Preparation method for preparing micro-nano structure pattern on surface of 3D cambered surface base material
By using nanoimprinting and plasma etching technologies on 3D curved surface substrates, the problem of preparing 3D curved surface micro-nano structures in the existing technology is solved, achieving better optical properties and tactile effects, and achieving Capable of mass production and cost control.
Patent Information
- Application Number
- CN202410896807.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
AI Technical Summary
The optical screens or back covers of existing consumer electronics products are usually based on flat substrates with limited structural adjustability. It is difficult to achieve efficient micro-nano structure pattern preparation on 3D curved surfaces, which limits the improvement of optical properties and tactility.
Nanoimprinting technology is used to spin-coat nanoimprinting glue on the surface of the 3D curved substrate, and use PDMS soft film for imprinting. Then the micro-nano structure pattern is transferred in ICP dry etching equipment, combined with plasma etching technology. Achieve better optical properties and tactile effects.
It achieves the efficient preparation of micro-nano structure patterns on 3D curved substrates, improves optical properties and tactile effects, and ensures mass production and cost control.
Smart Images

Figure CN118732386A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nanoimprinting, and in particular relates to a method for preparing micro-nano structure patterns on the surface of a 3D curved substrate. Background Art
[0002] In today's consumer electronics market, touch and optical components are widely used in a variety of consumer electronic equipment. As the most direct information transmission medium between users and electronic products, the pursuit of sensory and experience of optical components has become higher and higher over time, while the price has gradually decreased, which means that any visual and tactile device used in consumer electronics applications must have a high cost-effectiveness.
[0003] At present, the functions and decorative applications of optical screens or back covers of consumer electronic products such as mobile phones and tablets are basically achieved by covering the substrate itself with certain media or using wet etching to achieve certain optical properties. The structural adjustability is limited and most of them are flat substrates, which have certain structural and target limitations. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a method for preparing micro-nano structure patterns on the surface of a 3D curved substrate.
[0005] In order to achieve the above object, the technical solution of the present invention is as follows:
[0006] The present invention discloses a method for preparing a micro-nano structure pattern on the surface of a 3D curved surface substrate, comprising:
[0007] Step S1: placing a 3D curved surface substrate on a spin coating platform with a curved surface boss, and spin coating a layer of nanoimprint glue on the surface of the 3D curved surface substrate;
[0008] Step S2: placing the 3D curved surface substrate on an imprinting platform with a curved surface boss, and using a PDMS soft film with an inverse structure to imprint the nanoimprinting rubber surface of the 3D curved surface substrate to form a mask of a micro-nano structure pattern;
[0009] Step S3: placing the 3D curved surface substrate with the micro-nano structure pattern mask on an etching tray with a curved surface boss, and then placing the etching tray into an ICP dry etching device for etching;
[0010] Step S4: cleaning the etched 3D curved surface substrate;
[0011] Wherein: the outer contour of the shape of the curved surface boss matches the 3D curved surface substrate.
[0012] Based on the above technical solution, the following improvements can be made:
[0013] As a preferred solution, step S1 specifically includes:
[0014] Step S1.1: placing a 3D curved surface substrate on a spin coating platform having a curved surface boss;
[0015] Step S1.2: Rotate the spin coating platform clockwise to spin coat the nanoimprint glue on the surface of the 3D curved substrate;
[0016] Step S1.3: Rotate the spin coating platform counterclockwise to spin coat the nanoimprint glue on the surface of the 3D curved substrate;
[0017] Step S1.4: Repeat steps S1.2 to S1.3 until the nanoimprint glue on the surface of the 3D curved substrate reaches a set value.
[0018] As a preferred solution, the hardness of the PDMS soft film is 35 to 50 Mohs hardness, the thickness of the PDMS soft film is 3 to 6 mm, and the weight of the PDMS soft film is 90 to 110 g.
[0019] As a preferred solution, a limiting edge is further provided on the imprinting platform. The limiting edge is distributed on the outer side of the curved boss of the imprinting platform and its height is higher than that of the curved boss. The limiting edge is used to support the edge of the PDMS soft film.
[0020] As a preferred solution, at least two arc-surface bosses are distributed on the etching tray.
[0021] As a preferred solution, a plurality of positioning posts are distributed on the periphery of the arc-surface boss of each etching tray.
[0022] As a preferred solution, when the material of the 3D curved surface substrate is GG5 glass, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50sccm to 150sccm, the CHF3 gas flow rate is 25sccm to 100sccm, the O2 gas flow rate is 0sccm to 20sccm, the CHF3 / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / CHF3 gas input flow rate ratio is in the range of 0 to 15%;
[0023] The upper electrode power in the ICP dry etching equipment is 400W~1600W, the lower electrode power is 100W~1000W, the internal pressure control range is 2mT~6mT, the cooling temperature control range is -10℃~40℃, and the He gas pressure control range is 4T~8T.
[0024] As a preferred solution, when the material of the 3D curved surface substrate is sapphire, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50sccm to 120sccm, the CHF3 gas flow rate is 25sccm to 80sccm, the O2 gas flow rate is 0sccm to 20sccm, the CHF3 / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / CHF3 gas input flow rate ratio is in the range of 0 to 15%;
[0025] The upper electrode power in the ICP dry etching equipment is 1000W~1500W, the lower electrode power is 200W~800W, the internal pressure control range is 3.8mT~7.2mT, the cooling temperature control range is 20℃~40℃, and the He gas pressure control range is 3T~8T.
[0026] As a preferred solution, when the material of the 3D curved surface substrate is quartz, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50sccm to 120sccm, the CHF3 gas flow rate is 25sccm to 80sccm, the CF4 gas flow rate is 25sccm to 80sccm, the O2 gas flow rate is 0sccm to 20sccm, the (CHF3+CF4) / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / (CHF3+CF4) gas input flow rate ratio is in the range of 0 to 15%;
[0027] The upper electrode power in the ICP dry etching equipment is 800W~1200W, the lower electrode power is 200W~800W, the internal pressure control range is 3.8mT~6.0mT, the cooling temperature control range is 20℃~40℃, and the He gas pressure control range is 3T~8T.
[0028] As a preferred solution, when the material of the 3D curved surface substrate is metal aluminum, the Cl2 gas flow rate range of the ICP dry etching equipment is 25sccm to 80sccm, the BCl3 gas flow rate range is 50sccm to 120sccm, and the Cl2 / BCl3 gas input flow rate ratio range is 50% to 120%;
[0029] The upper electrode power in the ICP dry etching equipment is 1000W~1500W, the lower electrode power is 200W~800W, the internal pressure control range is 2.3mT~5.0mT, the cooling temperature control range is 25℃~45℃, and the He gas pressure control range is 3T~8T.
[0030] The present invention discloses a method for preparing micro-nano structure patterns on the surface of a 3D curved surface substrate. The method utilizes nanoimprinting to replicate the target micro-nano structure patterns onto the 3D curved surface substrate, and then utilizes plasma etching to transfer the nanoimprint mask pattern structure to the surface of the 3D curved surface substrate, so that the substrate can achieve better optical properties and tactile and visual effects, while achieving full-process mass production and cost-controllable goals. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 The present invention provides a flowchart of the preparation method of the present invention.
[0033] Figure 2 A schematic structural diagram of a spin coating platform provided in an embodiment of the present invention.
[0034] Figure 3 A top view of a spin coating platform provided in an embodiment of the present invention.
[0035] Figure 4 for Figure 3 Section view along AA direction.
[0036] Figure 5 A top view of an imprinting platform provided in an embodiment of the present invention.
[0037] Figure 6 A top view of an etching tray provided in an embodiment of the present invention.
[0038] Wherein: 1-spin coating platform, 11-cambered boss;
[0039] 2-imprinting platform, 21-cambered boss, 22-limiting edge;
[0040] 3-etching tray, 31-cambered boss, 32-positioning column. DETAILED DESCRIPTION
[0041] The preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] In addition, the expression of “comprising” an element is an “open” expression, which merely means that corresponding components or steps exist, and should not be interpreted as excluding additional components or steps.
[0044] In order to achieve the purpose of the present invention, in some embodiments of the method for preparing a micro-nano structure pattern on a 3D curved surface substrate, as Figure 1 As shown, the preparation method comprises:
[0045] Step S1: placing a 3D curved surface substrate (e.g., a substrate with downward curved surfaces on all four edges, with two long sides having larger curved surfaces and two short sides having smaller curved surfaces) on a spin coating platform 1 having a curved surface boss 11, and spin coating a layer of nanoimprint glue on the surface of the 3D curved surface substrate;
[0046] Step S2: placing the 3D curved surface substrate on the imprinting platform 2 having the curved surface boss 21, and using the PDMS soft film with the reverse structure to imprint the nanoimprinting rubber surface of the 3D curved surface substrate to form a mask of the micro-nano structure pattern;
[0047] Step S3: placing the 3D curved surface substrate with the micro-nano structure pattern mask on the etching tray 3 with the curved surface boss 31, and then placing the etching tray into the ICP dry etching equipment for etching;
[0048] Step S4: cleaning the etched 3D curved surface substrate;
[0049] Among them: the outer contour of the shape of the curved boss matches the 3D curved substrate. It is worth noting that since the curvature of the two short sides of the substrate is relatively low, it can be compatible with the plane. In the design of the curved boss, only the corresponding curved surfaces are designed on the two long sides of the curved boss.
[0050] The materials of 3D curved surface substrates include but are not limited to glass, sapphire, quartz, aluminum, etc. The line width characteristics of the graphic structure include 0.05-5um, and the depth characteristics include 0.08-5um array or non-array hole / column micro-nano structure graphics.
[0051] Before executing step S1, the 3D curved surface substrate needs to be cleaned.
[0052] In order to further optimize the implementation effect of the present invention, in some other implementations, the remaining characteristic technologies are the same, except that step S1 specifically includes:
[0053] Step S1.1: Place the 3D curved surface substrate on the spin coating platform 1 having the curved surface boss 11, as shown in FIG. Figure 2-4 As shown;
[0054] Step S1.2: rotating the spin coating platform 1 clockwise to spin coat the nanoimprint glue on the surface of the 3D curved substrate;
[0055] Step S1.3: rotating the spin coating platform 1 counterclockwise to spin coat the nanoimprint glue on the surface of the 3D curved substrate;
[0056] Step S1.4: Repeat steps S1.2 to S1.3 until the nanoimprint glue on the surface of the 3D curved substrate reaches a set value.
[0057] Step S1: Cover the surface of the 3D curved surface substrate with a layer of nano-imprint glue. In order to ensure the uniformity of the glue on the surface of the 3D curved surface substrate, a special spin coating platform is designed. A curved surface boss is provided on the spin coating platform, and the curved surface boss is used to support the 3D curved surface substrate. And the clockwise and counterclockwise alternating spin coating method is adopted to ensure that all curved surfaces of the 3D curved surface substrate can be covered with a layer of nano-imprint glue.
[0058] In order to further optimize the implementation effect of the present invention, in some other implementations, the remaining characteristic technologies are the same, except that step S2 is used to achieve nanoimprinting.
[0059] First, before nanoimprinting, a PDMS soft film needs to be prepared.
[0060] A type A / B silica gel is used to mix and stir in a 1:1 ratio for 40 to 90 minutes, and then allowed to stand for 2 to 3 hours in an environment of temperature and humidity of 23±2°C (temperature) / 50%±5% (humidity). Then, the PDMS soft film is used to replicate the graphics of the source design template structure, thereby forming a reverse structure of the source design graphics on the PDMS soft film.
[0061] Then, through the nanoimprint process, the reverse structure on the PDMS soft film is used to transfer the pattern to the surface of the 3D curved substrate to form the original designed pattern structure.
[0062] Because the substrate has a 3D curved surface with curved surfaces on all four sides, it is difficult to cover the curved surface with curved patterns using conventional flat substrate embossing processes. This application reduces the hardness of the PDMS soft film to 35-50 Mohs hardness, the thickness of the PDMS soft film to 3-6 mm, and the weight of the PDMS soft film to 90-110 g (the diameter of the PDMS soft film is 250 mm).
[0063] like Figure 5 As shown, a curved surface boss 21 is provided on the imprinting platform 2, and the curved surface boss 21 is used to support the 3D curved surface substrate.
[0064] Furthermore, two limiting edges 22 are provided on the imprinting platform 2 , and the two limiting edges 22 are respectively distributed outside two opposite short sides of the arc-surface boss 21 of the imprinting platform.
[0065] During embossing, the PDMS soft film cavity is pressurized 0-5Kap for the first time and 15-45Kap for the second time. The imprinting platform rises at a low speed of 0.2-2mm / s, and the demolding speed is 0.1-1.5mm / s. The boost position is 49mm, and the target position is 50mm. The imprinting equipment process can be used to transfer graphics covering the entire surface of the 3D curved surface substrate.
[0066] Furthermore, the height of the limiting edge 22 is higher than the height of the arc-surface boss 21. The limiting edge 22 can support the edge of the PDMS soft film to prevent the edge of the soft film from being sunken too much when the PDMS soft film is pressurized for the second time and the platform rises to the highest position, causing the soft film in the middle area to be pulled and deformed, thereby ensuring that the pattern can be accurately transferred and imprinted.
[0067] In order to further optimize the implementation effect of the present invention, in some other embodiments, the remaining characteristic technologies are the same, except that, Figure 6 As shown, there are six arc-surface bosses 31 distributed on the etching tray 3. Of course, in other embodiments, the number of the arc-surface bosses 31 on the etching tray 3 can be other numbers, such as: 2, 3, 4, 5, etc.
[0068] Four positioning posts 32 are distributed on the periphery of the arc-surface boss 31 of each etching tray.
[0069] The material of the etching tray 3 and the positioning pillar 32 can be, but is not limited to, silicon carbide with good thermal conductivity. The etching tray 3 is used to perform load-bearing etching on the 3D curved surface substrate to prevent damage to the edge of the 3D curved surface substrate and its graphic structure.
[0070] In some embodiments, when the material of the 3D curved surface substrate is GG5 glass, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50 sccm to 150 sccm, the CHF3 gas flow rate is 25 sccm to 100 sccm, the O2 gas flow rate is 0 sccm to 20 sccm, the CHF3 / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / CHF3 gas input flow rate ratio is in the range of 0 to 15%;
[0071] The upper electrode power in the ICP dry etching equipment is 400W~1600W, the lower electrode power is 100W~1000W, the internal pressure control range is 2mT~6mT, the cooling temperature control range is -10℃~40℃, and the He gas pressure control range is 4T~8T.
[0072] In some embodiments, when the material of the 3D curved surface substrate is sapphire, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50 sccm to 120 sccm, the CHF3 gas flow rate is 25 sccm to 80 sccm, the O2 gas flow rate is 0 sccm to 20 sccm, the CHF3 / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / CHF3 gas input flow rate ratio is in the range of 0 to 15%;
[0073] The upper electrode power in the ICP dry etching equipment is 1000W~1500W, the lower electrode power is 200W~800W, the internal pressure control range is 3.8mT~7.2mT, the cooling temperature control range is 20℃~40℃, and the He gas pressure control range is 3T~8T.
[0074] In some embodiments, when the material of the 3D curved surface substrate is quartz, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50 sccm to 120 sccm, the CHF3 gas flow rate is 25 sccm to 80 sccm, the CF4 gas flow rate is 25 sccm to 80 sccm, the O2 gas flow rate is 0 sccm to 20 sccm, the (CHF3+CF4) / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / (CHF3+CF4) gas input flow rate ratio is in the range of 0 to 15%;
[0075] The upper electrode power in the ICP dry etching equipment is 800W~1200W, the lower electrode power is 200W~800W, the internal pressure control range is 3.8mT~6.0mT, the cooling temperature control range is 20℃~40℃, and the He gas pressure control range is 3T~8T.
[0076] In some embodiments, when the material of the 3D curved surface substrate is metal aluminum, the Cl2 gas flow rate range of the ICP dry etching equipment is 25 sccm to 80 sccm, the BCl3 gas flow rate range is 50 sccm to 120 sccm, and the Cl2 / BCl3 gas input flow rate ratio range is 50% to 120%;
[0077] The upper electrode power in the ICP dry etching equipment is 1000W~1500W, the lower electrode power is 200W~800W, the internal pressure control range is 2.3mT~5.0mT, the cooling temperature control range is 25℃~45℃, and the He gas pressure control range is 3T~8T.
[0078] The present invention discloses a method for preparing micro-nano structure patterns on the surface of a 3D curved surface substrate. The method utilizes nanoimprinting to replicate the target micro-nano structure patterns onto the 3D curved surface substrate, and then utilizes plasma etching to transfer the nanoimprint mask pattern structure to the surface of the 3D curved surface substrate, so that the substrate can achieve better optical properties and tactile and visual effects, while achieving full-process mass production and cost-controllable goals.
[0079] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a micro-nano structure pattern on a 3D curved surface substrate, characterized in that: include: Step S1: placing a 3D curved surface substrate on a spin coating platform with a curved surface boss, and spin coating a layer of nanoimprint glue on the surface of the 3D curved surface substrate; Step S2: placing the 3D curved surface substrate on an imprinting platform with a curved surface boss, and using a PDMS soft film with an inverse structure to imprint the nanoimprinting rubber surface of the 3D curved surface substrate to form a mask of a micro-nano structure pattern; Step S3: placing the 3D curved surface substrate with the micro-nano structure pattern mask on an etching tray with a curved surface boss, and then placing the etching tray into an ICP dry etching device for etching; Step S4: cleaning the etched 3D curved surface substrate; Wherein: the outer contour of the shape of the arc-surface boss matches the 3D arc-surface substrate.
2. The preparation method according to claim 1, characterized in that: The step S1 specifically includes: Step S1.1: placing a 3D curved surface substrate on a spin coating platform having a curved surface boss; Step S1.2: Rotate the spin coating platform clockwise to spin coat the nanoimprint glue on the surface of the 3D curved substrate; Step S1.3: Rotate the spin coating platform counterclockwise to spin coat the nanoimprint glue on the surface of the 3D curved substrate; Step S1.4: Repeat steps S1.2 to S1.3 until the nanoimprint glue on the surface of the 3D curved substrate reaches a set value.
3. The preparation method according to claim 1, characterized in that: The hardness of the PDMS soft film is 35-50 Mohs hardness, the thickness of the PDMS soft film is 3-6 mm, and the weight of the PDMS soft film is 90-110 g.
4. The preparation method according to claim 1, characterized in that: A limiting edge is also provided on the imprinting platform. The limiting edge is distributed on the outer side of the arc-surface boss of the imprinting platform and has a height higher than that of the arc-surface boss. The limiting edge is used to support the edge of the PDMS soft film.
5. The preparation method according to claim 1, characterized in that: At least two curved bosses are distributed on the etching tray.
6. The preparation method according to claim 5, characterized in that: A plurality of positioning posts are distributed on the periphery of the arc-surface boss of each etching tray.
7. The preparation method according to any one of claims 1 to 6, characterized in that: When the material of the 3D curved surface substrate is GG5 glass, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50 sccm to 150 sccm, the CHF3 gas flow rate is 25 sccm to 100 sccm, the O2 gas flow rate is 0 sccm to 20 sccm, the CHF3 / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / CHF3 gas input flow rate ratio is in the range of 0 to 15%; The upper electrode power in the ICP dry etching equipment is 400W-1600W, the lower electrode power is 100W-1000W, the internal pressure control range is 2mT-6mT, the cooling temperature control range is -10°C-40°C, and the He gas pressure control range is 4T-8T.
8. The preparation method according to any one of claims 1 to 6, characterized in that: When the material of the 3D curved surface substrate is sapphire, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50 sccm to 120 sccm, the CHF3 gas flow rate is 25 sccm to 80 sccm, the O2 gas flow rate is 0 sccm to 20 sccm, the CHF3 / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / CHF3 gas input flow rate ratio is in the range of 0 to 15%; The upper electrode power in the ICP dry etching equipment is 1000W-1500W, the lower electrode power is 200W-800W, the internal pressure control range is 3.8mT-7.2mT, the cooling temperature control range is 20°C-40°C, and the He gas pressure control range is 3T-8T.
9. The preparation method according to any one of claims 1 to 6, characterized in that: When the material of the 3D curved surface substrate is quartz, the BCl3 gas flow rate input into the ICP dry etching equipment is in the range of 50sccm to 120sccm, the CHF3 gas flow rate is 25sccm to 80sccm, the CF4 gas flow rate is 25sccm to 80sccm, the O2 gas flow rate is 0sccm to 20sccm, the (CHF3+CF4) / BCl3 gas input flow rate ratio is in the range of 30% to 75%, and the O2 / (CHF3+CF4) gas input flow rate ratio is in the range of 0 to 15%; The upper electrode power in the ICP dry etching equipment is 800W-1200W, the lower electrode power is 200W-800W, the internal pressure control range is 3.8mT-6.0mT, the cooling temperature control range is 20°C-40°C, and the He gas pressure control range is 3T-8T.
10. The preparation method according to any one of claims 1 to 6, characterized in that: When the material of the 3D curved surface substrate is metal aluminum, the Cl2 gas flow rate range of the ICP dry etching equipment is 25 sccm to 80 sccm, the BCl3 gas flow rate range is 50 sccm to 120 sccm, and the Cl2 / BCl3 gas input flow rate ratio range is 50% to 120%; The upper electrode power in the ICP dry etching equipment is 1000W-1500W, the lower electrode power is 200W-800W, the internal pressure control range is 2.3mT-5.0mT, the cooling temperature control range is 25°C-45°C, and the He gas pressure control range is 3T-8T.
Citation Information
Cited By
Preparation method for preparing micro-nano structure pattern on surface of 3D cambered-surface substrate
WO2026007452A1