Light ultrathin metal vacuum insulation sleeve and processing method thereof
By setting seals in vacuum stainless steel tubes for vacuum brazing, the problem of thermal insulation effect and welded joints of small products is solved, the thermal insulation requirements of different shapes can be adapted, and the reliability and applicability of the product are improved.
Patent Information
- Application Number
- CN202410991951.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
AI Technical Summary
Existing vacuum stainless steel pipes have limited thermal insulation effect in small products, and due to excessive thickness, the residual stress at the welded joints is large and easy to break or leak. The outer pipe is prone to cracking after shrinking, and it is only suitable for round pipes and cannot be used. Adapt to the thermal insulation needs of different shapes.
The first and second sets of the same length are used. The radius of the second set is smaller than that of the first set. A vacuum zone is formed between the two, and seals are set at both ends for vacuum brazing to solve the problem of welded joints and lack of shape adaptability. problem.
Through the vacuum brazing seal, the residual stress of the welded joint is reduced, the air leakage problem is avoided, and the vacuum insulation sleeve can adapt to the heat insulation requirements of different shapes, improving the applicability and reliability of the product.
Smart Images

Figure CN118729092A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of vacuum insulation, and in particular relates to a lightweight ultra-thin metal vacuum insulation sleeve and a processing method thereof. Background Art
[0002] At present, heat insulation is needed in many fields. Traditional heat insulation generally uses vacuum glass and rock wool vacuum stainless steel for heat insulation. Each material has its own application segment. For the sake of lightweight and processing considerations, vacuum stainless steel pipes will be used for heat insulation. The existing vacuum stainless steel is widely used in fields such as thermos cups. The thickness of the vacuum stainless steel used is relatively thick. The processing technology generally uses direct welding or uses a stainless steel sealing machine for processing, and then welding.
[0003] However, when it is applied to smaller products, the scope of heat insulation is limited, and there are requirements for weight. Ultra-thin stainless steel vacuum tubes are needed for heat insulation. At this time, the existing direct welding or external tube shrinkage treatment and welding technology cannot meet the product use requirements. There are many welding points at the direct welding joints, and the residual stress is large, which will cause problems such as breakage and gas leakage. The use of external tube shrinkage will cause stainless steel to be too thin and easy to crack, and it is easy to leak in the later stage, and the product defective rate is very high. At the same time, the external tube shrinkage is suitable for round stainless steel tubes, but not other shapes. The stainless steel vacuum sleeve is too small and too thin and cannot be used. There are many restrictions, so it is urgent to find a processing method that can solve the above problems. Summary of the invention
[0004] The object of the present invention is to provide a lightweight ultra-thin metal vacuum insulation sleeve and a processing method thereof, aiming to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above-mentioned purpose, an embodiment of the present invention provides a lightweight, ultra-thin metal vacuum insulation sleeve, comprising a first sleeve and a second sleeve of the same length; the radius of the second sleeve is smaller than that of the first sleeve, the second sleeve is arranged inside the first sleeve, and there is a vacuum area between the first sleeve and the second sleeve, and it is characterized in that a seal is provided at both ends of the first sleeve and the second sleeve, and the two seals are vacuum welded between the first sleeve and the second sleeve to seal the vacuum area.
[0006] Optionally, the first kit and the second kit are made of stainless steel.
[0007] Optionally, the thickness of the first set is 0.05-0.2 mm.
[0008] Optionally, the second set has a thickness of 0.05-0.2 mm.
[0009] Optionally, the sealing member is a flange member.
[0010] Optionally, the two sealing members are respectively interference fit with two ends of the first set and the second set to seal the vacuum area.
[0011] Optionally, a method for processing a lightweight ultra-thin metal vacuum insulation sleeve comprises the following steps:
[0012] S1 Preparation: prepare the brazing material, and use solvent to remove grease and dirt on the surface of the first set, the second set and the sealing part, and use sandpaper, polishing wheel and other tools to remove oxides and impurities on the surface to increase the wettability of the brazing material;
[0013] S2: assembling and fixing, the sealing member is interference-fitted with the first set and the second set to obtain a preliminary product, and then both ends of the preliminary product are respectively immersed in the solder paste for 1 to 2 mm, so that both ends are evenly covered with a layer of solder paste, and then dried, and after drying, the preliminary product is fixed with a clamp;
[0014] S3 brazing, put the preliminary product into the brazing furnace, start the vacuum pump, and evacuate to 10 -4 ~10 -6 Torr, then preheat, further increase the temperature after preheating, and keep it for 20 to 60 minutes, and then slowly cool to room temperature to obtain a finished vacuum insulation sleeve;
[0015] S4 post-processing, cleaning the vacuum insulation sleeve to remove residual solder and oxides.
[0016] Optionally, in the S1 preparation step, the solder is selected from one of silver-based solder, copper-based solder and nickel-based solder.
[0017] Optionally, in the S1 preparation step, the solvent is selected from one or a mixture of acetone, isopropanol and ethanol.
[0018] Optionally, in the S3 brazing step, the preheating temperature is 300-500° C., the preheating time is 10-20 minutes, and the temperature is further increased to 700-1300° C. after preheating.
[0019] Compared with the prior art, the above one or more technical solutions in the lightweight ultra-thin metal vacuum insulation sleeve and the processing method thereof provided in the embodiment of the present invention have at least one of the following technical effects:
[0020] The present invention solves the problem in the prior art that the first and second sets are too thin and easy to crack after the outer tube shrinkage treatment, and easy to leak in the later stage by setting the sealing member to be vacuum brazed with the two ends of the first set and the second set respectively. It also solves the problem that there are many welding points at the direct welding joint, the residual stress is large, and there will be fracture and gas leakage. At the same time, the shapes of the sealing member, the first set and the second set can be varied, which solves the disadvantage that the outer tube shrinkage can only be round tube-shaped. The vacuum insulation sleeve of the present invention can meet the needs of different product insulation shapes. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0022] Figure 1 It is a schematic diagram of the structure of the present invention.
[0023] Among them, the reference numerals in the figure are:
[0024] 100, first set;
[0025] 200, second set;
[0026] 300. Seals. DETAILED DESCRIPTION
[0027] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the embodiments of the present invention, and should not be construed as limiting the present invention.
[0028] In the description of the embodiments of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0029] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0030] In the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present invention can be understood according to specific circumstances.
[0031] according to Figure 1 As shown, a lightweight ultra-thin metal vacuum insulation sleeve includes a first sleeve 100 and a second sleeve 200 of the same length; the radius of the second sleeve 200 is smaller than that of the first sleeve 100, and the second sleeve 200 is sleeved inside the first sleeve 100, and there is a vacuum zone between the first sleeve 100 and the second sleeve 200, characterized in that a sealing member 300 is provided at both ends of the first sleeve 100 and the second sleeve 200, and the two sealing members 300 are vacuum welded between the first sleeve 100 and the second sleeve 200 to seal the vacuum zone. The first sleeve 100 and the second sleeve 200 are made of stainless steel. The two sealing members 300 are respectively interference fit with the two ends of the first sleeve 100 and the second sleeve 200 to seal the vacuum zone.
[0032] Specifically, the present invention solves the problem in the prior art that the first set 100 and the second set 200 are too thin and easy to crack after the outer tube shrinkage treatment, and easy to leak in the later stage by setting the seal 300 to be vacuum brazed with the two ends of the first set 100 and the second set 200 respectively. It also solves the problem that there are many welding points at the direct welding joint, the residual stress is large, and there will be fracture and gas leakage. At the same time, the shapes of the seal 300, the first set 100 and the second set 200 can be varied, which solves the disadvantage that the outer tube shrinkage can only be a round tube. The vacuum insulation sleeve of the present invention can meet the needs of different product insulation shapes.
[0033] It can be understood that the cross-sectional shape of the vacuum area formed by the sealing member 300, the first set 100 and the second set 200 is adapted to each other. At the same time, the sealing member 300 is a flange member, and the material of the sealing member can be carbon steel, stainless steel, cast iron, etc., as long as the material can be welded with the first set 100 and the second set 200. As a preferred material, stainless steel can be selected.
[0034] Furthermore, the thickness of the first kit 100 is 0.05 to 0.2 mm. The thickness of the second kit 200 is 0.05 to 0.2 mm. Both the first kit 100 and the second kit 200 are ultra-thin stainless steel. In many daily products, the insulation space is not very large, so a smaller vacuum insulation sleeve is needed. At the same time, some products need to be carried, and there is also a need for lightweighting. It is necessary to make the thickness of the first kit 100 and the second kit 200 thinner to meet the needs of the product. At the same time, stainless steel can meet the demand for lightweighting. In portable products, lightweighting has always been the goal that production has been constantly pursuing. If other materials such as insulating glass are used, the weight will increase a lot, which will directly affect the quality of the overall product and bring a bad experience to users.
[0035] A method for processing a lightweight ultra-thin metal vacuum insulation sleeve comprises the following steps:
[0036] S1 preparation work, prepare the solder, and use a solvent to remove grease and dirt on the surface of the first set 100, the second set 200 and the sealing member 300, and use sandpaper, a polishing wheel and other tools to remove oxides and impurities on the surface to increase the wettability of the solder;
[0037] S2: assembling and fixing, the sealing member 300 is assembled with the first set 100 and the second set 200 by interference fit to obtain a preliminary product, and then both ends of the preliminary product are respectively immersed in the solder paste for 1 to 2 mm, so that both ends are evenly covered with a layer of solder paste, and then dried, and after drying, the preliminary product is fixed with a clamp;
[0038] S3 brazing, put the preliminary product into the brazing furnace, start the vacuum pump, evacuate to the required vacuum degree, and then preheat. After preheating, further increase the temperature and keep it for 20 to 60 minutes, and then slowly cool it to room temperature to obtain the finished vacuum insulation sleeve;
[0039] In step S4 post-processing, the vacuum insulation sleeve is cleaned to remove residual solder and oxides. In step S1 preparation, the solder is selected from one of silver-based solder, copper-based solder and nickel-based solder. In step S1 preparation, the solvent is selected from one or a mixture of acetone, isopropanol and ethanol. In step S3 brazing, the vacuum is evacuated to 10 -4 ~10 -6In the S3 brazing step, the preheating temperature is 300-500°C for 10-20 minutes, and the temperature is further increased to 700-1300°C after preheating.
[0040] Specifically, solvent cleaning and physical grinding and polishing can increase the wettability of the surface and the solder to remove oxides and impurities on the surface, which can improve welding and reduce the risk of gas leakage in the later stage. Preheating is to remove volatile substances and residual gases on the surface of the workpiece. The heating temperature of different solders is different (silver-based solder is about 700-800℃, copper-based solder is about 850-1200℃, and nickel-based solder is about 850-1300℃). The purpose of maintaining the temperature is to ensure that the solder fully wets the parent material and forms a firm joint. The purpose of slow cooling is to avoid excessive internal stress and cracks.
[0041] Example 1
[0042] The thickness of the first set 100 is 0.05 mm. The thickness of the second set 200 is 0.05 mm.
[0043] A method for processing a lightweight ultra-thin metal vacuum insulation sleeve comprises the following steps:
[0044] S1 preparation work, prepare the solder, and use a solvent to remove grease and dirt on the surface of the first set 100, the second set 200 and the sealing member 300, and use sandpaper, a polishing wheel and other tools to remove oxides and impurities on the surface to increase the wettability of the solder;
[0045] S2: assembling and fixing, the sealing member 300 is assembled with the first set 100 and the second set 200 by interference fit to obtain a preliminary product, and then both ends of the preliminary product are respectively immersed in the solder paste for 1 mm, so that both ends are evenly covered with a layer of solder paste, and then dried, and after drying, the preliminary product is fixed with a clamp;
[0046] S3 brazing, put the preliminary product into the brazing furnace, start the vacuum pump, evacuate to the required vacuum degree, and then preheat, further increase the temperature after preheating, and keep it for 20 minutes, and then slowly cool it to room temperature to obtain the finished vacuum insulation sleeve;
[0047] In S4 post-processing, the vacuum insulation sleeve is cleaned to remove residual solder and oxides. In the S1 preparation step, the solder is silver-based solder. In the S1 preparation step, acetone is used as the solvent. In the S3 brazing step, vacuum is drawn to 10 -4 In the S3 brazing step, the preheating temperature is 300°C, the preheating time is 10 minutes, and the temperature is further increased to 700°C after preheating.
[0048] Example 2
[0049] The thickness of the first set 100 is 0.1 mm. The thickness of the second set 200 is 0.2 mm.
[0050] A method for processing a lightweight ultra-thin metal vacuum insulation sleeve comprises the following steps:
[0051] S1 preparation work, prepare the solder, and use a solvent to remove grease and dirt on the surface of the first set 100, the second set 200 and the sealing member 300, and use sandpaper, a polishing wheel and other tools to remove oxides and impurities on the surface to increase the wettability of the solder;
[0052] S2: assembling and fixing, the sealing member 300 is assembled with the first set 100 and the second set 200 by interference fit to obtain a preliminary product, and then both ends of the preliminary product are respectively immersed in the solder paste for 2 mm, so that both ends are evenly covered with a layer of solder paste, and then dried, and after drying, the preliminary product is fixed with a clamp;
[0053] S3 brazing, put the preliminary product into the brazing furnace, start the vacuum pump, evacuate to the required vacuum degree, and then preheat, further increase the temperature after preheating, and keep it for 40 minutes, and then slowly cool it to room temperature to obtain the finished vacuum insulation sleeve;
[0054] In S4 post-processing, the vacuum insulation sleeve is cleaned to remove residual solder and oxides. In the S1 preparation step, copper-based solder is used as solder. In the S1 preparation step, isopropyl alcohol is used as solvent. In the S3 brazing step, vacuum is drawn to 10 -5 In the S3 brazing step, the preheating temperature is 400°C, the preheating time is 15 minutes, and the temperature is further increased to 1000°C after preheating.
[0055] Example 3
[0056] The thickness of the first set 100 is 0.2 mm. The thickness of the second set 200 is 0.1 mm.
[0057] A method for processing a lightweight ultra-thin metal vacuum insulation sleeve comprises the following steps:
[0058] S1 preparation work, prepare the solder, and use a solvent to remove grease and dirt on the surface of the first set 100, the second set 200 and the sealing member 300, and use sandpaper, a polishing wheel and other tools to remove oxides and impurities on the surface to increase the wettability of the solder;
[0059] S2: assembling and fixing, the sealing member 300 is assembled with the first set 100 and the second set 200 by interference fit to obtain a preliminary product, and then both ends of the preliminary product are respectively immersed in the solder paste by 1.5 mm, so that both ends are evenly covered with a layer of solder paste, and then dried, and after drying, the preliminary product is fixed with a clamp;
[0060] S3 brazing, put the preliminary product into the brazing furnace, start the vacuum pump, evacuate to the required vacuum degree, and then preheat, further increase the temperature after preheating, and keep it for 60 minutes, and then slowly cool it to room temperature to obtain the finished vacuum insulation sleeve;
[0061] In S4 post-processing, the vacuum insulation sleeve is cleaned to remove residual solder and oxides. In the S1 preparation step, the solder is selected from one of the nickel-based solders. In the S1 preparation step, ethanol is selected as the solvent. In the S3 brazing step, the vacuum is evacuated to 10 -6 In the S3 brazing step, the preheating temperature is 500°C, the preheating time is 20 minutes, and the temperature is further increased to 1300°C after preheating.
[0062] Example 4
[0063] The thickness of the first set 100 is 0.1 mm. The thickness of the second set 200 is 0.1 mm.
[0064] A method for processing a lightweight ultra-thin metal vacuum insulation sleeve comprises the following steps:
[0065] S1 preparation work, prepare the solder, and use a solvent to remove grease and dirt on the surface of the first set 100, the second set 200 and the sealing member 300, and use sandpaper, a polishing wheel and other tools to remove oxides and impurities on the surface to increase the wettability of the solder;
[0066] S2: assembling and fixing, the sealing member 300 is assembled with the first set 100 and the second set 200 by interference fit to obtain a preliminary product, and then both ends of the preliminary product are respectively immersed in the solder paste for 2 mm, so that both ends are evenly covered with a layer of solder paste, and then dried, and after drying, the preliminary product is fixed with a clamp;
[0067] S3 brazing, put the preliminary product into the brazing furnace, start the vacuum pump, evacuate to the required vacuum degree, and then preheat, further increase the temperature after preheating, and keep it for 30 minutes, and then slowly cool it to room temperature to obtain the finished vacuum insulation sleeve;
[0068] In S4 post-processing, the vacuum insulation sleeve is cleaned to remove residual solder and oxides. In the S1 preparation step, the solder is a silver-based solder. In the S1 preparation step, the solvent is a mixture of acetone and isopropanol. In the S3 brazing step, the vacuum is evacuated to 10 -5 In the S3 brazing step, the preheating temperature is 400°C, the preheating time is 15 minutes, and the temperature is further increased to 800°C after preheating.
[0069] The above content is a further detailed description of the present invention in combination with specific preferred implementation methods, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, its architecture can be flexible and can derive a series of products. Just making a few simple deductions or substitutions should be regarded as belonging to the scope of patent protection of the present invention determined by the submitted claims.
Claims
1. A lightweight ultra-thin metal vacuum insulation sleeve, comprising a first sleeve and a second sleeve of the same length; the radius of the second sleeve is smaller than that of the first sleeve, the second sleeve is arranged inside the first sleeve, and there is a vacuum area between the first sleeve and the second sleeve, characterized in that: Both ends of the first set and the second set are provided with a sealing member, and the two sealing members are vacuum welded between the first set and the second set to seal the vacuum area.
2. The lightweight ultra-thin metal vacuum insulation sleeve according to claim 1, characterized in that: The first set and the second set are made of stainless steel.
3. The lightweight ultra-thin metal vacuum insulation sleeve according to claim 1, characterized in that: The thickness of the first set is 0.05-0.2 mm.
4. The lightweight ultra-thin metal vacuum insulation sleeve according to claim 1, characterized in that: The thickness of the second set is 0.05-0.2 mm.
5. The lightweight ultra-thin metal vacuum insulation sleeve according to claim 1, characterized in that: The sealing member is a flange member.
6. The lightweight ultra-thin metal vacuum insulation sleeve according to claim 1, characterized in that: The two sealing members are respectively interference-fitted with two ends of the first set and the second set to seal the vacuum area.
7. A method for processing a lightweight ultra-thin metal vacuum insulation sleeve, characterized in that: The steps include: S1 Preparation: prepare the brazing material, and use solvent to remove grease and dirt on the surface of the first set, the second set and the sealing part, and use sandpaper, polishing wheel and other tools to remove oxides and impurities on the surface to increase the wettability of the brazing material; S2: assembling and fixing, the sealing member is interference-fitted with the first set and the second set to obtain a preliminary product, and then both ends of the preliminary product are respectively immersed in the solder paste for 1 to 2 mm, so that both ends are evenly covered with a layer of solder paste, and then dried, and after drying, the preliminary product is fixed with a clamp; S3 brazing, put the preliminary product into the brazing furnace, start the vacuum pump, and evacuate to 10 -4 ~10 -6 Torr, then preheat, further increase the temperature after preheating, and keep it for 20 to 60 minutes, and then slowly cool to room temperature to obtain a finished vacuum insulation sleeve; S4 post-processing, cleaning the vacuum insulation sleeve to remove residual solder and oxides.
8. The method for processing a lightweight ultra-thin metal vacuum insulation sleeve according to claim 6, characterized in that: In the preparation step S1, the solder is selected from one of silver-based solder, copper-based solder and nickel-based solder.
9. The method for processing a lightweight ultra-thin metal vacuum insulation sleeve according to claim 6, characterized in that: In the preparation step S1, the solvent is selected from one or a mixture of acetone, isopropanol and ethanol.
10. The method for processing a lightweight ultra-thin metal vacuum insulation sleeve according to claim 6, characterized in that: In the S3 brazing step, the preheating temperature is 300-500° C., the preheating time is 10-20 minutes, and the temperature is further increased to 700-1300° C. after preheating.
Citation Information
Patent Citations
Manufacturing process for vacuum heat preservation titanium cup
CN109175746A
Method and system for generating vacuum cup based on vacuum brazing furnace
CN113600951A
Super low temperature fluid carries special metal hose
CN205479805U
Anti-freezing composite water supply pipeline
CN210687437U
High-temperature and high-pressure steam vacuum heat insulation pipeline connecting structure for ship
CN214305741U