Thin film transistor, preparation method thereof and display substrate

By performing ultrasonic annealing treatment on the semiconductor material of the thin film transistor, the problem of interlayer peeling of the thin film transistor during bending is solved, the stability of mobility and threshold voltage is improved, and the stability and yield of the product are improved.

CN118738098APending Publication Date: 2024-10-01BEIJING INST OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310324517.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing thin film transistors are prone to interlayer delamination when the film layer is bent, have low mobility, and easily drift in threshold voltage, resulting in reduced product stability and yield.

Method used

Semiconductor materials are patterned to form active layers, and ultrasonic annealing is performed during the process. Ultrasonic annealing can promote atomic bonding, uniform distribution and improvement of mechanical properties, reduce interlayer peeling, and improve mobility and threshold voltage stability.

Benefits of technology

Through ultrasonic annealing treatment, the surface flatness and density of the thin film transistor are improved, the mechanical and electrical properties are enhanced, the yield and bending resistance of the device are improved, and the threshold voltage is stabilized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738098A_ABST
    Figure CN118738098A_ABST
Patent Text Reader

Abstract

The invention provides a thin film transistor, a preparation method thereof and a display substrate, and belongs to the technical field of display. The preparation method of the thin film transistor comprises the following steps: patterning a semiconductor material to form an active layer; the preparation method further comprises a step of performing ultrasonic annealing on the semiconductor material on which the active layer is to be formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure belongs to the field of display technology, and specifically relates to a thin film transistor and a preparation method thereof, and a display substrate. Background Art

[0002] In the development of the information age, various human-computer interactions are inseparable from display screens, and in order to meet the demand for screens in various scenarios, display technology has received more and more attention. As the core and key technology of display technology, the preparation process of thin-film transistors (TFT) needs to be further improved. Due to the presence of multiple layers of thin films on the display substrate, the film layer is easily subjected to greater stress when it is bent, resulting in interlayer peeling of the film. In addition, the mobility of the thin-film transistor also determines the display performance of the product. For example, the mobility of the currently mass-produced amorphous thin-film transistors is generally low. For example, the mobility of the thin-film transistor IGZO-TFT whose active layer material is indium gallium zinc oxide is about 10cm 2 V -1 s -1 It is about 100%, and it is easy to cause threshold voltage drift, which reduces the stability of TFT characteristics and thus reduces product yield. Summary of the invention

[0003] The present disclosure aims to solve at least one of the technical problems existing in the prior art, and provides a thin film transistor and a method for preparing the same, and a display substrate.

[0004] In a first aspect, the technical solution adopted to solve the technical problem of the present disclosure is a method for preparing a thin film transistor, comprising: a step of patterning a semiconductor material layer to form an active layer; wherein the preparation method also comprises: a step of ultrasonic annealing the semiconductor material to form the active layer.

[0005] In some embodiments, the step of ultrasonically annealing the semiconductor material to form the active layer comprises:

[0006] Forming the semiconductor material layer, at least performing ultrasonic annealing on the semiconductor material at a position of the semiconductor material layer corresponding to the position where the active layer is to be formed;

[0007] The step of patterning the semiconductor material layer to form an active layer comprises:

[0008] The semiconductor material layer after ultrasonic annealing is patterned to form an active layer of the thin film transistor.

[0009] In some embodiments, the forming of the semiconductor material layer, at least ultrasonically annealing the semiconductor material at a position of the semiconductor material layer corresponding to the position where the active layer is to be formed, comprises:

[0010] The semiconductor material layer is formed, and ultrasonic annealing is performed on the entire semiconductor material layer; the acoustic field of the ultrasonic annealing is located in the center and edge areas of the entire semiconductor material layer.

[0011] In some embodiments, the ultrasonic frequency of the ultrasonic annealing is between 40 kHz and 200 kHz.

[0012] In some embodiments, the ultrasonic annealing lasts for 5 min to 240 min.

[0013] In some embodiments, the ultrasonic annealing environment includes an environment filled with any one of nitrogen, oxygen and argon.

[0014] In some embodiments, the heating method of the ultrasonic annealing includes any one of laser, microwave, light wave, solid-state heat conduction, and gaseous heat conduction.

[0015] In some embodiments, the material of the active layer is an amorphous material.

[0016] In some embodiments, the semiconductor material is an amorphous oxide material;

[0017] The bonding ratio of metal atoms to oxygen atoms in the amorphous oxide material after the ultrasonic annealing is greater than the bonding ratio of metal atoms to oxygen atoms in the amorphous oxide material not after the ultrasonic annealing;

[0018] The bonding ratio of oxygen atoms to hydrogen atoms in the amorphous oxide material after the ultrasonic annealing is less than the bonding ratio of oxygen atoms to hydrogen atoms in the amorphous oxide material not after the ultrasonic annealing;

[0019] The vacancy ratio of oxygen atoms in the amorphous oxide material after the ultrasonic annealing is less than the vacancy ratio of oxygen atoms in the amorphous oxide material not after the ultrasonic annealing;

[0020] The sum of the bonding ratio of metal atoms to oxygen atoms, the bonding ratio of oxygen atoms to hydrogen atoms, and the vacancy ratio of oxygen atoms in the amorphous oxide material that has undergone the ultrasonic annealing is 1; the sum of the bonding ratio of metal atoms to oxygen atoms, the bonding ratio of oxygen atoms to hydrogen atoms, and the vacancy ratio of oxygen atoms in the amorphous oxide material that has not undergone the ultrasonic annealing is 1.

[0021] In some embodiments, the sum of the elastic modulus distribution ratios of the semiconductor material that has undergone the ultrasonic annealing within the elastic modulus range a is greater than the sum of the elastic modulus distribution ratios of the semiconductor material that has not undergone the ultrasonic annealing within the elastic modulus range b; a∈[c-5Gpa, c+5Gpa], where c is the elastic modulus corresponding to the maximum elastic modulus distribution ratio of the semiconductor material that has undergone the ultrasonic annealing; b∈[d-5Gpa, d+5Gpa], where d is the elastic modulus corresponding to the maximum elastic modulus distribution ratio of the semiconductor material that has not undergone the ultrasonic annealing.

[0022] In some embodiments, when the bending degree of the semiconductor material before and after the ultrasonic annealing is the same, a first difference between the maximum value and the minimum value of the stress experienced by the semiconductor material after the ultrasonic annealing is smaller than a second difference between the maximum value and the minimum value of the stress experienced by the semiconductor material without the ultrasonic annealing.

[0023] In a second aspect, the embodiments of the present disclosure further provide a thin film transistor, comprising a source electrode, a drain electrode, an active layer and a gate electrode, wherein the active layer comprises a source contact region, a drain contact region and a channel region sandwiched between the source contact region and the drain contact region; the channel region overlaps with the orthographic projection of the gate electrode on the substrate where the thin film transistor is located, the source electrode is electrically connected to the active layer located in the source contact region, and the drain electrode is electrically connected to the active layer located in the drain contact region;

[0024] The material of the active layer is indium gallium zinc oxide; the bonding ratio of metal atoms to oxygen atoms in the indium gallium zinc oxide is greater than 53%; the metal atoms include indium, gallium and zinc; the bonding ratio of hydrogen atoms to oxygen atoms in the indium gallium zinc oxide is less than 23%; and the vacancy ratio of oxygen atoms in the indium gallium zinc oxide is less than 24%.

[0025] In some embodiments, the material of the active layer is indium gallium zinc oxide, and the composition ratio of indium, gallium and zinc is 1:1:1.

[0026] In some embodiments, the carrier mobility of the active layer is greater than or equal to 20 cm 2 V -- s -- .

[0027] In some embodiments, the switching ratio of the thin film transistor is greater than or equal to 10 8 .

[0028] In some embodiments, the subthreshold swing of the thin film transistor is between 0.05 mV / dec and 0.25 mV / dec.

[0029] In some embodiments, the threshold voltage of the thin film transistor is between 0V and 1V.

[0030] In a third aspect, the embodiments of the present disclosure also include a display substrate, which includes a base substrate and a pixel driving circuit arranged on the base substrate; at least one thin film transistor in the pixel driving circuit is a thin film transistor described in any one of the above embodiments.

[0031] In some embodiments, the substrate substrate is a flexible substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 An exemplary flow chart of forming an active layer provided in an embodiment of the present disclosure;

[0033] Figure 2a A schematic diagram of an X-ray photoelectron spectroscopy (XPS) test of indium gallium zinc oxide (IGZO) without ultrasonic annealing provided in an embodiment of the present disclosure;

[0034] Figure 2b A schematic diagram of an XPS test of indium gallium zinc oxide (IGZO) that has been ultrasonically annealed for 120 minutes according to an embodiment of the present disclosure;

[0035] Figure 2c A schematic diagram of an XPS test of indium gallium zinc oxide (IGZO) that has been ultrasonically annealed for 180 minutes provided in an embodiment of the present disclosure;

[0036] Figure 3 A schematic diagram showing the atomic bonding comparison of indium gallium zinc oxide (IGZO) without ultrasonic annealing and after ultrasonic annealing provided in an embodiment of the present disclosure;

[0037] Figure 4a Energy displacement curves of gallium-oxygen bonding of IGZO thin films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing provided in the embodiments of the present disclosure;

[0038] Figure 4b Energy displacement curves of indium-oxygen bonding of IGZO films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing provided in the embodiments of the present disclosure;

[0039] Figure 5a A schematic diagram of elastic modulus distribution of an exemplary indium oxide material that has not been ultrasonically annealed provided in an embodiment of the present disclosure;

[0040] Figure 5b A schematic diagram of elastic modulus distribution of an exemplary ultrasonically annealed indium oxide material provided in an embodiment of the present disclosure;

[0041] Figure 6a A schematic diagram of the morphology of an indium oxide material that has not been ultrasonically annealed under AFM provided in an exemplary embodiment of the present disclosure;

[0042] Figure 6b A schematic diagram of the morphology of an indium oxide material that has undergone ultrasonic annealing under AFM provided in an exemplary embodiment of the present disclosure;

[0043] Figure 7a A schematic diagram of elastic modulus distribution of an exemplary indium gallium zinc oxide (IGZO) material that has not been ultrasonically annealed provided in an embodiment of the present disclosure;

[0044] Figure 7b A schematic diagram of elastic modulus distribution of an indium gallium zinc oxide (IGZO) material subjected to 120 minutes of ultrasonic annealing provided in an embodiment of the present disclosure;

[0045] Figure 7c A schematic diagram of elastic modulus distribution of an indium gallium zinc oxide (IGZO) material subjected to 180 minutes of ultrasonic annealing provided in an embodiment of the present disclosure;

[0046] Figure 7d A schematic diagram of elastic modulus distribution of an indium gallium zinc oxide (IGZO) material subjected to 240 minutes of ultrasonic annealing provided in an embodiment of the present disclosure;

[0047] Figure 8a A schematic diagram of the morphology of an exemplary IGZO material that has not been ultrasonically annealed under AFM provided in an embodiment of the present disclosure;

[0048] Figure 8b A schematic diagram of the morphology of an exemplary IGZO material subjected to 120 minutes of ultrasonic annealing under AFM provided in an embodiment of the present disclosure;

[0049] Figure 8c A schematic diagram of the morphology of an exemplary IGZO material subjected to 180 minutes of ultrasonic annealing under AFM provided in an embodiment of the present disclosure;

[0050] Figure 8d A schematic diagram of the morphology of an exemplary IGZO material subjected to 240 minutes of ultrasonic annealing under AFM provided in an embodiment of the present disclosure;

[0051] Figure 9a A schematic diagram of a bending simulation of an exemplary indium gallium zinc oxide (IGZO) material that has not been ultrasonically treated provided in an embodiment of the present disclosure;

[0052] Figure 9bA schematic diagram of a bending simulation of an exemplary ultrasonically treated indium gallium zinc oxide (IGZO) material provided in an embodiment of the present disclosure;

[0053] Figures 10a to 10c The measured images of DIW contact angle of IGZO films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing respectively;

[0054] Figures 11a to 11c The measured images of (CH2OH)2 contact angle of IGZO films without ultrasonic annealing, after 120min ultrasonic annealing, and after 180min ultrasonic annealing respectively;

[0055] Fig.12 Schematic diagram of surface energy data of IGZO films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing;

[0056] Fig.13 Electrical characteristics diagram of a thin film transistor provided in an embodiment of the present disclosure. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical scheme and advantages of the embodiments of the present disclosure clearer, the technical scheme in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. The components of the embodiments of the present disclosure generally described and shown in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present disclosure provided in the drawings is not intended to limit the scope of the present disclosure for protection, but merely represents the selected embodiments of the present disclosure. Based on the embodiments of the present disclosure, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present disclosure.

[0058] Unless otherwise defined, the technical terms or scientific terms used in the present disclosure should be understood by people with ordinary skills in the field to which the present disclosure belongs. The "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, similar words such as "one", "one" or "the" do not indicate quantity restrictions, but indicate that there is at least one. Similar words such as "include" or "comprise" mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Similar words such as "connect" or "connected" are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0059] The "multiple or several" mentioned in this disclosure refers to two or more. "And / or" describes the association relationship of the associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0060] In the related art, the main reasons for interlayer peeling include: 1. Uneven distribution of atoms in the film layer; 2. Uneven relaxation of atoms in the film layer. For example, clusters or holes are generated by uneven distribution of atoms in the film layer, and uneven distribution of atoms in the surface causes local mechanical parameters (such as elastic modulus, etc.) to differ too much from the overall mechanical parameters, causing interlayer peeling. For another example, the microstructure and dynamic behavior (such as atomic relaxation) of the prefabricated film both show non-uniform characteristics. This non-uniformity shows different areas of high energy dissipation and low energy dissipation at the nanoscale in terms of energy dissipation (energy required for atomic relaxation, energy required for formation), and the mechanical properties of these areas are very different, causing interlayer peeling. In addition, the main reason for the low mobility of IGZO-TFT is determined by the material itself, such as the uneven microscopic distribution of elements in amorphous oxides. Therefore, metal atoms will preferentially bond with neighboring atoms during the preparation of the active layer (IGZO), which will lead to different element bonding ratios under the same element ratio. The different bonding ratios of different elements directly affect the mobility and threshold voltage of IGZO-TFT. When the indium-oxygen (In-O) bonding ratio is high, the mobility is improved, but the off-state current decreases, causing it to lose its switching ability. When the gallium-oxygen (Ga-O) bonding ratio is high, the mobility decreases and the threshold voltage drift will also occur. Each metal element will not only bond with oxygen, but also form metal-metal bonds, and form metal-hydrogen bonds with the environment and hydrogen diffused from other layers.

[0061] In view of this, the embodiments of the present disclosure provide a method for preparing a thin film transistor, which substantially eliminates one or more of the problems caused by the limitations and defects of the related art. Specifically, the step of patterning the semiconductor material to form an active layer; wherein the preparation method also includes: the step of ultrasonically annealing the semiconductor material to form the active layer.

[0062] The disclosed embodiment performs ultrasonic annealing on the semiconductor material to be formed into the active layer, which promotes the mutual diffusion between atoms in the semiconductor material, so that the material of the active layer finally formed has fewer clusters and holes than the semiconductor material before ultrasonic annealing, and the atomic distribution in the surface is more uniform, which improves the surface flatness and density, and avoids the stress from causing interlayer peeling. In addition, ultrasonic annealing can change the elemental bonding without changing the elemental composition of the active layer, promote the atomic relaxation before the atomic bonding in the semiconductor material before ultrasonic annealing, so that the mechanical properties and electrical properties of the active layer are closer to the theoretical values, and improve the yield rate of device preparation.

[0063] The following is a detailed introduction to a method for preparing a thin film transistor provided in an embodiment of the present disclosure. The method for preparing a thin film transistor includes: a step of patterning a semiconductor material to form an active layer; and a step of ultrasonically annealing the semiconductor material to form the active layer. Exemplarily, the unpatterned semiconductor material may be ultrasonically annealed, and then the semiconductor material after ultrasonic annealing may be patterned to form an active layer. Alternatively, the deposited semiconductor material may be patterned first, and then the patterned semiconductor material may be ultrasonically annealed to form an active layer.

[0064] Figure 1 An exemplary flow chart of forming an active layer is provided for an embodiment of the present disclosure, as shown in FIG. Figure 1 As shown, it includes steps S11 to S13, wherein:

[0065] S11. Forming a semiconductor material layer.

[0066] The material of the semiconductor material layer may be, for example, an amorphous oxide material.

[0067] S12. Perform ultrasonic annealing on at least the semiconductor material at the position of the semiconductor material layer corresponding to the position where the active layer is to be formed.

[0068] S13, patterning the semiconductor material layer after ultrasonic annealing to form an active layer of a thin film transistor.

[0069] Here, ultrasonic annealing followed by patterning is taken as an example. Specifically, a layer of semiconductor material can be deposited on a substrate. After that, the substrate on which the semiconductor material has just been deposited is fixed on an ultrasonic device, and an ultrasonic glass is loaded on the semiconductor material for ultrasonic annealing. After a preset period of time, the semiconductor material after ultrasonic annealing is obtained. After that, the semiconductor material after ultrasonic annealing is patterned based on a mask to form an active layer of a thin film transistor.

[0070] Here, ultrasonic vibration can produce cavitation effect and mechanical effect, which can effectively break up particle clusters and inhibit the formation of columnar particles, making the particles more uniform, and effectively improving the flatness and density of the active layer. Ultrasonic vibration of semiconductor materials can promote the mutual diffusion between atoms in semiconductor materials, making the distribution of atoms in the surface more uniform, reducing the generation of clusters and holes, and ultimately improving the surface flatness and density of the active layer, thereby avoiding stress-induced interlayer peeling.

[0071] Ultrasonic annealing can change the elemental bonding without changing the elemental composition of the active layer, promote atomic relaxation before atomic bonding in semiconductor materials, make the electrical properties of the active layer closer to the theoretical value, and improve the yield of device preparation.

[0072] In addition, ultrasonic annealing can reduce the difference in energy dissipation between high energy dissipation and low energy dissipation in semiconductor materials (which can be understood as promoting atomic relaxation before atomic bonding in semiconductor materials), so that the energy dissipation in the active layer after ultrasonic annealing is uniform, thereby promoting a uniform distribution of the single elastic modulus on the surface of the active layer, thereby improving the mobility of the thin film transistor and stabilizing the threshold voltage.

[0073] In addition, ultrasonic annealing can control the atomic bonding ratio in semiconductor materials, so that the atomic bonding ratio of semiconductor materials that have undergone ultrasonic annealing is more consistent with the theoretical value than the atomic bonding ratio of semiconductor materials that have not undergone ultrasonic annealing, thereby making the device mobility and threshold voltage closer to the theoretical value, thereby improving the yield of device preparation. At the same time, the use of ultrasonic annealing to control the atomic bonding ratio of semiconductor materials can also improve the interlayer shedding phenomenon of thin films caused by strain or certain stresses under conditions such as bending and torsion, thereby improving the yield of devices under strain and bending resistance.

[0074] In some embodiments, with respect to step S12, a semiconductor material layer is formed, and ultrasonic annealing is performed on the entire semiconductor material layer; the ultrasonic annealing sound field can be located in the center and edge areas of the entire semiconductor material layer, so that the ultrasonic wave is more evenly loaded throughout the semiconductor material layer.

[0075] Of course, for the convenience of installation, the acoustic field of ultrasonic annealing can also be located in the center and edge areas of the substrate.

[0076] In some embodiments, the ultrasonic frequency of ultrasonic annealing is between 40kHz and 200kHz. Preferably, the ultrasonic frequency can be set to 100kHz.

[0077] In some embodiments, the duration of ultrasonic annealing is between 5 min and 240 min. Preferably, the duration of ultrasonic annealing can be set to 180 min.

[0078] In some embodiments, the ultrasonic annealing environment is an environment filled with any one of nitrogen, oxygen and argon. Preferably, the ultrasonic annealing environment is an environment filled with an inert gas, such as an environment filled with nitrogen or argon, so that during ultrasonic annealing, the inert gas is used to protect the surface of the prefabricated layer to avoid oxidation. Further, the inert gas can be nitrogen or argon.

[0079] In some embodiments, the heating method of ultrasonic annealing includes any one of the following: laser, microwave, light wave, solid-state heat conduction, gaseous heat conduction. Among them, the heating method of solid-state heat conduction can be to use a heated resistance wire to heat a high heat conduction medium, thereby using the high heat conduction medium to anneal and heat the semiconductor material. The heating method of gaseous heat conduction can be to use a heated resistance wire to heat a gaseous medium, thereby using the gaseous medium to anneal and heat the semiconductor material.

[0080] The ultrasonic annealing is explained below with a complete example. Exemplarily, the ultrasonic device is built by itself. The substrate base on which the semiconductor material has just been deposited is placed and fixed on a steel box, and an ultrasonic piezoelectric transducer is installed in the steel box. The ultrasonic stage temperature is controlled by a water bath method when it is less than or equal to 80°C, and the ultrasonic stage temperature is controlled by a heating plate when it is greater than 80°C. At the same time, the sound field is set at the center and four corners of the substrate to ensure that the ultrasonic wave is loaded on the semiconductor material more evenly, and ultrasonic annealing is performed in an environment filled with inert gas. The ultrasonic frequency is set to 100kHz, and the annealing heating method includes but is not limited to laser, microwave, light wave, solid-state heat conduction, gaseous heat conduction, etc. After 180 minutes of ultrasonic annealing, the ultrasonic annealing of the semiconductor layer is completed.

[0081] In some embodiments, the material of the active layer is an amorphous material, such as an amorphous oxide material or an amorphous silicon material, etc. The amorphous oxide material may include but is not limited to any one of indium gallium zinc oxide (IGZO), indium gallium zinc tin oxide (IGZTO), indium zinc oxide (IZO), indium oxide (In2O3), etc.

[0082] In some embodiments, the semiconductor material is an amorphous oxide material.

[0083] The bonding ratio of metal atoms to oxygen atoms in the amorphous oxide material after ultrasonic annealing is greater than the bonding ratio of metal atoms to oxygen atoms in the amorphous oxide material that has not undergone ultrasonic annealing; the bonding ratio of oxygen atoms to hydrogen atoms in the amorphous oxide material after ultrasonic annealing is less than the bonding ratio of oxygen atoms to hydrogen atoms in the amorphous oxide material that has not undergone ultrasonic annealing; the vacancy ratio of oxygen atoms in the amorphous oxide material after ultrasonic annealing is less than the vacancy ratio of oxygen atoms in the amorphous oxide material that has not undergone ultrasonic annealing; the sum of the bonding ratio of metal atoms to oxygen atoms, the bonding ratio of oxygen atoms to hydrogen atoms, and the vacancy ratio of oxygen atoms in the amorphous oxide material after ultrasonic annealing is 1; the sum of the bonding ratio of metal atoms to oxygen atoms, the bonding ratio of oxygen atoms to hydrogen atoms, and the vacancy ratio of oxygen atoms in the amorphous oxide material that has not undergone ultrasonic annealing is 1.

[0084] Taking indium gallium zinc oxide (IGZO) as an example, the properties of the amorphous oxide material after ultrasonic annealing and the amorphous oxide material without ultrasonic annealing are analyzed below.

[0085] It should be noted that the elements and valence bands on the surface of the InGaZnO film were characterized using an X-ray photoelectron spectrometer (XPS, 5000Versaprobe III). In order to calibrate the electron binding energy (BE), the C1s peak of the carbon CC bond was assigned to 284.8 eV, and the oxygen O1s spectrum was fitted using vantage software to generate fitting data. The electrical properties of the InGaZnO film were tested using a semiconductor parameter analyzer (Keithley-2612A). Figure 2a A schematic diagram of an X-ray photoelectron spectroscopy (XPS) test of indium gallium zinc oxide (IGZO) without ultrasonic annealing provided in an embodiment of the present disclosure, Figure 2b This is a schematic diagram of an XPS test of indium gallium zinc oxide (IGZO) that has been ultrasonically annealed for 120 minutes according to an embodiment of the present disclosure. Figure 2c This is a schematic diagram of an XPS test of indium gallium zinc oxide (IGZO) that has been ultrasonically annealed for 180 minutes, provided in an embodiment of the present disclosure. Figure 3 A schematic diagram showing the atomic bonding comparison of indium gallium zinc oxide (IGZO) without and after ultrasonic annealing provided in the embodiment of the present disclosure. Figure 2a , 2b As shown in Figure 2c, the horizontal axis represents the electron binding energy, the vertical axis represents the intensity, the curve MO represents the chemical bond formed by the metal atom and the oxygen atom, the curve Vo represents the vacancy of the oxygen atom, and the curve impurity represents the chemical bond formed by the hydrogen atom and the oxygen atom.

[0086] Figure 3 It further shows Figure 2a , 2b The bonding ratios calculated from the XPS peak areas of different atoms in 2c, where the solid square curve represents the bonding ratio of metal atoms to oxygen atoms, the solid circle curve represents the vacancy ratio of oxygen atoms, and the solid triangle curve represents the bonding ratio of oxygen atoms to hydrogen atoms. Figure 3It can be seen intuitively from the curve that ultrasonic annealing can change the atomic bonding ratio. The bonding ratio of metal atoms to oxygen atoms in the IGZO subjected to ultrasonic annealing in the embodiment of the present disclosure (i.e., the bonding ratio of metal atoms to oxygen atoms corresponding to 120min and 180min) is greater than the bonding ratio of metal atoms to oxygen atoms in the IGZO that has not undergone ultrasonic annealing (i.e., the bonding ratio of metal atoms to oxygen atoms corresponding to w / o uitrasonic); the bonding ratio of oxygen atoms to hydrogen atoms in the IGZO subjected to ultrasonic annealing (i.e., the bonding ratio of oxygen atoms to hydrogen atoms corresponding to 120min and 180min) is less than the bonding ratio of oxygen atoms to hydrogen atoms in the IGZO that has not undergone ultrasonic annealing (i.e., the bonding ratio of metal atoms to oxygen atoms corresponding to w / o uitrasonic). uitrasonic corresponding to the bonding ratio of oxygen atoms to hydrogen atoms); the vacancy ratio of oxygen atoms in the IGZO after ultrasonic annealing (that is, the vacancy ratio of oxygen atoms corresponding to 120min and 180min) is smaller than the vacancy ratio of oxygen atoms in the IGZO without ultrasonic annealing (that is, the vacancy ratio of oxygen atoms corresponding to w / o uitrasonic).

[0087] For example, Figure 3 As shown, the bonding ratio of metal atoms to oxygen atoms in InGaZnO is greater than 53%; the metal atoms include indium, gallium and zinc; the bonding ratio of hydrogen atoms to oxygen atoms in InGaZnO is less than 23%; and the vacancy ratio of oxygen atoms in InGaZnO is less than 24%.

[0088] Figure 4a The energy displacement curves of gallium-oxygen bonding of the IGZO thin films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing provided in the embodiments of the present disclosure are as follows: Figure 4a The energy shift shown reflects that the Ga-O bonding ratio of the IGZO film after ultrasound is reduced, so that the oxide formed by Ga in the IGZO film after ultrasound is reduced. Figure 4b The energy displacement curves of indium-oxygen bonding of the IGZO film without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing provided in the embodiments of the present disclosure are as follows: Figure 4b The energy shift shown reflects that the In-O bonding ratio of the IGZO film after ultrasound is improved, so that the oxide formed by In in the IGZO film after ultrasound is increased, which can balance the bonding ratio of metal-oxygen atoms in the active layer.

[0089] Based on the above electrical performance tests of IGZO films that have been and have not been subjected to ultrasonic annealing, ultrasonic annealing can change the atomic bonding without changing the elemental composition of the semiconductor material, and the atomic bonding ratio after ultrasonic annealing is closer to the theoretical value, which can improve the mobility and stabilize the threshold voltage (subsequent tests have verified that the mobility of the device after ultrasonic annealing is greater than 20cm 2 V -1 s -1 , the threshold voltage is between 0 and 1V), thereby improving the yield of device preparation.

[0090] In some embodiments, the sum of the elastic modulus distribution ratios of the semiconductor material that has undergone ultrasonic annealing within the elastic modulus range a is greater than the sum of the elastic modulus distribution ratios of the semiconductor material that has not undergone ultrasonic annealing within the elastic modulus range b; a∈[c-5Gpa, c+5Gpa], c is the elastic modulus corresponding to the maximum elastic modulus distribution ratio of the semiconductor material that has undergone ultrasonic annealing; b∈[d-5Gpa, d+5Gpa], d is the elastic modulus corresponding to the maximum elastic modulus distribution ratio of the semiconductor material that has not undergone ultrasonic annealing.

[0091] Here, the semiconductor material is indium oxide as an example. Figure 5a A schematic diagram of elastic modulus distribution of an exemplary indium oxide material that has not been ultrasonically annealed provided in an embodiment of the present disclosure, Figure 5b A schematic diagram of elastic modulus distribution of an exemplary ultrasonically annealed indium oxide material provided in an embodiment of the present disclosure, wherein the abscissa represents the elastic modulus (GPa) and the ordinate represents the elastic modulus distribution ratio (%).

[0092] It should be noted that the method for testing the elastic modulus distribution of the film here is to use an atomic force microscope (AFM) in the quantitative nanomechanical mapping (QNM) mode to measure the elastic modulus distribution of the In2O3 film; the test conditions are room temperature and non-vacuum.

[0093] Depend on Figure 5a and 5bIt can be seen intuitively that the sum of the elastic modulus distribution ratios of the ultrasonically annealed indium oxide material in the elastic modulus range a is greater than the sum of the elastic modulus distribution ratios of the indium oxide material that has not been ultrasonically annealed in the elastic modulus range b. Here, the maximum elastic modulus distribution ratio of the ultrasonically annealed indium oxide material is 0.92%, c is 7.709GPa, and the maximum elastic modulus distribution ratio of the indium oxide material that has not been ultrasonically annealed is 0.78%, d is 8.860GPa. The elastic modulus of indium oxide is bimodal without ultrasound and unimodal after ultrasonic treatment. This may be because the microstructure and dynamic behavior of the precursor film before ultrasonic treatment show inhomogeneity, and the inhomogeneity of energy dissipation is manifested in different regions of high energy dissipation and low energy dissipation at the nanoscale, and the elastic moduli of these regions vary greatly. Ultrasound can make the distribution of these regions more uniform by promoting atomic relaxation. Low Young's modulus and uniform Young's modulus distribution can reduce the stress caused by strain in flexible indium oxide, and more importantly, it can improve the interface contact in the region where the Young's modulus changes.

[0094] like Figure 5a and 5b Comparative analysis shows that compared with the indium oxide material that has not been ultrasonically annealed, the elastic modulus distribution of the active layer after ultrasonic annealing presents a better single-peak normal distribution, that is, the elastic modulus distribution of the active layer is more concentrated on the highest peak, and the elastic modulus distribution is more uniform, which can improve the mobility of the thin film transistor and stabilize the threshold voltage. At the same time, the more uniform distribution of the elastic modulus can improve the interlayer shedding phenomenon of the thin film caused by strain or certain stress under conditions such as bending and torsion, and improve the yield rate and bending resistance of the device under strain.

[0095] Figure 6a A schematic diagram of the morphology of an indium oxide material that has not been ultrasonically annealed under AFM provided in an embodiment of the present disclosure, Figure 6b A schematic diagram of the morphology of an indium oxide material that has undergone ultrasonic annealing under AFM is provided in an exemplary embodiment of the present disclosure.

[0096] Figure 6a and Figure 6b The color depth of the indium oxide material represents the different distribution of elastic modulus values ​​in different regions. The smaller the color difference, the smaller the difference in elastic modulus and the more uniform the distribution of elastic modulus; conversely, the larger the color difference, the larger the difference in elastic modulus and the more uneven the distribution of elastic modulus. Figure 6a and 6b Comparative analysis shows that Figure 6a The black area in the image accounts for a large proportion. Figure 6bThe distribution of the black area accounts for a smaller proportion, which can indicate that the elastic modulus distribution of the indium oxide material after ultrasonic annealing is more uniform than that of the indium oxide material without ultrasonic annealing.

[0097] The above mechanical property tests all reflect that the elastic modulus distribution of the active layer after ultrasonic annealing is more uniform, which can improve the mobility of the thin film transistor and stabilize the threshold voltage. It can also improve the interlayer detachment phenomenon of the thin film caused by strain or certain stresses under conditions such as bending and torsion, thereby improving the yield and bending resistance of the device under strain.

[0098] In addition, the semiconductor material is indium oxide as an example. Figure 7a A schematic diagram of elastic modulus distribution of an exemplary indium gallium zinc oxide (IGZO) material that has not been ultrasonically annealed is provided in an embodiment of the present disclosure. Figure 7b A schematic diagram of elastic modulus distribution of an indium gallium zinc oxide (IGZO) material subjected to 120 min ultrasonic annealing provided in an embodiment of the present disclosure, Figure 7c A schematic diagram of elastic modulus distribution of an indium gallium zinc oxide (IGZO) material subjected to 180 minutes of ultrasonic annealing provided in an embodiment of the present disclosure, Figure 7d A schematic diagram of the elastic modulus distribution of an indium gallium zinc oxide (IGZO) material subjected to 240 min ultrasonic annealing provided in an embodiment of the present disclosure, wherein the abscissa represents the elastic modulus (GPa) and the ordinate represents the elastic modulus distribution ratio (%).

[0099] It should be noted that the method for testing the elastic modulus distribution of the film here is to use an atomic force microscope (AFM) in the quantitative nanomechanical mapping (QNM) mode to measure the elastic modulus distribution of the IGZO film; the test conditions are room temperature and non-vacuum.

[0100] Depend on Figure 7a to Figure 7d It can be seen intuitively that the sum of the elastic modulus distribution ratios of the IGZO material that has undergone ultrasonic annealing within the elastic modulus range a is greater than the sum of the elastic modulus distribution ratios of the IGZO material that has not undergone ultrasonic annealing within the elastic modulus range b. Figure 7a The maximum elastic modulus distribution ratio of the IGZO material without ultrasonic annealing is 2.19%, and d is 2.941 GPa; Figure 7b The maximum elastic modulus distribution ratio of the ultrasonically annealed IGZO material is 3.45%, and c is 3.395 GPa. Figure 7c The maximum elastic modulus distribution ratio of the ultrasonically annealed IGZO material is 1.77%, and c is 3.199 GPa. Figure 7d The maximum elastic modulus distribution ratio of the ultrasonically annealed IGZO material is 4.32%, and c is 4.692 GPa.

[0101] The elastic modulus of IGZO shows a bimodal distribution without ultrasound and a unimodal distribution after ultrasound treatment. This may be because the microstructure and dynamic behavior of the precursor film before ultrasound treatment show inhomogeneity, and the inhomogeneity of energy dissipation is manifested in different regions of high energy dissipation and low energy dissipation at the nanoscale, and the elastic moduli of these regions vary greatly. Ultrasound can make the distribution of these regions more uniform by promoting atomic relaxation. Low Young's modulus and uniform Young's modulus distribution can reduce the stress caused by strain in flexible IGZO, and more importantly, can improve the interface contact in the region where the Young's modulus changes.

[0102] like Figure 7a to Figure 7d Comparative analysis shows that compared with the IGZO material that has not been ultrasonically annealed, the elastic modulus distribution of the active layer after ultrasonic annealing presents a better single-peak normal distribution, that is, the elastic modulus distribution of the active layer is more concentrated on the highest peak, and the elastic modulus distribution is more uniform, which can improve the mobility of the thin film transistor and stabilize the threshold voltage. At the same time, the more uniform distribution of the elastic modulus can improve the interlayer shedding phenomenon of the thin film caused by strain or certain stress under conditions such as bending and torsion, and improve the yield rate and bending resistance of the device under strain.

[0103] Figure 8a A schematic diagram of the morphology of an exemplary IGZO material not subjected to ultrasonic annealing under AFM provided in an embodiment of the present disclosure, Figure 8b A schematic diagram of the morphology of an exemplary IGZO material subjected to 120 min ultrasonic annealing under AFM provided in an embodiment of the present disclosure, Figure 8c A schematic diagram of the morphology of an exemplary IGZO material subjected to 180 min ultrasonic annealing under AFM provided in an embodiment of the present disclosure, Figure 8d A schematic diagram of the morphology of an exemplary IGZO material that has undergone 240 minutes of ultrasonic annealing under AFM provided in an embodiment of the present disclosure.

[0104] Figures 8a to 8d The color depth of the IGZO material in the figure represents the different distribution of elastic modulus values ​​in different regions. The smaller the color difference, the smaller the difference in elastic modulus and the more uniform the distribution of elastic modulus; conversely, the larger the color difference, the larger the difference in elastic modulus and the more uneven the distribution of elastic modulus. Figures 8a to 8d Comparative analysis shows that Figure 8a The black area in the image accounts for a large proportion. Figure 8b and Figure 8c The black area accounts for a small proportion. Figure 8d compared to Figure 8bThe black area distribution accounts for a smaller proportion, but is larger than Figure 8c The distribution ratio of the black area in the middle can indicate that the elastic modulus distribution of the IGZO material after ultrasonic annealing is more uniform than that of the IGZO material without ultrasonic annealing. However, the ultrasonic annealing time should be well controlled to avoid uneven elastic modulus distribution caused by long-term ultrasonic annealing.

[0105] The above mechanical property tests all reflect that the elastic modulus distribution of the active layer after ultrasonic annealing is more uniform, which can improve the mobility of the thin film transistor and stabilize the threshold voltage. It can also improve the interlayer detachment phenomenon of the thin film caused by strain or certain stresses under conditions such as bending and torsion, thereby improving the yield and bending resistance of the device under strain.

[0106] Of course, this embodiment only simulates indium oxide and indium gallium zinc oxide. The elastic modulus distributions of other amorphous oxide semiconductor materials before and after ultrasonic annealing are similar and are not listed here one by one.

[0107] In some embodiments, a first difference between a maximum value and a minimum value of stress experienced by the semiconductor material that has undergone ultrasonic annealing is smaller than a second difference between a maximum value and a minimum value of stress experienced by the semiconductor material that has not undergone ultrasonic annealing. Figure 9a A schematic diagram of a bending simulation of an exemplary indium gallium zinc oxide (IGZO) material that has not been ultrasonically treated is provided in an embodiment of the present disclosure. Figure 9b A schematic diagram of a bending simulation of an exemplary ultrasonically treated indium gallium zinc oxide (IGZO) material provided in an embodiment of the present disclosure, wherein the semiconductor material is indium gallium zinc oxide (IGZO) material as an example for illustration, Figure 9a and Figure 9b As shown in the figure, the bending degree of the IGZO material before and after ultrasonic annealing is the same, and the surface stress distribution is different. For example, when the bending degree of the IGZO material without ultrasonic annealing and the IGZO material after ultrasonic annealing are at a certain preset value, the maximum stress of the IGZO material without ultrasonic annealing is 2.78×10 9 N / m 2 The minimum stress of the indium gallium zinc oxide (IGZO) material without ultrasonic annealing is 2.67×10 6 N / m 2 The maximum stress of the ultrasonically annealed indium gallium zinc oxide (IGZO) material is 2.76×10 9 N / m 2 The minimum stress of the ultrasonically annealed indium gallium zinc oxide (IGZO) material is 2.61×10 6 N / m2 The maximum difference in stress of the ultrasonically annealed indium gallium zinc oxide (IGZO) material is 2.757×10 9 N / m 2 The maximum difference in stress of the indium gallium zinc oxide (IGZO) material without ultrasonic annealing is 2.777×10 9 N / m 2 , the first difference of stress on the ultrasonically annealed indium gallium zinc oxide (IGZO) material is less than the second difference of stress on the ultrasonically annealed indium gallium zinc oxide (IGZO) material, which can explain that the stress distribution range of the ultrasonically annealed indium gallium zinc oxide (IGZO) material is narrower and more uniform than that of the indium gallium zinc oxide (IGZO) material that has not been ultrasonically annealed, thereby reflecting that the high energy dissipation area and the low energy dissipation area of ​​the active layer are more uniformly distributed, that is, the overall in-plane energy dissipation is uniform, reducing the difference in mechanical properties of the entire film, and reducing the difference between the extremely high and extremely low values ​​of the in-plane mechanical parameters and the average value. Energy dissipation can be reflected in the energy required for atomic relaxation, the energy required for formation, etc. Therefore, it can be seen that ultrasonic annealing has the effect of improving the mechanical stability between the layers of thin film transistors and resisting stress failure.

[0108] In some embodiments, the contact angle of the IGZO film was measured using the Sessile drop technique of a contact angle goniometer (Datphysics-oca50). The experimental liquids were deionized water (DIW) and ethylene glycol (CH2OH)2. Here, the contact angle refers to the angle between the tangent line of the gas-liquid interface at the intersection of the gas, liquid and solid phases and the solid-liquid boundary line.

[0109] Figures 10a to 10c The measured images of DIW contact angle of IGZO films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing are shown in Figure 2. Figures 10a to 10c As shown in Figure 5, the contact angle of DIW on the IGZO film increases continuously after ultrasonic treatment. Figures 11a to 11c The measured images of (CH2OH)2 contact angles of IGZO films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing are shown in Figure 2. Figures 11a to 11c As shown, after ultrasonic treatment, the contact angle of (CH2OH)2 on the IGZO film increases continuously. Fig.12 Figure 1 is a schematic diagram of the surface energy data of IGZO films without ultrasonic annealing, after 120 min ultrasonic annealing, and after 180 min ultrasonic annealing. s represents the surface energy, and They are γ sThe Disp component and Polar component of (CH2OH)2 and DIW contact angles show the same trend, that is, contact angle (without ultrasonic annealing) < contact angle (after 120 min ultrasonic annealing) < contact angle (after 180 min ultrasonic annealing). The trend of surface energy values ​​is surface energy (without ultrasonic annealing) > surface energy (after 120 min ultrasonic annealing) > surface energy (after 180 min ultrasonic annealing).

[0110] For IGZO films, the increase in contact angle and the decrease in surface energy will reduce the adsorption of water molecules in the air, which plays an important role in improving the performance of IGZO films. The reduction in surface energy is caused by atomic relaxation caused by ultrasound. Generally speaking, atomic relaxation is most intense in the atomic layer on the surface of the material. The surface of amorphous oxide materials is a non-stoichiometric surface, and its surface energy is usually greater than that of dense crystals. The strong relaxation of surface atoms causes the surface to transform from non-stoichiometric ratio to dense stacking, thereby reducing the surface energy of IGZO films.

[0111] In some embodiments, the method for preparing a thin film transistor further includes the step of forming other layer structures of the thin film transistor. Exemplarily, taking the preparation of a driving transistor as an example, after forming an active layer, a pattern including a gate insulating layer is formed on the side of the active layer away from the substrate through a patterning process; thereafter, a pattern including a gate is formed on the side of the gate insulating layer away from the substrate through a patterning process.

[0112] Here, the patterning process includes at least the process of depositing material layers and patterning. The deposition method may include but is not limited to physical and chemical methods such as atomic layer deposition, magnetron sputtering, plasma enhanced chemical vapor deposition, electron beam evaporation, and chemical spin coating. The patterning method may include but is not limited to adding a mask during the deposition process, etching after film preparation, and photolithography.

[0113] In addition, an embodiment of the present disclosure also provides a thin film transistor, which includes a source, a drain, an active layer and a gate, the active layer includes a source contact region, a drain contact region and a channel region sandwiched between the source contact region and the drain contact region; the channel region overlaps with the gate in the orthographic projection on the substrate where the thin film transistor is located, the source is electrically connected to the active layer located in the source contact region, and the drain is electrically connected to the active layer located in the drain contact region.

[0114] Here, the material of the active layer can be obtained by ultrasonic annealing of semiconductor materials. Figure 2a to 2c , Figure 3 ,as well as Figure 4a-4bAs shown, the material of the active layer is indium gallium zinc oxide; the bonding ratio of metal atoms to oxygen atoms in indium gallium zinc oxide is greater than 53%; the metal atoms include indium, gallium and zinc; the bonding ratio of hydrogen atoms to oxygen atoms in indium gallium zinc oxide is less than 23%; the vacancy ratio of oxygen atoms in indium gallium zinc oxide is less than 24%. The material of the active layer in the disclosed embodiment is a material that has been subjected to ultrasonic annealing. The atomic bonding ratio of the active layer after ultrasonic annealing is closer to the theoretical value, which can improve the mobility and stabilize the threshold voltage (subsequent tests have verified that the mobility of the device after ultrasonic annealing is greater than 20cm 2 V -1 s -1 , the threshold voltage is between 0 and 1V), thereby improving the yield of device preparation.

[0115] The thin film transistor provided in the embodiment of the present disclosure can be prepared by using the method for preparing the thin film transistor provided in the above embodiment, and the repeated parts will not be described again.

[0116] In some embodiments, the material of the active layer includes indium gallium zinc oxide, and the composition ratio of indium, gallium and zinc is 1:1:1.

[0117] In some embodiments, Fig.13 The electrical characteristics diagram of the thin film transistor provided by the embodiment of the present disclosure is as follows: Fig.13 As shown, the horizontal axis represents the gate voltage V G , the first ordinate represents the driving current I D The second ordinate represents the 1 / 2 power of the driving current I D 1 / 2 Among them, the solid square curve represents the TFT characteristic curve when the ultrasonic annealing time is 120 minutes, the solid circle curve represents the TFT characteristic curve when the ultrasonic annealing time is 180 minutes, and the solid triangle curve represents the TFT characteristic curve without ultrasonic annealing.

[0118] The active layer finally formed by ultrasonic annealing has a carrier mobility greater than or equal to 20cm 2 V -1 s -1 .like Fig.13 It can be seen from the characteristic curves shown that the mobility of the thin film transistor after ultrasonic annealing (ie, curve A1 and curve A2) is smaller than the mobility of the thin film transistor without ultrasonic annealing (ie, curve A3).

[0119] Mobility is an important parameter for evaluating the characteristics of thin film transistors (TFTs). High mobility can enable thin film transistors to obtain better characteristics. The carrier mobility of the active layer formed by ultrasonic annealing in this embodiment is greater than or equal to 20 cm 2 V-1 s -1 Such higher mobility enables the thin film transistor of this embodiment to obtain better characteristics.

[0120] In some embodiments, the on / off ratio of the thin film transistor prepared by ultrasonic annealing is greater than or equal to 10 8 .like Fig.13 As shown, the lowest point of each curve in the A group of curves represents the off-state current, the highest point of each curve represents the on-state current, and the ratio of the on-state current to the off-state current is the switching ratio. Fig.13 It can be seen intuitively from the characteristic curve diagram that the on-state current of the thin film transistor prepared by ultrasonic annealing (i.e., curve A1 and curve A2) is greater than the on-state current of the thin film transistor prepared without ultrasonic annealing (i.e., curve A3); the off-state current of the thin film transistor prepared by ultrasonic annealing (i.e., curve A1 and curve A2) is less than the off-state current of the thin film transistor prepared without ultrasonic annealing (i.e., curve A3), so the switching ratio of the thin film transistor prepared by ultrasonic annealing (i.e., curve A1 and curve A2) is greater than the switching ratio of the thin film transistor prepared without ultrasonic annealing (i.e., curve A3).

[0121] The device on-off ratio is an important parameter for evaluating the characteristics of thin film transistors (TFTs). The on-off ratio of the thin film transistors prepared by ultrasonic annealing in this embodiment is greater than or equal to 10 8 This higher switching ratio can effectively improve the characteristics of thin film transistors (TFTs).

[0122] In some embodiments, the subthreshold swing of the thin film transistor is between 0.05 mV / dec and 0.25 mV / dec. Fig.13 It can be seen from the characteristic curves shown that the subthreshold swing of the thin film transistor prepared by ultrasonic annealing (ie, curve A1 and curve A2) is smaller than the subthreshold swing of the thin film transistor prepared without ultrasonic annealing (ie, curve A3).

[0123] Subthreshold swing is a performance indicator that measures the conversion rate between the on and off states of a transistor. It represents the change in gate voltage required for a tenfold change in source-drain current, also known as the S factor. The smaller the S factor, the faster the on / off rate. The subthreshold swing of the thin-film transistor prepared by ultrasonic annealing in this embodiment is between 0.05mV / dec and 0.25mV / dec, from which it can be seen that ultrasonic annealing improves the electrical characteristics of the thin-film transistor.

[0124] In some embodiments, the threshold voltage of the thin film transistor is between 0 and 1 V. Fig.13As shown, the gate voltage corresponding to the tangent of each curve in the B group of curves on the ordinate is the threshold voltage. It can be seen intuitively from the characteristic curve diagram of Figure 11 that the threshold voltage of the thin film transistor prepared by ultrasonic annealing (i.e., curve B1 and curve B2) is about 0V, which is smaller than the threshold voltage of the thin film transistor prepared without ultrasonic annealing (i.e., curve B3) which is about 2V.

[0125] The threshold voltage of the thin film transistor prepared by ultrasonic annealing in this embodiment is closer to 0V, which can effectively improve the TFT characteristics.

[0126] In addition, an embodiment of the present disclosure further provides a display substrate, including a base substrate and a pixel driving circuit arranged on the base substrate; at least one thin film transistor in the pixel driving circuit is a thin film transistor of any one of the above embodiments.

[0127] The thin film transistor can be any one of the following: a polysilicon thin film transistor, an amorphous silicon thin film transistor, or an amorphous silicon thin film transistor. Exemplarily, the pixel driving circuit includes a switching transistor and a driving transistor. The switching transistor can be a low-temperature polysilicon thin film transistor or an amorphous silicon thin film transistor, and the driving transistor can be an amorphous oxide thin film transistor.

[0128] Exemplarily, each thin film transistor in the display substrate is a low temperature polysilicon thin film transistor; or each thin film transistor in the display substrate is an amorphous oxide thin film transistor. Alternatively, each thin film transistor in the display substrate includes at least a low temperature polysilicon thin film transistor and an amorphous oxide thin film transistor.

[0129] In some embodiments, the substrate substrate may be a flexible substrate. The thin film transistor in the display substrate of the embodiment of the present disclosure includes an active layer formed by an ultrasonic annealing process. Experimental tests show that the display substrate meets the electrical failure condition (that is, the mobility and switching ratio data drop to 70% of the initial state of the product), and the display substrate with flexible performance is bent more than 100,000 times. It can be seen that the display substrate prepared by ultrasonic annealing has good resistance to electrical failure. The display substrate with flexible performance meets the interlayer failure condition (that is, macroscopic mechanical damage is generated at the interface between the active layer and its upper and lower contact layers), and the display substrate is bent more than 200,000 times. It can be seen that the display substrate prepared by ultrasonic annealing has good resistance to interlayer failure.

[0130] In some embodiments, the substrate substrate includes, but is not limited to, various organic and inorganic, rigid and flexible substrates.

[0131] In some embodiments, the step of forming a display substrate may include providing a base substrate; forming a pattern including a buffer layer on the base substrate through a patterning process. Then, forming a pattern including an active layer on the side of the buffer layer facing away from the base substrate through a patterning process. Then, forming a pattern including a gate insulating layer on the side of the active layer facing away from the base substrate through a patterning process. Here, the patterning process at least includes the process of depositing material layers and patterning. Among them, the deposition method may include but is not limited to physical and chemical methods such as atomic layer deposition, magnetron sputtering, plasma enhanced chemical vapor deposition, electron beam evaporation, and chemical spin coating. The patterning method may include but is not limited to methods such as adding a mask during the deposition process, etching after film layer preparation, and photolithography. An active layer is formed on the buffer layer,

[0132] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A method for preparing a thin film transistor, comprising: The step of patterning the semiconductor material layer to form an active layer; wherein the preparation method further comprises: a step of ultrasonic annealing the semiconductor material to form the active layer.

2. The method for preparing a thin film transistor according to claim 1, wherein: The step of ultrasonically annealing the semiconductor material to form the active layer comprises: Forming the semiconductor material layer, at least performing ultrasonic annealing on the semiconductor material at a position of the semiconductor material layer corresponding to the position where the active layer is to be formed; The step of patterning the semiconductor material layer to form an active layer comprises: The semiconductor material layer after ultrasonic annealing is patterned to form an active layer of the thin film transistor.

3. The method for preparing a thin film transistor according to claim 2, wherein: The forming of the semiconductor material layer, at least ultrasonically annealing the semiconductor material at a position of the semiconductor material layer corresponding to the position where the active layer is to be formed, comprises: The semiconductor material layer is formed, and ultrasonic annealing is performed on the entire semiconductor material layer; the acoustic field of the ultrasonic annealing is located in the center and edge areas of the entire semiconductor material layer.

4. The method for preparing a thin film transistor according to claim 1, wherein: The ultrasonic frequency of the ultrasonic annealing is between 40kHz and 200kHz.

5. The method for preparing a thin film transistor according to claim 1, wherein: The duration of the ultrasonic annealing is between 5 minutes and 240 minutes.

6. The method for preparing a thin film transistor according to claim 1, wherein: The ultrasonic annealing environment includes an environment filled with any one of nitrogen, oxygen and argon.

7. The method for preparing a thin film transistor according to claim 1, wherein: The heating method of the ultrasonic annealing includes any one of laser, microwave, light wave, solid-state heat conduction, and gaseous heat conduction.

8. The method for preparing a thin film transistor according to any one of claims 1 to 7, wherein: The material of the active layer is amorphous material.

9. The method for preparing a thin film transistor according to claim 8, wherein: The semiconductor material is an amorphous oxide material; The bonding ratio of metal atoms to oxygen atoms in the amorphous oxide material after the ultrasonic annealing is greater than the bonding ratio of metal atoms to oxygen atoms in the amorphous oxide material not after the ultrasonic annealing; The bonding ratio of oxygen atoms to hydrogen atoms in the amorphous oxide material after the ultrasonic annealing is less than the bonding ratio of oxygen atoms to hydrogen atoms in the amorphous oxide material not after the ultrasonic annealing; The vacancy ratio of oxygen atoms in the amorphous oxide material after the ultrasonic annealing is less than the vacancy ratio of oxygen atoms in the amorphous oxide material not after the ultrasonic annealing; The sum of the bonding ratio of metal atoms to oxygen atoms, the bonding ratio of oxygen atoms to hydrogen atoms, and the vacancy ratio of oxygen atoms in the amorphous oxide material that has undergone the ultrasonic annealing is 1; the sum of the bonding ratio of metal atoms to oxygen atoms, the bonding ratio of oxygen atoms to hydrogen atoms, and the vacancy ratio of oxygen atoms in the amorphous oxide material that has not undergone the ultrasonic annealing is 1.

10. The method for preparing a thin film transistor according to any one of claims 1 to 7, wherein: The sum of the elastic modulus distribution ratios within the elastic modulus range a of the semiconductor material that has undergone the ultrasonic annealing is greater than the sum of the elastic modulus distribution ratios within the elastic modulus range b of the semiconductor material that has not undergone the ultrasonic annealing; a∈[c-5Gpa, c+5Gpa], where c is the elastic modulus corresponding to the maximum elastic modulus distribution ratio of the semiconductor material that has undergone the ultrasonic annealing; b∈[d-5Gpa, d+5Gpa], where d is the elastic modulus corresponding to the maximum elastic modulus distribution ratio of the semiconductor material that has not undergone the ultrasonic annealing.

11. The method for preparing a thin film transistor according to any one of claims 1 to 7, wherein: When the bending degrees of the semiconductor material before and after the ultrasonic annealing are the same, a first difference between the maximum value and the minimum value of the stress experienced by the semiconductor material after the ultrasonic annealing is smaller than a second difference between the maximum value and the minimum value of the stress experienced by the semiconductor material without the ultrasonic annealing.

12. A thin film transistor, comprising a source electrode, a drain electrode, an active layer and a gate electrode, wherein the active layer comprises a source contact region, a drain contact region and a channel region sandwiched between the source contact region and the drain contact region; the channel region overlaps with the orthographic projection of the gate electrode on the substrate where the thin film transistor is located, the source electrode is electrically connected to the active layer located in the source contact region, and the drain electrode is electrically connected to the active layer located in the drain contact region; The material of the active layer is indium gallium zinc oxide; the bonding ratio of metal atoms to oxygen atoms in the indium gallium zinc oxide is greater than 53%; the metal atoms include indium, gallium and zinc; the bonding ratio of hydrogen atoms to oxygen atoms in the indium gallium zinc oxide is less than 23%; and the vacancy ratio of oxygen atoms in the indium gallium zinc oxide is less than 24%.

13. The thin film transistor according to claim 12, wherein: The material of the active layer is indium gallium zinc oxide, and the composition ratio of indium, gallium and zinc is 1:1:

1.

14. The thin film transistor according to claim 12, wherein: The carrier mobility of the active layer is greater than or equal to 20 cm 2 V -1 s -1 .

15. The thin film transistor according to claim 12, wherein: The switching ratio of the thin film transistor is greater than or equal to 10 8 .

16. The thin film transistor according to claim 12, wherein: The subthreshold swing of the thin film transistor is between 0.05mV / dec and 0.25mV / dec.

17. The thin film transistor according to claim 12, wherein: The threshold voltage of the thin film transistor is between 0V and 1V.

18. A display substrate, comprising a base substrate and a pixel driving circuit arranged on the base substrate; at least one thin film transistor in the pixel driving circuit is the thin film transistor according to any one of claims 12 to 17.

19. The display substrate according to claim 18, wherein: The substrate base is a flexible substrate.