High-polymer-material high-sensitivity flexible tension sensor as well as preparation method and application thereof
Through the design of composite sandwich structure and polymer materials, the problem of easy damage and low sensitivity of flexible tension sensors is solved, and a high-sensitivity and high-strength flexible tension sensor is realized, which is suitable for monitoring applications in a variety of environments and overcomes the temperature problem. and humidity effects.
Patent Information
- Application Number
- CN202410705187.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
AI Technical Summary
Existing flexible tension sensors are easily damaged, have low strength and low sensitivity, are not suitable for a wide range of environments, and are greatly affected by temperature and humidity.
The polymer material flexible tension sensor adopts a composite sandwich structure, including a serpentine-shaped conductive film and a polymer material outer layer. It is prepared by 3D printing and laser cutting, combined with hot pressing and adhesive packaging technology, to achieve the natural texture of the conductive film. Rebound and compression to improve the sensitivity and stability of the sensor.
A flexible tension sensor with high sensitivity and strength is achieved, which can maintain stable performance in various environments. It is suitable for applications such as aircraft and human body monitoring, and is not affected by temperature and humidity.
Smart Images

Figure CN118730353A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flexible sensors, and in particular relates to a highly sensitive flexible tension sensor made of polymer materials and a preparation method and application thereof. Background Art
[0002] In recent years, high-performance wearable strain sensors have attracted much attention from academia and industry. With the popularization of smart electronic devices, strain sensors have been widely used in flexible electronic skin, human activity monitoring, speech recognition, and intelligent robots.
[0003] With the rapid development of flexible electronic technology, the requirements for flexible sensing materials are gradually increasing. Currently, the sensors reported mainly include resistive tension sensors, piezoelectric pressure sensors, and triboelectric pressure sensors. Piezoelectric pressure sensors and triboelectric pressure sensors have the disadvantage of being unable to detect dynamic loads, while resistive tension sensors are easily affected by changes in external environmental temperature or humidity, and are prone to problems such as low sensitivity, aging, and damage due to the limitations of sensitive materials. Therefore, it is of great practical significance to develop flexible tension sensors that are not affected by temperature and humidity, have high strength, high stability, and a wide range of applications. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a polymer material high-sensitivity flexible tension sensor and its preparation method and application, so as to solve the shortcomings of the existing flexible tension sensor such as easy damage, low strength, low sensitivity and not being widely applicable. The polymer material high-sensitivity flexible tension sensor provided by the present invention has high strength and sensitivity and can be applied to most environments.
[0005] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] The present invention provides a highly sensitive flexible tension sensor made of polymer material, which is a composite sandwich structure, including a serpentine-arranged conductive film and a polymer material outer layer arranged on both sides of the conductive film, wherein electrodes are connected to both ends of the serpentine-arranged conductive film.
[0007] The serpentine-arranged conductive film is a thermoplastic polyester elastomer pre-prepared by 3D printing and processed by a hot press and a laser cutting machine.
[0008] The polymer material high-sensitivity flexible tensile sensor has a tensile strength of 10.21-11.36 MPa and a sensitivity of 74-480. When the strain is 10%, the resistance change rate is 100-9800%. When the strain is 2%, it can be cycled 2000 times. When subjected to cyclic loads, the resistance change can remain stable. When subjected to 1-11J energy impact, the resistance change remains at 20%-160%.
[0009] The present invention provides a highly sensitive flexible tension sensor made of polymer material; the polymer material outer layer of the highly sensitive flexible tension sensor belongs to the information function layer, has high strength, excellent wear resistance, and can adapt to most harsh environments. The conductive film is encapsulated by utilizing the uniformly stretched polymer material outer layer, and after encapsulation, the polymer material outer layer drives the serpentine-arranged conductive film to rebound naturally, thereby compressing the serpentine-arranged conductive film, achieving a sudden change in resistance of the conductive layer, and further achieving highly sensitive sensing.
[0010] The polymer material high-sensitivity flexible tension sensor of the present invention is used as a monitoring device sensor for aircraft structures or a monitoring device sensor for human bodies.
[0011] The present invention provides a method for preparing a high-sensitivity flexible tensile sensor made of a polymer material, comprising the following steps:
[0012] S1: 3D printing the elastomer conductive coil into a prefabricated conductive film;
[0013] S2: hot pressing and vulcanizing the prefabricated conductive film into a conductive film;
[0014] S3: Laser cutting the conductive film into a serpentine structure and connecting electrodes at two ends;
[0015] S4: After the pure polymer elastomer material is uniformly stretched to obtain the outer layer of the polymer material, the conductive film is encapsulated with adhesive, and the film is allowed to rebound naturally after encapsulation;
[0016] S5: The packaged conductive film is vacuum dried to obtain a highly sensitive flexible tensile sensor made of polymer material.
[0017] Preferably, in S1, the elastomer is a thermoplastic polyester elastomer.
[0018] Preferably, in S1, the printing technology used in 3D printing is preferably fused deposition, the temperature of the printer nozzle is preferably 150-400° C., more preferably 170-250° C. The base plate temperature is preferably 10-50° C., more preferably 20-40° C.
[0019] Preferably, in said S1, the thickness of the prefabricated conductive film obtained by printing is preferably 0.5 to 1 mm.
[0020] Preferably, in S2, the temperature of the hot press is preferably 150-300°C, more preferably 200-250°C, the time is preferably 20-50s, and the hot press pressure is 2-3Mpa.
[0021] Preferably, in S2, the thickness of the conductive film prepared by vulcanization is preferably 0.25 to 0.5 mm.
[0022] Preferably, in S3, the serpentine arrangement structure is formed by the following technical scheme: a laser is used to cross-cut the closed port with the cutting port as the closed port; the coupling distance of the serpentine arrangement structure is preferably 0.5-2 mm, and the parallel coupling distance is preferably 4-30 mm. The laser cutting speed is preferably 40-60 mm / s, and the power is preferably 15%-25%. The electrode material is selected from one or more of platinum, copper, gold, and silver.
[0023] Preferably, in S4, the uniform stretching length is preferably 10% to 30% of the original length. The pure polymer elastomer is preferably a thermoplastic elastomer, more specifically one or more of thermoplastic polyester elastomer, polyurethane thermoplastic elastomer, and thermoplastic vulcanized rubber.
[0024] Preferably, in S4, the viscose is acrylic acid.
[0025] Preferably, in S5, the drying temperature is 100-150° C. and the drying time is 15-30 min.
[0026] Compared with the prior art, the present invention provides a highly sensitive flexible tensile sensor made of polymer material and its preparation method and application, which has the following beneficial effects:
[0027] The polymer material high-sensitivity flexible tensile sensor provided by the present invention benefits from the excellent mechanical properties of the polymer elastomer, has good flexibility, can adapt to various curved surfaces and shapes, and has good plasticity and adaptability. In addition, the polymer elastomer has low rigidity, is not easily deformed, can maintain high accuracy and repeatability, and can be used for high-precision measurement and control. In addition, thanks to the wear resistance of the polymer elastomer, the prepared sensor has excellent durability and can maintain stability and reliability during long-term use. Compared with other flexible materials, the cost of the polymer elastomer is relatively low, making it possible to invest in large-scale industrial production. The results of the embodiments show that the polymer material high-sensitivity flexible tensile sensor provided by the present invention can maintain a high resistance change under small strains.
[0028] The present invention uniformly stretches the polymer elastomer, uses the uniformly stretched elastomer to encapsulate the polymer serpentine conductive film, and allows it to rebound naturally after encapsulation. Thanks to the rebound of the outer layer and the serpentine structure of the conductive film, the resistance of the information function layer changes significantly after being strained. The current path changes from a straight line connecting two sections to a serpentine structure before being compressed, and the sensing performance of the sensor is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A physical picture of a highly sensitive flexible tensile sensor made of a polymer material prepared in Example 1 of the present invention;
[0030] Figure 2 The present invention is a flow chart of the operation steps of the method for preparing a highly sensitive flexible tensile sensor made of polymer materials;
[0031] Figure 3 These are the model diagrams that need to be imported in the laser printing step in the embodiments of the present invention; (a) is the model diagram of Embodiment 1; (b) is the model diagram of Embodiment 2; (c) is the model diagram of Embodiment 3; (d) is the model diagram of Embodiment 4; and (e) is the model diagram of Embodiment 1.
[0032] Figure 4 This is a test diagram of a polymer material high-sensitivity flexible tensile sensor prepared in Example 1 of the present invention subjected to an 11J energy impact test;
[0033] Figure 5 This is a graph of a polymer material highly sensitive flexible tensile sensor prepared in Example 1 of the present invention undergoing a 2% cyclic deformation test. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with the embodiments and drawings.
[0035] The present invention provides the polymer material high-sensitivity flexible tension sensor. The polymer material high-sensitivity flexible tension sensor provided by the present invention has high sensitivity, repeatability and reliability, and can be adapted to most complex environments.
[0036] The present invention provides a method for preparing the polymer material highly sensitive flexible tension sensor described in the above scheme, comprising the following steps:
[0037] (1): 3D printing the elastomer conductive coil into a prefabricated conductive film;
[0038] (2): hot pressing and vulcanizing the prefabricated conductive film into a conductive film;
[0039] (3): Laser cutting the conductive film into a serpentine-shaped structure, and connecting electrodes at both ends of the serpentine-shaped conductive film;
[0040] (4): After the pure polymer elastomer material is uniformly stretched to obtain the outer layer of the polymer material, the conductive film is encapsulated by using adhesive;
[0041] (5): The encapsulated conductive film is vacuum dried to obtain a highly sensitive flexible tensile sensor made of polymer material
[0042] The present invention uses 3D printing technology to prepare the elastomeric conductive coil into a prefabricated conductive film. In the present invention, the elastomer is selected from a thermoplastic polyester elastomer. The present invention has no special requirements on the source of the polymer elastomer, and the corresponding products commercially available in the field can be used. In the present invention, the nozzle temperature of the printer is preferably 150-400°C, more preferably 170°C-250°C. The bottom plate temperature is preferably 10-50°C, more preferably 20°C-40°C. The present invention has no special requirements on the source of the elastomeric conductive coil, and the corresponding products commercially available in the field can be used. The thickness of the prefabricated conductive film prepared by printing is preferably 0.5-1mm.
[0043] The present invention heat-presses and vulcanizes the prefabricated conductive film into a conductive film. In the present invention, the temperature of the hot press is preferably 150-300°C, more preferably 200-250°C, the time is preferably 20-50s, and the thickness of the prefabricated conductive film is preferably 0.25-0.5mm.
[0044] The present invention uses a laser machine to cut the conductive film into a serpentine structure. The coupling distance of the serpentine structure is preferably 0.5 to 2 mm, more preferably 0.75 to 1.5 mm, and the parallel coupling distance is preferably 4 to 30 mm. The laser cutting speed is preferably 40 to 60 mm / s, and the power is preferably 15% to 25%. After the cutting is completed, a serpentine conductive film is obtained. After the two sections of the serpentine conductive film are thinly coated with conductive silver paste, electrodes are pasted, and the electrode material is selected from one or more of platinum, copper, gold, and silver.
[0045] The present invention uses viscose to encapsulate the conductive film and the electrode after pre-stretching the pure polymer elastomer material. The pure polymer elastomer is preferably a polyurethane thermoplastic elastomer with a uniform stretch length of preferably 10% to 30%. The pure polymer elastomer is preferably one or more of a thermoplastic polyester elastomer, a polyurethane thermoplastic elastomer, and polylactic acid. The encapsulation glue uses acrylic glue to bond the polymer outer layer and the conductive film. The present invention has no special requirements for the acrylic glue, and the corresponding products commercially available in the field can be used. The present invention uses upper and lower layers of elastomers with a pre-stretch length of preferably 10% to 30% to encapsulate the prepared serpentine conductive film and electrodes to form a sandwich structure.
[0046] The present invention vacuum dries the serpentine elastic conductive film, the drying temperature is preferably 100-150°C, the time is 15-30 minutes, and the drying atmosphere is selected as air. After the drying is completed, the film is safely taken out to obtain a high-sensitivity flexible tensile sensor made of polymer materials.
[0047] The present invention provides a method for preparing the above-mentioned polymer material highly sensitive flexible tension sensor. The preparation method provided by the present invention is simple, has relatively loose conditions, has excellent operability, can further realize continuous preparation, and is conducive to industrial production.
[0048] The polymer material highly sensitive flexible tension sensor and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0049] Example 1
[0050] A method for preparing a highly sensitive flexible tensile sensor made of polymer material, the flow chart of which is shown in Figure 2 , including the following steps:
[0051] (1) A 40×80×0.5 mm cuboid was designed and modeled, and then imported into a 3D printer to 3D print the thermoplastic polyurethane elastomer conductive coil into a prefabricated conductive film. The printer nozzle temperature was set to 210°C, and the base plate temperature was set to 30°C. After printing, ultrasonic cleaning was performed for 20 minutes and the prefabricated conductive film was obtained by drying.
[0052] (2) Set the temperature of the upper and lower clamping plates of the hot press to 220°C and the time to 30 seconds. After the hot press is heated to the set temperature, place the prefabricated conductive film obtained in step (1) between the upper and lower racks and clamp the clamping plates. Then lock the overflow valve and increase the displayed pressure to 2.1 MPa. Wait for the hot pressing time to end and safely remove the conductive film.
[0053] (3) The designed pattern ( Figure 3 (a)) is imported into the laser cutting machine. The cross-shaped dimensions in the figure are as follows Figure 3 (a) A laser is used to cross-cut the conductive film with the cutting port as a closed port to form a serpentine structure. The power of the laser cutting machine is set to 18%, and the scanning speed is set to 50 mm / s. After the laser cutting is completed, a serpentine conductive film with a coupling distance of 1 mm and a parallel coupling distance of 13 mm is obtained. After obtaining the serpentine conductive film, a thin layer of conductive silver paste is applied to the two sections of the serpentine structure to enhance the conductive performance, and then the copper electrode is pasted.
[0054] (4) Take two sections of pure thermoplastic polyurethane elastomer, cut them into rectangles with a width of 22 mm and a length of 44 mm, stretch both sections evenly to 50 mm, sandwich the serpentine conductive film prepared in step (3) and the electrode in the middle, and encapsulate them with acrylic glue.
[0055] (5) The encapsulated conductive film and electrode prepared in step (4) are placed in a vacuum dryer, the temperature is set to 110° C., and after waiting for 15 min, a high-sensitivity flexible tensile sensor made of polymer material is obtained. See the actual picture. Figure 1 .
[0056] After testing, the polymer material high-sensitivity flexible tensile sensor prepared in this embodiment has a resistance change rate of 3800% when the tensile strain is 10%. When the compressive strain is 2%, the resistance change rate is 20% (see Figure 5 ), the resistance change after receiving 11J energy shock is 160% (see Figure 4 ), tensile strength is 10.97MPa, and sensitivity is 258.
[0057] Example 2
[0058] (1) A 40×80×0.5 mm cuboid was designed and modeled, and then imported into a 3D printer to 3D print the thermoplastic polyurethane elastomer conductive coil into a prefabricated conductive film. The printer nozzle temperature was set to 210°C, and the base plate temperature was set to 30°C. After printing, ultrasonic cleaning was performed for 20 minutes and the prefabricated conductive film was obtained by drying.
[0059] (2) Set the temperature of the upper and lower clamping plates of the hot press to 220°C and the time to 30 seconds. After the hot press is heated to the set temperature, place the prefabricated conductive film obtained in step (1) between the upper and lower racks and clamp the clamping plates. Then lock the overflow valve and increase the displayed pressure to 2.1 MPa. Wait for the hot pressing time to end and safely remove the conductive film.
[0060] (3) The designed pattern ( Figure 3 (b)) is imported into the laser cutting machine. The cross-shaped dimensions in the figure are as follows Figure 3 (b) A laser is used to cross-cut the conductive film with the cutting port as a closed port to form a serpentine structure. The power of the laser cutting machine is set to 18%, and the scanning speed is set to 50 mm / s. After the laser cutting is completed, a serpentine conductive film with a coupling distance of 1 mm and a parallel coupling distance of 28 mm is obtained. After obtaining the serpentine conductive film, a thin layer of conductive silver paste is applied to the two sections of the serpentine structure to enhance the conductive performance, and then the copper electrode is pasted.
[0061] (4) Take two sections of pure thermoplastic polyurethane elastomer, cut them into rectangles with a width of 22 mm and a length of 44 mm, stretch both sections evenly to 50 mm, sandwich the serpentine conductive film prepared in step (3) and the electrode in the middle, and encapsulate them with acrylic glue.
[0062] (5) The encapsulated conductive film and electrode prepared in step (4) are placed in a vacuum dryer, the temperature is set to 110° C., and after waiting for 15 minutes, they are taken out to obtain a highly sensitive flexible tensile sensor made of polymer materials.
[0063] After testing, the high-sensitivity flexible tensile sensor made of polymer material prepared in this embodiment has a resistance change rate of 9800% when the tensile strain is 10%, a tensile strength of 11.36 MPa, and a sensitivity of 480.
[0064] Example 3
[0065] (1) A 40×80×0.5 mm cuboid was designed and modeled, and then imported into a 3D printer to 3D print the thermoplastic polyurethane elastomer conductive coil into a prefabricated conductive film. The printer nozzle temperature was set to 210°C, and the base plate temperature was set to 30°C. After printing, ultrasonic cleaning was performed for 20 minutes and the prefabricated conductive film was obtained by drying.
[0066] (2) Set the temperature of the upper and lower clamping plates of the hot press to 220°C and the time to 30 seconds. After the hot press is heated to the set temperature, place the prefabricated conductive film obtained in step (1) between the upper and lower racks and clamp the clamping plates. Then lock the overflow valve and increase the displayed pressure to 2.1 MPa. Wait for the hot pressing time to end and safely remove the conductive film.
[0067] (3) The designed pattern ( Figure 3 (c)) is imported into the laser cutting machine to cut the designed pattern ( Figure 3 (c)) The conductive film is introduced into a laser cutting machine, and a laser is used to cross-cut the conductive film with the cutting port as a closed port to form a serpentine structure. The power of the laser cutting machine is set to 18%, and the scanning speed is set to 50 mm / s. After the laser cutting is completed, a serpentine conductive film with a coupling distance of 1 mm and a parallel coupling distance of 4 mm is obtained. After the serpentine conductive film is obtained, a thin layer of conductive silver paste is applied to the two sections of the serpentine structure to enhance the conductive performance, and then the copper electrode is pasted.
[0068] (4) Take two sections of pure thermoplastic polyurethane elastomer, cut them into rectangles with a width of 22 mm and a length of 44 mm, stretch both sections evenly to 50 mm, sandwich the serpentine conductive film prepared in step (3) and the electrode in the middle, and encapsulate them with acrylic glue.
[0069] (5) The encapsulated conductive film and electrode prepared in step (4) are placed in a vacuum dryer, the temperature is set to 110° C., and after waiting for 15 minutes, they are taken out to obtain a highly sensitive flexible tensile sensor made of polymer materials.
[0070] After testing, the polymer material high-sensitivity flexible tensile sensor prepared in this embodiment has a resistance change rate of 100% when the tensile strain is 10%, a tensile strength of 10.21 MPa, and a sensitivity of 74.
[0071] Example 4
[0072] (1) A 40×80×0.5 mm cuboid was designed and modeled, and then imported into a 3D printer to 3D print the thermoplastic polyurethane elastomer conductive coil into a prefabricated conductive film. The printer nozzle temperature was set to 210°C, and the base plate temperature was set to 30°C. After printing, ultrasonic cleaning was performed for 20 minutes and the prefabricated conductive film was obtained by drying.
[0073] (2) Set the temperature of the upper and lower clamping plates of the hot press to 220°C and the time to 30 seconds. After the hot press is heated to the set temperature, place the prefabricated conductive film obtained in step (1) between the upper and lower racks and clamp the clamping plates. Then lock the overflow valve and increase the displayed pressure to 2.1 MPa. Wait for the hot pressing time to end and safely remove the conductive film.
[0074] (3) Place the designed pattern on the Figure 3 (d)) is introduced into a laser cutting machine, and a laser is used to cross-cut the conductive film with the cutting port as a closed port to form a serpentine structure. The cross-shaped size in the figure is as follows Figure 3 (d) Set the power of the laser cutting machine to 18%, the scanning speed to 50 mm / s, and wait for the laser cutting to be completed to obtain a serpentine conductive film with a coupling distance of 2 mm and a parallel coupling distance of 13 mm. After obtaining the serpentine conductive film, a thin layer of conductive silver paste is applied to the two sections of the serpentine conductive film to enhance the conductive performance, and then the copper electrode is attached.
[0075] (4) Take two sections of pure thermoplastic polyurethane elastomer, cut them into rectangles with a width of 22 mm and a length of 44 mm, pre-stretch both sections to 50 mm, and then sandwich the serpentine conductive film prepared in step (3) and the electrode in the middle and encapsulate them with acrylic glue.
[0076] (5) The encapsulated conductive film and electrode prepared in step (4) are placed in a vacuum dryer, the temperature is set to 110° C., and after waiting for 15 minutes, they are taken out to obtain a highly sensitive flexible tensile sensor made of polymer materials.
[0077] After testing, the high-sensitivity flexible tensile sensor made of polymer material prepared in this embodiment has a resistance change rate of about 450% when the tensile strain is 10%, a tensile strength of 10.73 MPa, and a sensitivity of 85.
[0078] Example 5
[0079] (1) A 40×80×0.5 mm cuboid was designed and modeled, and then imported into a 3D printer to 3D print the thermoplastic polyurethane elastomer conductive coil into a prefabricated conductive film. The printer nozzle temperature was set to 210°C, and the base plate temperature was set to 30°C. After printing, ultrasonic cleaning was performed for 20 minutes and the prefabricated conductive film was obtained by drying.
[0080] (2) Set the temperature of the upper and lower clamping plates of the hot press to 220°C and the time to 30 seconds. After the hot press is heated to the set temperature, place the prefabricated conductive film obtained in step (1) between the upper and lower racks and clamp the clamping plates. Then lock the overflow valve and increase the displayed pressure to 2.1 MPa. Wait for the hot pressing time to end and safely remove the conductive film.
[0081] (3) Place the designed pattern on the Figure 3 (e)) is introduced into a laser cutting machine, and a laser is used to cross-cut the conductive film with the cutting port as a closed port to form a serpentine structure. The cross-shaped size in the figure is as follows Figure 3 (e) The power of the laser cutting machine is set to 18%, the scanning speed is set to 50 mm / s, and the laser cutting is completed to obtain a serpentine conductive film with a coupling distance of 0.5 mm and a parallel coupling distance of 13 mm. After obtaining the serpentine conductive film, a conductive silver paste is thinly coated on two sections to enhance the conductive performance, and then the copper electrode is attached.
[0082] (4) Take two sections of pure thermoplastic polyurethane elastomer, cut them into rectangles with a width of 22 mm and a length of 44 mm, pre-stretch both sections to 50 mm, and then sandwich the serpentine conductive film prepared in step (3) and the electrode in the middle and encapsulate them with acrylic glue.
[0083] (5) The encapsulated conductive film and electrode prepared in step (4) are placed in a vacuum dryer, the temperature is set to 110° C., and after waiting for 15 minutes, they are taken out to obtain a highly sensitive flexible tensile sensor made of polymer materials.
[0084] According to tests, the high-sensitivity flexible tensile sensor made of polymer material prepared in this embodiment has a resistance change rate of about 1400% when the tensile strain is 10%, a tensile strength of 10.85 MPa, and a sensitivity of 132.
[0085] By comparing the above embodiments, it can be seen that the cost performance is the best when the embodiment sets the coupling distance to 1mm and the parallel coupling distance to 13mm. Although embodiment 2 is more sensitive, the required information function layer is wider and is not suitable for use in special environments. The performance of test embodiment 1 is as follows: the tensile strength is 10.97MPa, it can stably cycle 2000 times when the strain is 2%, the resistance change rate is 20% when the compressive strain is 2%, and the resistance change is stable at 20% to 160% when the energy is increased from 1 to 11J, and the resistance change reaches 160% when the energy is impacted by 11J. When twisted 0 to 90° for 5 cycles, the resistance change rate is stable at 40% to 60%, indicating stability; the sensitivity is 258, indicating high sensitivity.
[0086] Test Example 1
[0087] After testing at different temperatures, the resistance change rate of the flexible tension sensor only changed by 3%, indicating that it is not affected by temperature.
[0088] Test Example 2
[0089] After testing under different humidity conditions, the resistance change rate of the flexible tensile sensor only changed by 5%, indicating that it is not affected by temperature.
[0090] Comparative Example 1
[0091] The same as Example 1, except that in step (4), two sections of pure thermoplastic polyurethane elastomer are directly taken and cut into rectangles with a width of 50 mm and a length of 50 mm; the serpentine conductive film prepared in step (3) is sandwiched with the electrode in the middle and encapsulated with acrylic glue. There is no uniform stretching process, and the sensor sensitivity performance is poor. The reason is that when the outer layer does not compress the serpentine structure, the current path of the sensor is not significantly changed after being subjected to external stress, and the resistance change is not obvious.
[0092] Comparative Example 2
[0093] The same as Example 1, except that there is no step (3), and the conductive film and the electrode prepared in step (2) are directly encapsulated in the middle using acrylic adhesive. Then the conductive film is not serpentine, and since the current path is not changed, the resistance change is not obvious.
[0094] Comparative Example 3
[0095] The same as Example 1, except that there is no step (2), and thus no heat pressing process, so the outer layer cannot completely seal the information sensitive layer, and the performance changes more under different temperatures and humidity.
[0096] Comparative Example 4
[0097] If the conductive film arranged in a serpentine pattern is directly used without packaging, the sensor will be easily broken and have poor mechanical properties.
[0098] Comparative Example 5
[0099] Directly using a serpentine-arranged conductive film and PVC packaging will fail to effectively compress the serpentine-arranged conductive film, resulting in reduced sensitivity and reduced flexibility of the sensor.
Claims
1. A highly sensitive flexible tensile sensor made of polymer material, characterized in that: The polymer material highly sensitive flexible tension sensor is a composite sandwich structure, including a serpentine-arranged conductive film and a polymer material outer layer arranged on both sides of the conductive film, and electrodes are connected to both ends of the serpentine-arranged conductive film.
2. The polymer material highly sensitive flexible tension sensor according to claim 1 is characterized in that: The serpentine-arranged conductive film is a thermoplastic polyester elastomer pre-prepared by 3D printing and processed by a hot press and a laser cutting machine.
3. The polymer material highly sensitive flexible tension sensor according to claim 1, characterized in that: The outer layer of polymer material is a polymer elastic material that has been uniformly stretched.
4. The polymer material highly sensitive flexible tension sensor according to claim 3 is characterized in that: The polymer elastic material is selected from one or more of thermoplastic polyester elastomer, polyurethane thermoplastic elastomer and thermoplastic vulcanized rubber; and / or the uniform stretching length is 10% to 30% of the original length.
5. The polymer material highly sensitive flexible tension sensor according to any one of claims 1 to 4, characterized in that: The polymer material high-sensitivity flexible tensile sensor has a tensile strength of 10.21-11.36 MPa and a sensitivity of 74-480. When the strain is 10%, the resistance change rate is 100-9800%. When the strain is 2%, it can be cycled 2000 times. When subjected to cyclic loads, the resistance change can remain stable. When subjected to 1-11J energy impact, the resistance change remains at 20%-160%.
6. Application of the polymer material high-sensitivity flexible tensile sensor according to any one of claims 1 to 4 as a sensor for aircraft structure monitoring equipment or a sensor for human body monitoring equipment.
7. The method for preparing a polymer material highly sensitive flexible tension sensor according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: 3D printing the elastomer conductive coil into a prefabricated conductive film; S2: hot pressing and vulcanizing the prefabricated conductive film into a conductive film; S3: Laser cutting the conductive film into a serpentine structure and connecting electrodes at two ends; S4: After the pure polymer elastomer material is uniformly stretched to obtain the outer layer of the polymer material, the conductive film is encapsulated with adhesive, and the film is allowed to rebound naturally after encapsulation; S5: The packaged conductive film is vacuum dried to obtain a highly sensitive flexible tensile sensor made of polymer material.
8. The method for preparing a highly sensitive flexible tensile sensor made of polymer material according to claim 7, characterized in that: In S1, the printing technology used in 3D printing is fused deposition, the temperature of the printer nozzle is 150-400° C., and the temperature of the base plate is 10-50° C.; and / or the thickness of the prefabricated conductive film obtained by printing is 0.5-1 mm.
9. The method for preparing a highly sensitive flexible tensile sensor made of polymer material according to claim 8, characterized in that: In S2, the temperature of the hot press is 150-300°C, the time is 20-50s, and the hot press pressure is 2-3Mpa; and / or the thickness of the conductive film prepared by vulcanization is 0.25-0.5mm.
10. The method for preparing a highly sensitive flexible tensile sensor made of polymer material according to claim 8, characterized in that: In S3, the serpentine structure is formed by the following technical scheme: a laser is used to form the structure by cross-cutting with the cutting port as a closed port; the coupling distance of the serpentine structure is 0.5 to 2 mm, and the parallel coupling distance is 4 to 30 mm; and / or, the laser cutting speed is 40 to 60 mm / s, and the power is 15% to 25%; and / or, the electrode material is selected from one or more of platinum, copper, gold, and silver.
Citation Information
Cited By
Pressure sensor with rigidity and flexibility and preparation method
CN119984584A