, which is 0.05 g of an isoquinoline compound Iso-TPECN8Qu.

[0087] Test example

[0088] This test example tests the acid-base stimulus response performance of the fiber membrane prepared in the example and the fluorescent material in the comparative example. The specific operation is as follows:

[0089] Take the samples of the embodiment and the comparative example and carry out fumigation treatment with acid vapor (HCl) and alkali vapor (NH3) under the same conditions, and test their response time and fluorescence change. At 25°C, put a small amount of hydrochloric acid solution or ammonia water in a closed desiccator (use hydrochloric acid aqueous solution, wherein the content of HCl is 36% to 38%; use ammonia water as the alkali solution, wherein the content of NH3 is 25% to 28%. Take 10 to 15 ml of hydrochloric acid or ammonia solution and place it in a desiccator of about 6.28 liters, wait for about 30 minutes at room temperature (about 25°C), and the container will be filled with acid or alkali vapor). After the acid vapor and ammonia vapor fill the desiccator, put the sample in a culture dish and put it in the desiccator, use a 365nm ultraviolet lamp to observe the fluorescence change, and record the response time.

[0090] The results showed that it takes a relatively long time for the Iso-TPECN3Qu compound to undergo acid-base stimulation testing in a powder state. This is because the acid vapor first contacts the outermost layer of the powder and takes time to diffuse to the inner layer.

[0091] The electron microscopy characterization results of PLA-Iso-TPECN3Qu fiber membrane are shown in Figure 1 As shown in the figure, it can be seen that the surface of the prepared composite fiber membrane is uniform and smooth, and no granular aggregates are observed, indicating that the Iso-TPECN3Qu compound has good compatibility with PLA, and the addition of the Iso-TPECN3Qu compound will not affect the spinning performance of PLA. At the same time, the Iso-TPECN3Qu compound is compounded with other polymers such as PS to prepare micro-nano fiber membranes in order to explore the fluorescence stability of the Iso-TPECN3Qu compound in different polymers. The results show that they all have good fluorescence stability. At the same time, by changing the mass of the Iso-TPECN3Qu compound, the micro-nano fiber membranes are compounded with different masses of PLA to prepare micro-nano fiber membranes in order to explore the effect of the content of the Iso-TPECN3Qu compound on the fluorescence properties of the micro-nano fiber membranes. The results are shown in Figure 2As shown in the figure, as the content of Iso-TPECN3Qu compound increases from 1% to 10% (mass ratio of Iso-TPECN3Qu: PLA, small molecule mass: polymer mass ratio = 0.01-0.1:1), the fluorescence color gradually shifts from 1% blue to 10% green. The experimental results show that the content of Iso-TPECN3Qu compound is positively correlated with the fluorescence performance of micro-nanofiber membrane.

[0092] The spun PLA-ISO-TPECNnQu micro-nanofiber membrane sample was named ISO-TPECNnQu-x. It was placed in a sealed HCl for 10 seconds. The acid-fumigated sample was cut into two equal parts, and the samples were named ISO-TPECNnQu-xh and ISO-TPECNnQu-xhn respectively. Then the sample named ISO-TPECNnQu-xhn was placed in a sealed ammonia vapor for 10 seconds, and the obtained sample was called ISO-TPECNnQu-xhn. Photos of ISO-TPECNnQu-x, ISO-TPECNnQu-xh and ISO-TPECNnQu-xhn were taken under ultraviolet light, and the fluorescence spectrum of these three samples was tested.

[0093] During the acid stimulation response experiment, the fluorescence color of the PLA-Iso-TPECN3Qu micro-nanofiber membrane changed from blue to light green after being fumigated with hydrochloric acid vapor for about 3 seconds (the results are shown in Figure 3 The maximum emission wavelength of fluorescence also shifted from 499nm to 559nm, a red shift of 60nm (the results are shown in Figure 4 NH3 vapor was used to deprotonate it, and its wavelength returned to its initial state. The shift of the fluorescence emission wavelength before and after the acid-base stimulation response did not decay significantly after 10 cycles (the results are shown in Figure 5 This indicates that the acid-base stimuli response performance of the PLA-Iso-TPECN3Qu micro-nanofiber membrane has good stability and repeatability. This experimental result shows that the larger surface area of ​​the electrospun micro-nanofiber significantly enhances the HCl sensing ability, and this reversible acid-base stimuli responsive micro-nanofiber film can be used in acid detection and anti-counterfeiting and other fields.

[0094] The effects of other embodiments are similar to those of Embodiment 1, and are not shown one by one to avoid redundancy.

[0095] After the initial powder of Iso-TPECN3Qu in Comparative Example 1 was fumigated with hydrochloric acid vapor, its fluorescence color changed significantly: the initial blue fluorescence changed to green fluorescence, and the emission wavelength also red-shifted from the initial 463nm to 510nm, indicating that the solid powder of Iso-TPECN3Qu has a significant acid stimulation response. Interestingly, when the acid-fumigated sample was deprotonated with ammonia vapor, it was found that the maximum emission wavelength of fluorescence further red-shifted (536nm) and did not fully return to the initial state. And its response time takes more than 10s.

[0096] The SEM images of the fiber membranes obtained in Examples 4 to 6 are as follows: Figures 6 to 8 As shown in the figure. It can be seen from the figure that the cross-section of the fiber membrane prepared by the scheme of the present invention is nearly circular, and the longitudinal cross-section of the fiber is smooth. In addition, the SEM images of the fiber membrane prepared by the embodiment of the present invention and the pure polymer fiber membrane are compared. The results show that even if the fiber membrane prepared by blending the tetraphenylethylene-isoquinoline compound and the polymer of the scheme of the present invention is prepared, there is no obvious difference compared with the pure polymer membrane, and they all have similar special-shaped fiber filament structures. Therefore, the presence of tetraphenylethylene-isoquinoline compounds (ISO-TPECNnQu) does not affect the fiber-forming performance of PLA.

[0097] The acid-base stimulation test of the fiber membranes prepared in Examples 4 to 6 is as follows: Fig. 9 As shown (test process is the same as before). Fig. 9 As can be seen from the upper left figure, the original PLA-ISO-TPECN4Qu micro-nanofiber membrane red-shifts 11nm from blue-green fluorescence (475nm) to yellow-green fluorescence (486nm) under 365nm ultraviolet light, showing obvious reversible acid-induced color change. Fig. 9 As can be seen in the upper right figure, the original PLA-ISO-TPECN5Qu micro-nano fiber membrane red-shifts 19nm from dark green fluorescence (484nm) to bright green fluorescence (511nm) under 365nm ultraviolet light, indicating that it has a certain reversible acid-induced color change performance, which is more obvious than that of PLA-ISO-TPECN4Qu. Fig. 9 As can be seen from the lower middle figure, the original PLA-ISO-TPECN8Qu micro-nanofiber membrane red-shifts 43nm from dark green fluorescence (490nm) to dark yellow fluorescence (533nm) under 365nm ultraviolet light, indicating that it has a certain reversible acid-induced color change property, which is more obvious than that of PLA-ISO-TPECN5Qu.

[0098] The acid-induced color-changing properties of Examples 4 to 6 and Comparative Examples 2 to 4 are shown in Table 3 below.

[0099] Table 3

[0100]

[0101]

[0102] As can be seen from the table above, the acid-base fumigation time of PLA-ISO-TPECNnQu is lower than that of ISO-TPECNnQu because the micro-nano fiber membrane has a large specific surface area, short detection time, and fast response speed, so it has a more obvious reversible acid-induced color change performance in a short time. Among the three PLA-ISO-TPECNnQu micro-nano fiber membranes, the acid-induced color change performance is: ISO-TPECN8Qu red-shifts from dark green fluorescence (490nm) to dark yellow fluorescence (533nm), ISO-TPECN5Qu red-shifts from dark green fluorescence (484nm) to bright green fluorescence (511nm), ISO-TPECN4Qu red-shifts from blue-green fluorescence (475nm) to yellow-green fluorescence (486nm), ISO-TPECN8Qu has the most obvious red shift, followed by ISO-TPECN5Qu, and can all be restored to or close to the state before acid fumigation by ammonia fumigation. All three compounds have good reversible acid-induced color change performance.

[0103] In summary, the present invention prepares PLA-Iso-TPECNnQu micro-nanofiber membrane by compounding isoquinoline derivatives with polylactic acid, and exhibits the same acid and alkali color-changing properties as the compound itself. However, unlike the powder state, the acid-fumigated film of the nanofiber membrane has good reversible properties, and its response time is greatly improved compared with the powder state compound.

[0104] The embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. An isoquinoline micro-nanofiber membrane, Features: The raw materials for preparing the fiber membrane include a polymer and a tetraphenylethylene-isoquinoline compound, and the general structural formula of the tetraphenylethylene-isoquinoline compound is as follows: Ar represents isoquinoline.

2. The isoquinoline micro-nano fiber membrane according to claim 1, Features: The structural formula of the tetraphenylethylene-isoquinoline compound is shown in one of the following formulas:

3. The isoquinoline micro-nano fiber membrane according to claim 1, Features: The polymer includes at least one of cellulose acetate, polystyrene, polyvinyl alcohol and polylactic acid; preferably, the mass ratio of the polymer to the tetraphenylethylene-isoquinoline compound is 1:0.01-0.

1.

4. The isoquinoline micro-nano fiber membrane according to claim 1, Features: The preparation raw material also includes a solvent, and the solvent is selected from a mixed solution of DMF and DCM.

5. A method for preparing a fiber membrane, Features: The steps include: Weighing tetraphenylethylene-isoquinoline compounds and polymers and dissolving them in a solvent to prepare an electrospinning solution, loading the solution into a syringe, and extruding the solution through a spinneret at a speed of 0.8 to 1.2 mL / h to form filaments under the action of high-voltage static electricity; wherein the spinning voltage is 15 to 20 kV and the working distance is 11 to 15 cm; The general structural formula of the tetraphenylethylene-isoquinoline compound is as follows: Ar represents isoquinoline.

6. Use of the fiber membrane according to any one of claims 1 to 4 in the field of detection or anti-counterfeiting.

7. The use according to claim 6, Features: The detection includes at least one of the following detection contents: 1) Acidic substances; 2) Alkaline substances.

8. The use according to claim 7, Features: The detection comprises the following steps: applying the detection content to the fiber membrane, irradiating the compound with an ultraviolet light source as an excitation light source, and observing the fluorescence change.

9. The use according to claim 8, Features: The applying comprises at least one of coating, dipping and fumigating.

10. The use according to claim 6, Features: The wavelength of the ultraviolet light source is 320nm to 405nm, preferably 345nm to 385nm, and more preferably 365nm.

Citation Information

Patent Citations

  • Tetraphenyl ethylene Schiff base red-light zinc ion probe and preparation method and application

    CN106928141A

  • Tetraphenylethylene-8-hydroxyquinoline compound, and preparation method and application thereof

    CN110467570A

  • Photoinduced crystallization isoquinoline salt compound, preparation method and application thereof, and preparation method of nanocrystal

    CN112079776A

  • Aggregation-induced light-emitting electric activity polyamide acid polymer, nanofiber detection test strip and application of nanofiber detection test strip

    CN113004519A

  • Fluorescent material and application thereof

    CN114315732A