Electrochemical device and electronic device

By designing cathode and anode material layers with specific structures in lithium-ion batteries, combined with specific delithiation products and silicon elements, the problem of energy density, safety performance and cycle performance in the existing technology is difficult to balance, and high energy density and Battery with good safety performance.

CN118738520APending Publication Date: 2024-10-01NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410916811.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When existing lithium-ion batteries improve safety performance and cycle performance, they usually need to sacrifice energy density, making it difficult to balance the three under high energy density conditions.

Method used

An electrochemical device including a positive electrode piece and a negative electrode piece is used. The positive electrode piece is composed of first and second positive electrode material layers. The first positive electrode material layer contains specific delithiation products such as Li5-xFeO4-y, Li5-xCoO4-y. , Li2-zMnO2 or L i1.2-rNi0.13Fe0.13Mn0.54O2, the second positive electrode material layer contains lithium cobalt oxide and other materials, and the negative electrode sheet contains silicon element. By adjusting the material proportion and structural design, the energy density, safety performance and safety performance of the electrochemical device are improved. Cycle performance.

Benefits of technology

It achieves high energy density while improving the safety performance and cycle performance of lithium-ion batteries, reducing irreversible capacity loss and the decrease in first Coulomb efficiency, and extending the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738520A_ABST
    Figure CN118738520A_ABST
Patent Text Reader

Abstract

The invention provides an electrochemical device and an electronic device. The electrochemical device comprises a positive pole piece and a negative pole piece, the positive pole piece comprises a first active material, and a lithium removal product of the first active material comprises at least one of Li < 5-x > FeO < 4-y >, Li < 5-x > CoO < 4-y >, Li < 2-z > MnO2, Li < 1.2-r > Ni < 0.13 > Fe < 0.13 > Mn < 0.54 > O2 or Li < 1-t > FePO4; the negative pole piece comprises a negative pole material layer, the negative pole material layer comprises a silicon element, and based on the mass of the negative pole material layer, the mass percentage of the silicon element is 1-50%; the mass of the lithium removal product of the first active material in the positive pole piece is A mg / 1540 mm < 2 >, the mass of the silicon element in the negative pole piece is B mg / 1540 mm < 2 >, and A / B is greater than or equal to 29% and less than or equal to 230%. With the characteristics, the electrochemical device can have high energy density, good safety performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art

[0002] Electrochemical devices, such as lithium-ion batteries, have entered our daily lives with the advancement of technology and the improvement of environmental protection requirements. With the widespread popularity of lithium-ion batteries, safety issues such as puncturing lithium-ion batteries by external forces will occur on the user side. Its safety performance has received more and more attention, especially the continued fermentation of some mobile phone explosion incidents, which has led to new requirements for the safety performance of lithium-ion batteries by users, after-sales service and lithium-ion battery manufacturers.

[0003] Currently, most methods for improving the safety performance of lithium-ion batteries are at the expense of their energy density and cycle performance. Therefore, there is an urgent need to provide a technical means to improve the safety performance and cycle performance of lithium-ion batteries under conditions of higher energy density. Summary of the invention

[0004] The purpose of this application is to provide an electrochemical device and an electronic device, so that the electrochemical device has both high energy density and good safety performance and cycle performance. The specific technical solution is as follows:

[0005] The first aspect of the present application provides an electrochemical device, which includes a positive electrode sheet and a negative electrode sheet, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer, the positive electrode material layer includes a first positive electrode material layer and a second positive electrode material layer, the first positive electrode material layer is arranged between the positive electrode current collector and the second positive electrode material layer, the first positive electrode material layer includes a first active material, and the delithiation product of the first active material includes Li 5-x FeO 4-y , Li 5-x CoO 4-y , Li 2-z MnO 2 , Li 1.2- r Ni 0.13 Fe 0.13 Mn 0.54 O 2 or Li 1-t FePO 4At least one of the following, wherein 4≤x≤5, 2≤y≤3, 1.6≤z≤2, 1≤r≤1.2, 0.8≤t≤1. The second positive electrode material layer includes a second active material, and the second active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate or lithium manganese oxide; the negative electrode plate includes a negative electrode material layer, and the negative electrode material layer includes silicon element, and the mass percentage of silicon element is 1% to 50% based on the mass of the negative electrode material layer. The mass of the delithiation product of the first active material in the positive electrode plate is Amg / 1540mm 2 The mass of silicon in the negative electrode is B mg / 1540 mm 2 , 29%≤A / B≤230%. The electrochemical device includes a positive electrode plate and a negative electrode plate having the above characteristics, and the mass percentage of silicon element and the value of A / B are regulated within the above range. The negative electrode material layer has a higher gram capacity. At the same time, the first active material is used for lithium supplementation, which is beneficial to reduce the loss of irreversible capacity of the second active material during the first charge, and improve the first coulomb efficiency of the second active material, thereby improving the energy density and cycle performance of the secondary battery. At the same time, the delithiation product of the first active material is the above substance, which can make the positive electrode plate have suitable resistivity and bonding properties, and thus can also improve the safety performance of the electrochemical device. Therefore, satisfying the above characteristics can enable the electrochemical device to have both high energy density, good safety performance and cycle performance.

[0006] In some embodiments of the present application, 39%≤A / B≤200%. By regulating the value of A / B within the above range, the electrochemical device can have high energy density, better safety performance and cycle performance.

[0007] In some embodiments of the present application, the delithiation product of the first active material includes LiFeO 2 、CoO 2 、MnO 2 、Ni 0.13 Fe 0.13 Mn 0.54 O 2 、FePO 4 ,FeO 2 , Fe 2 O 3 The delithiation product of the first active material in the first positive electrode material layer includes the above materials, which can make the first positive electrode material layer have suitable resistivity and good bonding performance, and can make the electrochemical device have high energy density while improving its safety performance and cycle performance.

[0008] In some embodiments of the present application, based on the mass of the first positive electrode material layer, the mass percentage of the delithiation product of the first active material is 30% to 96%. By regulating the mass percentage of the delithiation product of the first active material within the above range, the first positive electrode material layer can have a suitable resistivity and bonding performance, and the electrochemical device can have a high energy density while improving its safety performance and cycle performance.

[0009] In some embodiments of the present application, in the positive electrode sheet, the mass of the second active material is C mg / 1540 mm 2 , 0.45%≤A / C≤6%, preferably 0.9%≤A / C≤4.5%. By regulating the A / C value within the above range, the electrochemical device can have a high energy density while improving its safety performance and cycle performance.

[0010] In some embodiments of the present application, based on the mass of the negative electrode material layer, the mass percentage of the silicon element is 1% to 20%, which can make the electrochemical device have a higher energy density while improving its safety performance.

[0011] In some embodiments of the present application, the electrochemical device satisfies at least one of the following characteristics: (1) 1 mg / 1540 mm 2 / ≤A≤14mg / 1540mm 2 ; (2) 3mg / 1540mm 2 ≤B≤12mg / 1540mm 2 ; (3) 200mg / 1540mm 2 ≤C≤300mg / 1540mm 2 Meeting the above characteristics can make the electrochemical device have high energy density while improving its safety performance and cycle performance.

[0012] In some embodiments of the present application, the first positive electrode material layer also includes an inorganic material, and the inorganic material includes at least one of aluminum oxide, lithium lanthanum zirconium oxide, lithium lanthanum titanate, lithium aluminum titanium phosphate, antimony-doped tin oxide or titanium oxide; based on the mass of the first positive electrode material layer, the mass percentage of the inorganic material is 5% to 60%. The first positive electrode material layer includes the above-mentioned inorganic material, and its mass percentage is regulated within the above-mentioned range, which can improve the stability of the first positive electrode material layer, so that the first positive electrode material layer has good bonding properties and suitable resistivity, reduces the probability of internal short circuit and the heat generated by the internal short circuit, thereby facilitating further improving the safety performance of the electrochemical device.

[0013] In some embodiments of the present application, the specific capacity of the first positive electrode material layer is 130 mAh / g to 780 mAh / g. Since the first active material has a high specific capacity, the specific capacity of the first positive electrode material layer is within the above range. When the electrochemical device is charged for the first time, the loss of active lithium caused by the formation of a solid electrolyte interface film (SEI film) can be improved, and the irreversible capacity loss of the electrochemical device and the reduction of the first coulombic efficiency can be reduced, so that the electrochemical device has a high energy density while further improving its cycle performance.

[0014] In some embodiments of the present application, the specific capacity of the first positive electrode material layer is greater than or equal to the specific capacity of the second positive electrode material layer. The specific capacities of the first positive electrode material layer and the second positive electrode material layer satisfy the above relationship, which is more conducive to exerting the lithium replenishing effect of the first active material during the first charge and discharge, reducing the loss of active lithium in the second positive electrode material layer, reducing the irreversible capacity loss of the electrochemical device and the reduction of the first coulombic efficiency, so that the electrochemical device has a high energy density while further improving its cycle performance.

[0015] In some embodiments of the present application, the first active material includes at least one of the following compounds: Li 5 QO 4 or Li 5 QO 6 , Q includes at least one of Ni, Co, Fe, Sn or Mn, and the valence state of the Q element is lower than its own highest oxidation valence state; Li q Fe 0.5(1+q) PO 4 , 1≤q≤5; Li 2-a-b-c-d Ni a R b Mn c M d O 2-f , 0≤a<0.35, 0<b<0.5, 0.3<c≤0.6, 0≤d<0.05, 0.7<a+b+c+d<0.9, 0≤f<0.2, R includes at least one of Fe or Co, M includes at least one of Mg, Al, Ti, V, Cr, Cu, Y, Zr, Nb, Mo, La or W; Li 1+e Mn 1-p X p O 2-s Y s, -0.1<e<0.2, 0≤p<0.2, 0≤s<0.2, X includes at least one of Fe, Co, Ni, Ti, Zn, Mg, Al, V, Cr or Zr, and Y includes at least one of S, N, F, Cl or Br. The first active material within the above range has a higher specific capacity and a lower first coulombic efficiency, which is beneficial to reduce the loss of the first coulombic efficiency and the irreversible capacity. The above first active material has good stability, which can make the electrochemical device have good cycle performance. At the same time, the positive electrode sheet has a suitable resistivity, the positive electrode material layer and the positive electrode current collector have a high bonding force, and the safety performance of the electrochemical device can also be improved. Therefore, the selection of the above materials can make the electrochemical device have high energy density, good safety performance and cycle performance.

[0016] In some embodiments of the present application, the first active material includes Li 5 FeO 4 , Li 5 CoO 4 , Li 2 MnO 2 , Li 1.2 Ni 0.13 Fe 0.13 Mn 0.54 O 2 or LiFePO 4 The selection of the first active material is more conducive to the lithium supplementation effect of the first active material, so that the electrochemical device has a high energy density and further improves its safety performance and cycle performance.

[0017] In some embodiments of the present application, the negative electrode material layer includes a negative electrode active material, and the negative electrode active material includes at least one of silicon, silicon carbon or silicon oxygen. The above materials have a high gram capacity, and the negative electrode active material includes the above materials, which can make the electrochemical device have a high energy density.

[0018] In some embodiments of the present application, the negative electrode active material further includes at least one of graphite, hard carbon, soft carbon or mesophase microcarbon beads.

[0019] In some embodiments of the present application, the resistivity of the positive electrode material layer is ρΩ·m, 44≤ρ≤155. The resistivity of the positive electrode material layer is within the above range, indicating that the positive electrode material layer has a suitable impedance, which can reduce the probability of internal short circuit of the electrochemical device and reduce the heat generated during the internal short circuit, thereby facilitating further improving the safety performance of the electrochemical device.

[0020] The second aspect of the present application provides an electronic device, which includes the electrochemical device provided in the first aspect of the present application. The electrochemical device provided in the first aspect of the present application has high energy density, good safety performance and cycle performance, so that the electronic device of the present application has good performance and a long service life.

[0021] Beneficial effects of this application:

[0022] The present application provides an electrochemical device and an electronic device. The electrochemical device includes a positive electrode sheet and a negative electrode sheet, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer, the positive electrode material layer includes a first positive electrode material layer and a second positive electrode material layer, the first positive electrode material layer is arranged between the positive electrode current collector and the second positive electrode material layer, the first positive electrode material layer includes a first active material, and the delithiation product of the first active material includes Li 5-x FeO 4-y , Li 5-x CoO 4-y , Li 2-z MnO 2 , Li 1.2- r Ni 0.13 Fe 0.13 Mn 0.54 O 2 or Li 1-t FePO 4 At least one of the above, the second positive electrode material layer includes a second active material, the second active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate or lithium manganese oxide; the negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes silicon element, and the mass percentage of silicon element is 1% to 50% based on the mass of the negative electrode material layer; the mass of the delithiation product of the first active material in the positive electrode plate is Amg / 1540mm 2 The mass of silicon in the negative electrode is B mg / 1540 mm 2 , 29%≤A / B≤230%. The electrochemical device includes a positive electrode sheet and a negative electrode sheet having the above characteristics, and the mass percentage of silicon element and the value of A / B are regulated within the above range, so that the electrochemical device has high energy density, good safety performance and cycle performance.

[0023] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0025] Figure 1 It is a schematic diagram of the structure of the positive electrode plate in one embodiment of the present application.

[0026] Reference numerals: positive electrode sheet 10 , first positive electrode material layer 11 , second positive electrode material layer 12 , positive electrode current collector 13 . DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0028] It should be noted that in the specific implementation of the present application, lithium-ion batteries are used as an example of electrochemical devices to explain the present application, but the electrochemical devices of the present application are not limited to lithium-ion batteries. The specific technical solution is as follows:

[0029] The first aspect of the present application provides an electrochemical device, which includes a positive electrode sheet and a negative electrode sheet, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer, the positive electrode material layer includes a first positive electrode material layer and a second positive electrode material layer, the first positive electrode material layer is arranged between the positive electrode current collector and the second positive electrode material layer. The first positive electrode material layer includes a first active material, and the delithiation product of the first active material includes Li 5-x FeO 4-y , Li 5-x CoO 4-y , Li 2-z MnO 2 , Li 1.2- r Ni 0.13 Fe 0.13 Mn 0.54 O 2 or Li 1-t FePO 4At least one of, wherein 4≤x≤5, 2≤y≤3, 1.6≤z≤2, 1≤r≤1.2, 0.8≤t≤1. The second positive electrode material layer includes a second active material, and the second active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate or lithium manganese oxide; the negative electrode plate includes a negative electrode material layer, and the negative electrode material layer includes silicon element, and the mass percentage of silicon element is 1% to 50%, preferably 1% to 20% based on the mass of the negative electrode material layer; for example, the mass percentage of silicon element can be 1%, 2.2%, 5%, 8%, 10%, 12.2%, 14.2%, 17%, 20%, 23%, 26%, 30%, 33%, 35%, 37%, 40%, 43%, 45%, 47%, 50% or a range consisting of any two of the values. The mass of the delithiation product of the first active material in the positive electrode sheet is Amg / 1540mm 2 The mass of silicon in the negative electrode is B mg / 1540 mm 2 , 29%≤A / B≤230%, preferably 39%≤A / B≤200%. For example, the value of A / B can be 29%, 34%, 39%, 45%, 47%, 50%, 55%, 58%, 60%, 62%, 69%, 70%, 75%, 78%, 80%, 85%, 88%, 92%, 95%, 100%, 105%, 110%, 114%, 116%, 130%, 150%, 160%, 175%, 190%, 210%, 215%, 230%, or a range consisting of any two of the values.

[0030] The negative electrode material layer includes silicon elements and the mass percentage of silicon elements is regulated within the above range, which can make the electrochemical device have a higher energy density. Selecting the above second active material as the main positive electrode material can make the electrochemical device have better cycle performance and higher first coulombic efficiency. During the first charge of the electrochemical device, the formation of a solid electrolyte interface film (SEI film) on the surface of the silicon-containing negative electrode will consume a large amount of active lithium released from the positive electrode, resulting in a decrease in the first coulombic efficiency of the electrochemical device and irreversible capacity loss. The inventors found that when the first active material is used for lithium supplementation, the first active material has a higher specific capacity and a lower first coulombic efficiency. After the electrochemical device is charged for the first time, the above first active material is delithiated to obtain a delithiation product of the first active material. During the charging process, the first active material is delithiated to obtain a delithiated product of the first active material. The lithium ions released from the first active material can be consumed to form a film at the negative electrode instead of the lithium ions released from the second active material, and the lithium ions are less embedded after the first delithiation, which is beneficial to reduce the loss of irreversible capacity of the second active material during the first charging, improve the first coulombic efficiency of the second active material, and thus help improve the first coulombic efficiency and cycle performance of the secondary battery. At the same time, with the above characteristics, the positive electrode plate can have a suitable resistivity, and the positive electrode material layer and the positive electrode current collector have a high bonding force, so the safety performance of the electrochemical device can also be improved. Therefore, the first active material whose delithiation product is the above substance is matched with the above second active material and the silicon-containing negative electrode plate, which is beneficial to make the electrochemical device have a high energy density while improving its cycle performance and safety performance. If the value of A / B is too small, for example, less than 29%, the formation of the SEI film will consume the lithium ions in the second active material, so that the active lithium is reduced, resulting in a decrease in the first coulombic efficiency of the electrochemical device and an irreversible capacity loss, and is also not conducive to improving the safety performance of the lithium-ion battery. When the value of A / B is too large, for example, greater than 230%, the first active material and the silicon element are not properly matched. At the same time, too many side reactions occur between the first active material and the negative electrode material layer and the electrolyte, which will have a greater impact on the electrical performance of the electrochemical device. The capacity decays rapidly during the cycle, which is not conducive to improving the cycle performance of the electrochemical device. Therefore, the second active material and the delithiation product are selected as the first active material of the above-mentioned substances, the negative electrode material layer includes the silicon element and regulates its mass percentage content and the value of A / B within the above-mentioned range, so that the electrochemical device can have high energy density, good safety performance and cycle performance at the same time.

[0031] In some embodiments, the process of the first charging process can be: at 45°C, first charge at a constant current of 0.1 times (C) for 10 minutes, then charge at a constant current of 0.5C to a voltage Q (Q ≥ 4.45V), and then charge at a constant voltage to a current less than or equal to 0.05C. For example, Q can be 4.45V, 4.48V, 4.5V, 4.53V, 4.6V, 4.7V, or a range consisting of any two of these values. In an electrochemical device that needs to be formed, the first charging process can be a formation process.

[0032] In this application, if Figure 1 As shown, the positive electrode plate 10 includes a first positive electrode material layer 11, a second positive electrode material layer 12 and a positive electrode current collector 13. The first positive electrode material layer 11 is arranged between the positive electrode current collector 13 and the second positive electrode material layer 12, which can improve the protection of the positive electrode current collector and the interlayer bonding of the positive electrode material layers, reduce the probability of internal short circuit and internal short circuit Joule heat caused by external mechanical damage, and is more conducive to making the electrochemical device have high energy density while having good safety performance.

[0033] In some embodiments of the present application, the delithiation product of the first active material includes LiFeO 2 、CoO 2 、MnO 2 、Ni 0.13 Fe 0.13 Mn 0.54 O 2 、FePO 4 ,FeO 2 , Fe 2 O 3 or at least one of FeO. The delithiation product of the first active material in the first positive electrode material layer includes the above materials, and the lithium ions released from the first active material can be consumed and formed into a film at the negative electrode instead of the lithium ions released from the second active material, and the lithium ions are less embedded after the first delithiation, which is beneficial to reduce the loss of irreversible capacity of the second active material during the first charge, and improve the first coulombic efficiency of the second active material, thereby improving the first coulombic efficiency and cycle performance of the secondary battery. At the same time, the first positive electrode material layer has a suitable resistivity and good bonding performance, which can make the electrochemical device have a high energy density while improving its safety performance and cycle performance.

[0034] In some embodiments of the present application, based on the mass of the first positive electrode material layer, the mass percentage of the delithiation product of the first active material is 30% to 96%, for example, the mass percentage of the delithiation product of the first active material can be 30%, 36%, 40%, 45%, 50%, 55%, 58%, 60%, 62%, 69%, 70%, 75%, 78%, 80%, 85%, 88%, 92%, 96% or a range consisting of any two of the values. The mass percentage of the delithiation product of the first active material is within the above range, which is conducive to giving full play to the lithium supplement effect of the first active material. At the same time, the first positive electrode material layer has a suitable resistivity and good bonding properties, which can make the electrochemical device have a high energy density while improving its safety performance and cycle performance.

[0035] Generally, the mass percentage of the delithiation product of the first active material can be adjusted by changing the mass percentage of the first active material in the first positive electrode material layer during the preparation process. When other conditions remain unchanged, the mass percentage of the first active material increases, and the mass percentage of the delithiation product of the first active material increases; when the mass percentage of the first active material decreases, the mass percentage of the delithiation product of the first active material decreases.

[0036] The present application has no particular limitation on the mass percentage of the first active material in the first positive electrode material layer, and can be adjusted according to the mass percentage of the delithiation product of the first active material actually required, as long as the purpose of the present application can be achieved.

[0037] In some embodiments of the present application, in the positive electrode sheet, the mass of the second active material is C mg / 1540 mm 2 , 0.45%≤A / C≤6%, preferably 0.9%≤A / C≤4.5%; for example, the value of A / C can be 0.45%, 0.5%, 0.8%, 1%, 1.4%, 1.8%, 2%, 2.5%, 2.8%, 3%, 3.4%, 3.8%, 4%, 4.5%, 4.8%, 5%, 5.2%, 5.6%, 6% or a range consisting of any two of the values. When the value of A / C is regulated within the above range, there are fewer side reactions between the first active material and the negative electrode material layer and the electrolyte, which is conducive to making the positive electrode material layer have a higher specific capacity and good cycle stability, so that the electrochemical device has a high energy density while improving its safety performance and cycle performance.

[0038] In some embodiments of the present application, 1 mg / 1540 mm 2 / ≤A≤14mg / 1540mm 2 , 3mg / 1540mm 2 ≤B≤12mg / 1540mm 2, 200mg / 1540mm 2 ≤C≤300mg / 1540mm 2 For example, the value of A can be 1, 3, 5, 6, 8, 10, 12, 13, 14 or a range consisting of any two of these values, and the value of B can be 3 mg / 1540 mm 2 , 4mg / 1540mm 2 、6mg / 1540mm 2 、8mg / 1540mm 2 、9mg / 1540mm 2 、10mg / 1540mm 2 、12mg / 1540mm 2 Or a range consisting of any two values, the value of C can be 200mg / 1540mm 2 , 220mg / 1540mm 2 , 240mg / 1540mm 2 、250mg / 1540mm 2 、280mg / 1540mm 2 、300mg / 1540mm 2 Or a range consisting of any two of the values. Meeting the above characteristics can make the electrochemical device have a high energy density while improving its safety performance and cycle performance.

[0039] In some embodiments of the present application, the negative electrode material layer includes a negative electrode active material, and the negative electrode active material includes at least one of silicon, silicon carbon or silicon oxygen. The above silicon-containing material has a higher gram capacity, and the negative electrode active material includes the above silicon-containing material, which can make the electrochemical device have a higher energy density.

[0040] In some embodiments of the present application, the negative electrode active material further comprises at least one of graphite, hard carbon, soft carbon or mesophase microcarbon beads. The above graphite comprises at least one of artificial graphite or natural graphite. In the present application, based on the mass of the negative electrode material layer, the mass percentage of the above carbon material can be 0.7% to 97.2%.

[0041] In some embodiments, the silicon element in the negative electrode material layer is derived from the above-mentioned silicon-containing materials such as silicon, silicon carbon or silicon oxygen. Based on the mass of the negative electrode material layer, the mass percentage of the silicon-containing material can be 2% to 98.5%. Generally, the mass percentage of the silicon element and the value of B can be adjusted by changing the mass percentage of the above-mentioned silicon-containing material in the negative electrode material layer and the coating weight of the negative electrode material layer. When other conditions remain unchanged, the mass percentage of the silicon-containing material in the negative electrode material layer is increased, and the mass percentage of the silicon element and the value of B increase; when the mass percentage of the silicon-containing material in the negative electrode material layer is reduced, the mass percentage of the silicon element and the value of B decrease. When other conditions remain unchanged, the coating weight of the negative electrode material layer is increased, and the value of B increases; when the coating weight of the negative electrode material layer is reduced, the value of B decreases.

[0042] Generally, the value of A can be adjusted by changing the coating weight of the first positive electrode material layer and the mass percentage of the first active material in the first positive electrode material layer. When other conditions remain unchanged, increasing the coating weight of the first positive electrode material layer increases A, and reducing the coating weight of the first positive electrode material layer decreases A. When other conditions remain unchanged, increasing the mass percentage of the first active material increases A, and reducing the mass percentage of the first active material decreases A.

[0043] Generally, the value of C can be adjusted by changing the coating weight of the second positive electrode material layer and the mass percentage of the second active material in the second positive electrode material layer. When other conditions remain unchanged, increasing the coating weight of the second positive electrode material layer increases C, and reducing the coating weight of the second positive electrode material layer decreases C. When other conditions remain unchanged, increasing the mass percentage of the second active material increases C, and reducing the mass percentage of the second active material decreases C.

[0044] In the present application, there is no particular restriction on the coating weight of the first positive electrode material layer and the coating weight of the second positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the coating weight of the first positive electrode material layer can be 3 mg / 1540 mm 2 Up to 20mg / 1540mm 2 The coating weight of the second positive electrode material layer can be 200 mg / 1540 mm 2 Up to 300mg / 1540mm 2 .

[0045] In some embodiments of the present application, the first positive electrode material layer further includes an inorganic material, and the inorganic material includes at least one of aluminum oxide, lithium lanthanum zirconium oxide, lithium lanthanum titanate, lithium aluminum titanium phosphate, antimony-doped tin oxide or titanium oxide; based on the mass of the first positive electrode material layer, the mass percentage of the inorganic material is 0.2% to 60%, preferably 5% to 60%. For example, the mass percentage of the inorganic material can be 0.2%, 2%, 3%, 5%, 8%, 10%, 12.2%, 14.2%, 17%, 20%, 23%, 26%, 30%, 33%, 35%, 37%, 40%, 43%, 45%, 47%, 50%, 60% or a range consisting of any two of the values. The first positive electrode material layer includes the above-mentioned inorganic material, and its mass percentage is adjusted within the above-mentioned range, which can improve the stability of the positive electrode material layer, so that the first positive electrode material layer has good bonding properties and suitable resistivity, reduces the probability of internal short circuit and the heat generated by the internal short circuit, thereby helping to further improve the safety performance of the electrochemical device.

[0046] In some embodiments of the present application, the specific capacity of the first positive electrode material layer is 130mAh / g to 780mAh / g. For example, the specific capacity of the first positive electrode material layer can be 130mAh / g, 150mAh / g, 160mAh / g, 180mAh / g, 200mAh / g, 250mAh / g, 300mAh / g, 350mAh / g, 400mAh / g, 500mAh / g, 600mAh / g, 700mAh / g, 780mAh / g or a range composed of any two values. Since the first active material has a higher specific capacity, the specific capacity of the first positive electrode material layer can be within the above range, so that when the electrochemical device is charged for the first time, the loss of active lithium caused by the formation of the SEI film can be improved, the irreversible capacity loss of the electrochemical device and the reduction of the first coulombic efficiency can be reduced, so that the electrochemical device has a high energy density while further improving its cycle performance and safety performance. In some embodiments of the present application, it is preferred that the specific capacity of the first positive electrode material layer is greater than or equal to the specific capacity of the second positive electrode material layer. While the specific capacity of the first positive electrode material layer is within the scope of the present application, the specific capacities of the first positive electrode material layer and the second positive electrode material layer satisfy the above relationship, which is more conducive to reducing the active lithium loss of the second positive electrode material layer during the first charge and discharge, exerting the lithium replenishing effect of the first active material, reducing the irreversible capacity loss of the electrochemical device and the reduction of the first coulombic efficiency, thereby making the electrochemical device have a high energy density while further improving its cycle performance.

[0047] In some embodiments, the specific capacity of the second positive electrode material layer can be 130mAh / g to 280mAh / g, for example, the specific capacity of the second positive electrode material layer can be 130mAh / g, 150mAh / g, 170mAh / g, 186mAh / g, 192mAh / g, 200mAh / g, 220mAh / g, 245mAh / g, 260mAh / g, 280mAh / g or a range consisting of any two of the values. The specific capacity of the second positive electrode material layer is within the above range, which can make the electrochemical device have a higher energy density.

[0048] Generally, the specific capacity of the first positive electrode material layer can be adjusted by adjusting the type and mass percentage of the active material in the first positive electrode material layer. If other conditions remain unchanged, the specific capacity of the first positive electrode material layer increases by using a first positive electrode material with a high specific capacity or increasing the mass percentage of the active material in the first positive electrode material layer, and the specific capacity of the first positive electrode material layer decreases by using a first positive electrode material with a low specific capacity or reducing the mass percentage of the active material in the first positive electrode material layer. The specific capacity of the second positive electrode material layer can be adjusted by adjusting the type and mass percentage of the active material in the second positive electrode material layer. If other conditions remain unchanged, the specific capacity of the second positive electrode material layer increases by using a second positive electrode material with a high specific capacity or increasing the mass percentage of the active material in the first positive electrode material layer, and the specific capacity of the second positive electrode material layer decreases by using a second positive electrode material with a low specific capacity or reducing the mass percentage of the active material in the second positive electrode material layer.

[0049] In some embodiments of the present application, the first active material includes at least one of the following compounds: Li 5 QO 4 or Li 5 QO 6 , Q includes at least one of Ni, Co, Fe, Sn or Mn, and the valence state of the Q element is lower than its own highest oxidation valence state; Li q Fe 0.5(1+q) PO 4 , 1≤q≤5; Li 2-a-b-c-d Ni a R b Mn c M d O 2-f , 0≤a<0.35, 0<b<0.5, 0.3<c≤0.6, 0≤d<0.05, 0.7<a+b+c+d<0.9, 0≤f<0.2, R includes at least one of Fe or Co, M includes at least one of Mg, Al, Ti, V, Cr, Cu, Y, Zr, Nb, Mo, La or W; Li 1+e Mn 1-p X p O 2-sY s , -0.1<e<0.2, 0≤p<0.2, 0≤s<0.2, X includes at least one of Fe, Co, Ni, Ti, Zn, Mg, Al, V, Cr or Zr, and Y includes at least one of S, N, F, Cl or Br. The first active material within the above range has a higher specific capacity and a lower first coulombic efficiency, which is beneficial to reduce the loss of the first coulombic efficiency and the irreversible capacity. The above first active material has good stability, which can make the electrochemical device have good cycle performance. At the same time, the positive electrode sheet has a suitable resistivity, the positive electrode material layer and the positive electrode current collector have a high bonding force, and the safety performance of the electrochemical device can also be improved. Therefore, the selection of the above materials can make the electrochemical device have high energy density, good safety performance and cycle performance.

[0050] In some embodiments of the present application, the first active material includes Li 5 FeO 4 , Li 5 CoO 4 , Li 2 MnO 2 , Li 1.2 Ni 0.13 Fe 0.13 Mn 0.54 O 2 or LiFePO 4 The selection of the first active material is more conducive to the lithium supplementation effect of the first active material, so that the electrochemical device has a high energy density and further improves its safety performance and cycle performance.

[0051] In some embodiments of the present application, the resistivity of the positive electrode material layer is ρΩ·m, 44≤ρ≤155. For example, the value of ρ can be 44, 50, 58, 65, 72, 84, 95, 100, 114, 130, 135, 148, 150, 155, or a range consisting of any two of the values. By regulating the resistivity of the positive electrode material layer within the above range, the positive electrode material layer can have a suitable impedance, reduce the probability of internal short circuit of the electrochemical device, and reduce the heat generated during the internal short circuit, thereby helping to further improve the safety performance of the electrochemical device.

[0052] The present application has no particular restrictions on the resistivity of the first positive electrode material layer and the second positive electrode material layer, as long as the sum of the two is within the above range. For example, the resistivity of the first positive electrode material layer can be 40Ω·m to 130Ω·m, and the resistivity of the second positive electrode material layer can be 2Ω·m to 50Ω·m.

[0053] In some embodiments, the first cathode material layer of the present application may further include a conductive agent, and the present application has no particular restrictions on the conductive agent, for example, it may include but is not limited to at least one of conductive carbon black or carbon nanotubes. The present application has no particular restrictions on its mass percentage, and those skilled in the art may select it according to actual needs, as long as the purpose of the present application can be achieved. For example, based on the mass of the first cathode material layer, the mass percentage of the conductive agent may be 0% to 5%.

[0054] In the present application, the first positive electrode material layer may further include a binder. The present application does not particularly limit the type of the binder, as long as the purpose of the present application can be achieved. The present application does not particularly limit the mass percentage of the binder, as long as the purpose of the present application can be achieved. For example, based on the mass of the first positive electrode material layer, the mass percentage of the binder may be 3% to 15%.

[0055] In some embodiments, the first positive electrode material layer includes a delithiation product of the first active material and a binder, in other embodiments, the first positive electrode material layer includes a delithiation product of the first active material, an inorganic material, and a binder. In still other embodiments, the first positive electrode material layer includes a delithiation product of the first active material, an inorganic material, a binder, and a conductive agent.

[0056] In the present application, the second positive electrode material layer may also include a conductive agent and a binder, and the present application has no particular restrictions on their types, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the mass percentage of the second active material, the conductive agent, and the binder in the second positive electrode material layer, as long as the purpose of the present application can be achieved. For example, based on the mass of the second positive electrode material layer, the mass percentage of the second active material can be 90% to 99%, the mass percentage of the conductive agent can be 0.2% to 5%, and the mass percentage of the binder can be 0.2% to 5%.

[0057] The above-mentioned binder may include but is not limited to at least one of polyacrylic acid, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyvinyl alcohol, carboxymethyl cellulose, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, polyamide-imide, styrene-butadiene rubber or polyvinylidene fluoride. The above-mentioned conductive agent may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metal materials or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers, and specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymer may include but is not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole.

[0058] In the present application, the positive electrode material layer is disposed on at least one surface of the positive electrode current collector, that is, the positive electrode material layer can be disposed on one surface in the thickness direction of the positive electrode current collector, or on two surfaces in the thickness direction of the positive electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the surface of the positive electrode current collector, or it can be a partial area of ​​the surface of the positive electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved.

[0059] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector), etc. The present application has no particular restrictions on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm. The present application has no particular restrictions on the thickness of the first positive electrode material layer and the second positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the first positive electrode material layer is 2μm to 5μm, and the thickness of the second positive electrode material layer is 30μm to 120μm.

[0060] In the present application, there is no particular restriction on the preparation method of the positive electrode sheet, as long as the purpose of the present application can be achieved. In some embodiments, the positive electrode sheet can be prepared by the following method: the first positive electrode material layer slurry is evenly coated on one surface of the positive electrode current collector and dried, and then the second positive electrode material layer slurry is evenly coated on the surface of the first positive electrode material layer, and the positive electrode sheet coated with the positive electrode material layer on one side is obtained after drying. Repeat the above coating steps on the other surface of the positive electrode current collector, and obtain the positive electrode sheet coated with the positive electrode material layer on both sides after drying. After coating, the positive electrode sheet is obtained by cold pressing and cutting.

[0061] The first positive electrode material layer slurry can be prepared by the following steps: mixing the first active material and the binder, optionally adding an inorganic material or an inorganic material and a conductive agent, adding N-methylpyrrolidone (NMP) and stirring evenly to obtain a first positive electrode material layer slurry with a solid content of 40wt% to 85wt%. The second positive electrode material layer slurry can be prepared by the following steps: mixing the second active material, the binder and the conductive agent, adding N-methylpyrrolidone (NMP) and stirring evenly to obtain a second positive electrode material layer slurry with a solid content of 65wt% to 85wt%.

[0062] The negative electrode sheet of the present application also includes a negative electrode current collector, and the negative electrode material layer is arranged on at least one surface of the negative electrode current collector. In the present application, the negative electrode material layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector, or it can be a partial area of ​​the negative electrode current collector. There is no special limitation in the present application, as long as the purpose of the present application can be achieved. In the present application, there is no special limitation on the thickness of the negative electrode current collector and the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 12μm, and the thickness of the single-sided negative electrode material layer is 30μm to 160μm.

[0063] The negative electrode material layer of the present application may also include a conductive agent, a binder and a thickener. The present application has no particular restrictions on the conductive agent and the binder, as long as the purpose of the present application can be achieved, for example, it may be at least one of the above conductive agent and the above binder. The thickener may include at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose or carboxymethyl cellulose. Based on the mass of the negative electrode material layer, the mass percentage of the conductive agent may be 0.5% to 5%, the mass percentage of the binder may be 0.2% to 2%, and the mass percentage of the thickener may be 0.1% to 2%.

[0064] In the present application, there is no particular restriction on the preparation method of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, it can be prepared by the following method: negative electrode active material, conductive agent, binder, thickener are mixed, deionized water is added and stirred evenly, and a negative electrode slurry with a solid content of 40wt% to 75wt% is obtained. The negative electrode slurry is evenly coated on one surface of the negative electrode collector, and a negative electrode sheet coated with a negative electrode material layer on one side is obtained after drying. Then the above coating steps are repeated on the other surface of the negative electrode collector, and a negative electrode sheet coated with a negative electrode material layer on both sides is obtained after drying. After coating, the negative electrode sheet is obtained by cold pressing and cutting.

[0065] The secondary battery of the present application also includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include LiPF 6 、LiNO3 , LiBF 4 、LiClO 4 、LiB(C 6 H 5 ) 4 、LiCH 3 SO 3 、LiCF 3 SO 3 、LiN(SO 2 CF 3 ) 2 、LiC(SO 2 CF 3 ) 3 , Li 2 SiF 6 , lithium bis(oxalatoborate) (LiBOB), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or lithium difluoroborate. The non-aqueous solvent may include but is not limited to at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The carbonate compound may include but is not limited to at least one of a chain carbonate compound or a cyclic carbonate compound. The chain carbonate compound may include but is not limited to at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or methyl ethyl carbonate. The cyclic carbonate may include but is not limited to at least one of ethylene carbonate, propylene carbonate (PC), butylene carbonate or vinyl ethylene carbonate. The carboxylate compound may include but is not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,3-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate. The present application does not limit the mass percentage of lithium salt and non-aqueous solvent, as long as the purpose of the present application can be achieved.

[0066] The electrochemical device of the present application also includes an isolating membrane. The present application has no particular restrictions on the isolating membrane, as long as the purpose of the present application can be achieved. For example, the material of the isolating membrane may include, but is not limited to, polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or at least one of aramid. The type of isolating membrane may include at least one of a woven membrane, a non-woven membrane, a microporous membrane, a composite membrane, a rolled membrane or a spinning membrane. In some embodiments, the isolating membrane may include a substrate layer and a surface treatment layer. The substrate layer may be a non-woven fabric, a film or a composite membrane having a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. In some embodiments, the inorganic layer includes inorganic particles and a binder. The present application has no particular restrictions on inorganic particles, such as inorganic particles can include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application has no particular restrictions on binders, such as binders can be at least one of the above-mentioned binders. In some embodiments of the present application, the polymer layer includes a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinyl pyrrolidone, polyvinyl ether or polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene). In the present application, there is no particular limitation on the thickness of the isolation film, as long as the purpose of the present application can be achieved. For example, the thickness of the isolation film may be 3 μm to 30 μm.

[0067] The electrochemical device also includes a housing for accommodating a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, as well as other components known in the field of electrochemical devices, and this application does not limit the above-mentioned other components. This application does not particularly limit the housing, and it can be a housing known in the art, as long as the purpose of this application can be achieved. For example, the housing can be a hard shell housing or a flexible shell. The material of the hard shell housing can be metal, and this application does not limit the type of metal, and a metal hard shell housing known in the art can be used, as long as the purpose of this application can be achieved. The flexible housing can be a metal plastic film, such as an aluminum plastic film, a steel plastic film, etc.

[0068] The present application does not particularly limit the type of electrochemical device, which may include any device that generates an electrochemical reaction. For example, the electrochemical device may include, but is not limited to, a lithium-ion battery, a sodium-ion battery, a lithium polymer secondary battery, and a lithium-ion polymer secondary battery.

[0069] The preparation process of the electrochemical device of the present application is well known to those skilled in the art, and the present application has no particular limitations. For example, the preparation process of the electrochemical device may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly with a wound structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain an electrochemical device. Alternatively, stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly with a stacked structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain an electrochemical device. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent pressure rise and overcharge and discharge inside the electrochemical device.

[0070] The second aspect of the present application provides an electronic device, which includes the electrochemical device provided in the first aspect of the present application. The electrochemical device provided in the first aspect of the present application has high energy density, good safety performance and cycle performance, so that the electronic device of the present application has good performance and a long service life.

[0071] The present application does not particularly limit the type of electronic device, which can be any electronic device known in the prior art. In some embodiments, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0072] Example

[0073] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0074] Test methods and equipment:

[0075] Sampling method for positive and negative electrodes:

[0076] Disassembly process in full discharge state: The lithium-ion batteries prepared in each embodiment and comparative example are charged at a constant current of 0.2C to the voltage upper limit setting value, reaching the full charge state, and the positive electrode sheet and the negative electrode sheet are taken out after disassembly, and the positive electrode sheet and the negative electrode sheet are cleaned with dimethyl carbonate, and then dried at 60°C to obtain the positive electrode sheet sample and the negative electrode sheet sample. The above voltage upper limit setting value is determined by the type of the second active material. When the second active material is lithium cobalt oxide, the above voltage upper limit setting value is 4.53V; when the second active material is lithium nickel cobalt manganese oxide, the above voltage upper limit setting value is 4.25V; when the second active material is lithium iron phosphate, the above voltage upper limit setting value is 4.3V; when the second active material is lithium nickel cobalt aluminum oxide, the above voltage upper limit setting value is 4.2V; when the second active material is lithium manganese oxide, the above voltage upper limit setting value is 4.3V.

[0077] Disassembly process in full discharge state: The lithium-ion batteries prepared in each embodiment and comparative example are discharged at a constant current of 0.2C to the voltage lower limit setting value to reach the full discharge state. After disassembly, the positive electrode sheet and the negative electrode sheet are taken out, and the positive electrode sheet and the negative electrode sheet are cleaned with dimethyl carbonate, and then dried at 60°C to obtain the positive electrode sheet sample and the negative electrode sheet sample. The above voltage lower limit setting value is determined by the type of the second active material. When the second active material is lithium cobalt oxide, the above voltage lower limit setting value is 3V; when the second active material is lithium nickel cobalt manganese oxide, the above voltage lower limit setting value is 3.2V; when the second active material is lithium iron phosphate, the above voltage lower limit setting value is 2.4V; when the second active material is lithium nickel cobalt aluminum oxide, the above voltage lower limit setting value is 2.8V; when the second active material is lithium manganese oxide, the above voltage lower limit setting value is 2.4V.

[0078] Determination of the delithiation product of the first active material:

[0079] A lithium-ion battery in a fully discharged state is disassembled to obtain a positive electrode sheet sample, the positive electrode material layer is scraped off the surface of the positive electrode current collector, the powder on the first positive electrode material layer originally close to the positive electrode current collector is scraped off, and the powder is placed in a muffle furnace and sintered at 500°C for 6 hours. The calcined powder sample is collected and then subjected to the following elemental analysis, using X-ray diffraction (XRD) test and Raman test to obtain the composition structure information of the delithiation product of the first active material, thereby inferring its chemical formula and calculating its mass percentage.

[0080] Elemental analysis: Take 0.4g of the above powder sample and digest it with 10mL of aqua regia, which is obtained by mixing concentrated nitric acid and concentrated hydrochloric acid in a volume ratio of 1:1. Then make the volume to 100mL, and use an inductively coupled plasma spectrometer (ICP) to measure the content of each element in the solution.

[0081] XRD analysis: XRD test was performed on the powder sample using an X-ray diffractometer (Bruker D8 ADVANCE) to obtain an XRD spectrum of the first cathode material layer. The XRD spectrum was analyzed and compared with the standard spectrum based on the position, intensity and shape of the diffraction peaks to obtain the phase composition of the delithiation product of the first active material. Cu Kα rays were used.

[0082] Raman spectroscopy analysis: Raman testing was performed on the powder samples using a Raman spectrometer (LabRAM HR Evolution) to obtain the Raman spectrum of the first cathode material layer. By comparing its characteristic peaks with the standard spectrum, the material metal bond structure information of the delithiation product of the first active material can be obtained.

[0083] Test of mass percentage of silicon element (Y):

[0084] Take a lithium-ion battery in a fully discharged state and disassemble it to obtain a negative electrode sheet sample, scrape off the negative electrode material layer powder on the surface of the negative electrode current collector, take 1 g of the above powder sample, and then use ICP to measure the mass percentage of silicon element in the negative electrode material layer.

[0085] Test of the mass (A) of the delithiation product of the first active material in the positive electrode sheet:

[0086] Take a lithium-ion battery in a fully charged state and disassemble it to obtain a positive electrode sheet sample. Scrape the positive electrode material layer from the surface of the positive electrode current collector. Scrape the powder of the first positive electrode material layer in the positive electrode sheet sample on the side originally close to the positive electrode current collector (i.e., parallel to the thickness direction of the current collector, within the range of 0 to 2 μm from the surface of the positive electrode current collector). Weigh its mass as M 1 mg, and the area of ​​the positive electrode current collector is S 1 mm 2 Then, a thermogravimetric analyzer is used to measure the mass percentage of the delithiation product of the first active material, w 1 , then the mass of the delithiation product of the first active material in the positive electrode sheet = M 1 × 1 ×1540 / S 1 , the unit is mg / 1540mm 2 .

[0087] Quality test of silicon element in negative electrode (B):

[0088] Take a lithium-ion battery in a fully discharged state and disassemble it to obtain a negative electrode sheet sample. Scrape off the negative electrode material layer powder on the surface of the negative electrode current collector of the above sample and weigh its mass as M. 2 mg, and the area of ​​the current collector of the negative electrode sample tested is S 2 mm 2Then, ICP was used to measure the mass percentage of silicon in the negative electrode material layer. 2 , then the mass of silicon in the negative electrode = M 2 × 2 ×1540 / S 2 , unit is mg / 1540mm 2 .

[0089] Quality test of the second active material in the positive electrode sheet (C):

[0090] Take a lithium-ion battery in a fully discharged state and disassemble it to obtain a positive electrode sheet sample. Scrape the positive electrode material layer from the surface of the positive current collector. Scrape the powder of the second positive electrode material layer in the positive electrode sheet sample from the side originally far away from the positive current collector (i.e., parallel to the thickness direction of the current collector, within the range of 0 to 20 μm from the surface of the positive electrode sheet). Weigh its mass as M 3 mg, and the area of ​​the positive electrode current collector is S 3 mm 2 Then the mass percentage of the second active material w is measured using a thermogravimetric analyzer. 3 , then the mass of the second active material in the positive electrode sheet = M 3 × 3 ×1540 / S 3 , the unit is mg / 1540mm 2 .

[0091] Specific capacity (θ1) test of the first positive electrode material layer:

[0092] The first positive electrode material layer slurry is prepared according to the slurry ratio in each embodiment and comparative example, and the slurry of the first positive electrode material layer is coated on the positive electrode collector, and the positive electrode sheet of the first positive electrode material layer with a single-side thickness of 12.6μm is obtained after drying and cold pressing. During the preparation process, the mass of the positive electrode collector and the mass of the positive electrode sheet are weighed, and the mass of the positive electrode collector per unit area and the mass of the positive electrode sheet per unit area are calculated, and the mass of the first positive electrode material layer per unit area is calculated to be M4. The above-mentioned positive electrode sheet, separator, and lithium sheet are stacked in sequence, and the electrolyte is injected to obtain a button battery. The above-mentioned positive electrode collector, separator and electrolyte are the same as those in Example 1.

[0093] The button cell was charged at a constant current of 0.05C to 4.58V, and the first charge capacity was recorded. The specific capacity of the first positive electrode material layer θ1 = first charge capacity / M4, in units of mAh / g.

[0094] Specific capacity (θ2) test of the second positive electrode material layer:

[0095] The second positive electrode material layer slurry is prepared according to the slurry ratio in each embodiment and comparative example, and the slurry of the second positive electrode material layer is coated on the positive electrode collector. After drying and cold pressing, a positive electrode sheet of the second positive electrode material layer with a single-side thickness of 53.6 μm is obtained. During the preparation process of the button battery, the mass of the positive electrode collector and the mass of the positive electrode sheet are weighed, and the mass of the positive electrode collector per unit area and the mass of the positive electrode sheet per unit area are calculated. The mass of the second positive electrode material layer per unit area is calculated to be M5. The above-mentioned positive electrode sheet, separator, and lithium sheet are stacked in sequence, and the electrolyte is injected to obtain a button battery. The above-mentioned positive electrode collector, separator and electrolyte are the same as those in Example 1.

[0096] The button cell was charged at a constant current of 0.05C to 4.58V, and the first charge capacity was recorded. The specific capacity of the second positive electrode material layer θ2 = first charge capacity / M5, in units of mAh / g.

[0097] Adhesion (F) test:

[0098] Take the lithium-ion battery in a fully discharged state and disassemble it to obtain the positive electrode sheet, and scrape off the positive electrode material on one surface of the positive current collector. Then cut a positive electrode sheet sample with a width of 20mm and a length of 160mm. Use a double-sided tape with a width of 20mm and a length of 150mm to paste the positive electrode sheet sample on a steel plate with a width of 20mm and a length of 300mm. The positive current collector is pasted to the steel plate, and a paper tape with the same width and a length of 200mm as the positive electrode sheet is connected and fixed to a section of the sample strip, and tested using a high-speed rail AI-3000 tensile testing machine. Fix the test sample on the test bench, fold the paper tape 180° upward, and fix it with a clamp. Then the tensile machine starts to pull the paper tape at a speed of 50mm / min, and the tensile displacement is 50mm. Take the tensile force value when the curve is flat and the displacement is greater than 10mm to calculate the bonding force F between the first positive electrode material layer and the positive current collector, unit: N / m.

[0099] Resistivity (ρ) test method:

[0100] Take a lithium-ion battery in a fully charged state and disassemble it to obtain a positive electrode sheet sample, test the total thickness of the positive electrode sheet, and then test the resistance R of the positive electrode sheet through a film resistor, where the test probe area of ​​the film resistor is S. Then scrape off the positive electrode material layer, test the thickness of the positive electrode current collector, and calculate the thickness h of the positive electrode material layer. In this application, the resistance of the positive electrode current collector is negligible, and the resistance R of the positive electrode sheet tested by the film resistor can represent the resistance of the positive electrode material layer. Then the resistivity of the positive electrode material layer ρ = R × S / h, the unit is Ω·m.

[0101] Cycle performance test:

[0102] At 25°C, charge the lithium-ion battery at a constant current of 3C to 4.53V, then charge at a constant voltage until the current is less than or equal to 0.05C, and then discharge at a constant current of 0.5C to 3V. This is a charge and discharge cycle, and record the discharge capacity of the first cycle of the lithium-ion battery. Perform charge and discharge cycles on the lithium-ion battery according to the above method, and record the discharge capacity of each cycle until the discharge capacity of the lithium-ion battery decays to 80% of the discharge capacity of the first cycle, and record the number of charge and discharge cycles.

[0103] Safety performance test:

[0104] Place the lithium-ion battery in a 25°C thermostat and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge the lithium-ion battery that has reached a constant temperature at a constant current of 0.5C to a voltage of 4.53V, and then charge it at a constant voltage of 4.53V to a current of 0.025C to obtain a fully charged lithium-ion battery. Transfer the fully charged lithium-ion battery to a nail penetration tester, maintain the test environment temperature at 25°C±2°C, use a steel nail with a diameter of 4mm, and uniformly penetrate the center of the lithium-ion battery at a speed of 30mm / s, retain it for 300s, and the lithium-ion battery will pass if it does not catch fire or explode. 10 lithium-ion batteries are tested for each embodiment or comparative example, and the pass rate of the nail penetration test (N / 10) is used as an indicator for evaluating the safety performance of the lithium-ion battery, and N is the number of lithium-ion batteries that pass the nail penetration test.

[0105] Volume energy density test:

[0106] Place the lithium-ion battery in a 25°C thermostat for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge the lithium-ion battery at a constant current of 0.5C to a voltage of 4.53V, then charge it at a constant voltage of 4.53V to a current of 0.05C, and then discharge it at 0.5C to a voltage of 3.0V. Record the discharge energy (unit: Wh). The volume energy density VED = discharge energy / (lithium-ion battery length × width × thickness), unit: Wh / L. Among them, length, width, and thickness all refer to the length, width, and thickness of the lithium-ion battery after packaging.

[0107] Example 1

[0108] <Preparation of positive electrode sheet>

[0109] The first active material Li 5 FeO 4 , a binder polyvinylidene fluoride (PVDF) was mixed in a mass ratio of 97:3, and N-methylpyrrolidone (NMP) was added as a solvent, and after stirring evenly, a first positive electrode material layer slurry with a solid content of 45 wt % was prepared.

[0110] The second active material is lithium cobalt oxide (LiCoO 2) Conductive carbon black, carbon nanotubes, and binder polyvinylidene fluoride are mixed in a mass ratio of 97.4:0.5:0.5:1.4, NMP is added as a solvent, and after stirring evenly, a second positive electrode material layer slurry with a solid content of 75wt% is prepared.

[0111] The prepared first positive electrode material layer slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10 μm, and dried to obtain a positive electrode sheet coated with the first positive electrode material layer on one side, and then the second positive electrode material layer slurry is evenly coated on the surface of the first positive electrode material layer, and dried to obtain a positive electrode sheet coated with the first positive electrode material layer and the second positive electrode material layer on one side, and then the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet coated with positive electrode material layers on both sides, and vacuum dried at 120°C for 6 hours, and then cold pressed, cut to pieces, and welded to the ears to obtain a positive electrode sheet with a specification of 74mm×867mm for standby use. Among them, the thickness of the single-sided first positive electrode material layer is 2.6μm, and the coating weight of the first positive electrode material layer is 5mg / 1540mm 2 The thickness of the second positive electrode material layer on one side is 43.6 μm, and the coating weight of the second positive electrode material layer is 230 mg / 1540 mm 2 .

[0112] <Preparation of negative electrode sheet>

[0113] The negative electrode active material silicon carbon and artificial graphite, the binder polyacrylic acid, the thickener sodium carboxymethyl cellulose, and the conductive agent conductive carbon black are mixed in a mass ratio of 20:77.5:1.5:0.5:0.5, and deionized water is added as a solvent to prepare a slurry with a solid content of 45wt%. The negative electrode slurry is obtained after being stirred evenly by a vacuum mixer. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 120°C to obtain a negative electrode sheet with a single-sided coating of a negative electrode material layer. The coating weight of the negative electrode material layer is 105mg / 1540mm 2 Then repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet with a negative electrode material layer coated on both sides. Dry at 120°C for 6 hours, then cold press, cut and weld the tabs to obtain a negative electrode sheet with a specification of 78mm×875mm for standby use. The thickness of the single-sided negative electrode material layer is 35.5μm.

[0114] <Preparation of Separator Film>

[0115] A polyethylene film with a thickness of 16 μm (provided by Celgard Company) was used as the isolation film.

[0116] <Preparation of Electrolyte>

[0117] In an environment where the water content is less than 10 ppm, ethylene carbonate and propylene carbonate are mixed in a mass ratio of 50:50 to obtain a non-aqueous solvent, and then lithium salt LiPF is added to the non-aqueous solvent. 6 , and mixed evenly to obtain an electrolyte, wherein the concentration of the lithium salt is 1.15 mol / L.

[0118] <Preparation of lithium-ion batteries>

[0119] The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain the electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, placed in an 85°C vacuum oven to dry for 12 hours to remove moisture, and the above-prepared electrolyte is injected. After vacuum packaging, standing, formation, degassing, trimming and other processes, a lithium-ion battery is obtained. The formation process is: at 45°C, the lithium-ion battery is charged at a constant current rate of 0.1C for 10 minutes, then charged at a constant current rate of 0.5C to 4.53V, and then charged at a constant voltage to a current of 0.05C.

[0120] Example 2 to Example 9

[0121] Except for adjusting the relevant parameters as shown in Table 1, the rest is the same as Example 1. Among them, the coating weight of the first positive electrode material layer can be adjusted so that A is as shown in Table 1, and the coating weight of the negative electrode material layer can be adjusted so that B is as shown in Table 1.

[0122] Example 10 to Example 14

[0123] Except that inorganic materials are further introduced into the first positive electrode material layer, and relevant parameters are adjusted as shown in Table 1, the rest is the same as Example 1. Among them, the mass percentage of the delithiation product of the first active material is adjusted by regulating the mass percentage of the first active material. When the mass percentage of the first active material and / or the inorganic material changes, the mass percentage of the binder changes accordingly, and the sum of the mass percentages of the three is 100%.

[0124] Example 15 to Example 17

[0125] Except for adjusting the mass percentage of silicon carbon so that the mass percentage of silicon element and the value of B are as shown in Table 1, the rest is the same as Example 12. Among them, when the mass percentage of silicon carbon changes, the mass percentage of artificial graphite changes accordingly, and the mass percentages of the binder, thickener and conductive agent remain unchanged.

[0126] Example 18 to Example 27

[0127] Except for adjusting the relevant parameters as shown in Table 1, the rest is the same as Example 10. Among them, the mass percentage of the delithiation product of the first active material is adjusted by regulating the mass percentage of the first active material. When the mass percentage of the first active material and / or the inorganic material changes, the mass percentage of the binder changes accordingly, and the sum of the mass percentages of the three is 100%.

[0128] Comparative Example 1

[0129] Except for preparing the positive electrode sheet by the following <Preparation of positive electrode sheet>, the rest is the same as Example 1.

[0130] <Preparation of positive electrode sheet>

[0131] The second positive electrode material layer slurry was prepared by the process of Example 1.

[0132] The prepared second positive electrode material layer slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10 μm, and dried to obtain a positive electrode sheet coated with the second positive electrode material layer on one side, and then the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet coated with the second positive electrode material layer on both sides, and vacuum dried at 120°C for 6 hours, and then cold pressed, cut, and welded to obtain a positive electrode sheet with a specification of 74mm×867mm for standby use. Among them, the thickness of the single-sided second positive electrode material layer is 46.2μm, and the coating weight of the second positive electrode material layer is 235mg / 1540mm 2 .

[0133] Comparative Example 2

[0134] Except for preparing the positive electrode sheet by the following <Preparation of positive electrode sheet>, the rest is the same as Example 1.

[0135] The second positive electrode material layer slurry was prepared by the process of Example 1.

[0136] The inorganic material Al 2 O 3 , a binder polyvinylidene fluoride (PVDF) was mixed in a mass ratio of 95:5, and N-methylpyrrolidone (NMP) was added as a solvent, and after stirring evenly, a first positive electrode material layer slurry with a solid content of 45 wt % was prepared.

[0137] The prepared first positive electrode material layer slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10 μm, and dried to obtain a positive electrode sheet coated with the first positive electrode material layer on one side, and then the second positive electrode material layer slurry is evenly coated on the surface of the first positive electrode material layer, and dried to obtain a positive electrode sheet coated with the first positive electrode material layer and the second positive electrode material layer on one side, and then the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet coated with positive electrode material layers on both sides, and vacuum dried at 120°C for 6 hours, and then cold pressed, cut to pieces, and welded to the ears to obtain a positive electrode sheet with a specification of 74mm×867mm for standby use. Among them, the thickness of the single-sided first positive electrode material layer is 2.6μm, and the coating weight of the first positive electrode material layer is 5mg / 1540mm 2 The thickness of the second positive electrode material layer on one side is 43.6 μm, and the coating weight of the second positive electrode material layer is 230 mg / 1540 mm 2 .

[0138] Comparative Example 3

[0139] Except for preparing the first positive electrode material layer slurry by the following steps, the rest is the same as that of Comparative Example 2.

[0140] The inorganic material Al 2 O 3 Conductive carbon black (SP), a conductive agent, and polyvinylidene fluoride (PVDF) as a binder are mixed in a mass ratio of 93:2:5, and N-methylpyrrolidone (NMP) is added as a solvent. After stirring evenly, the mixture is prepared into a first positive electrode material layer slurry with a solid content of 45 wt%.

[0141] Comparative Examples 4 to 7

[0142] Except for adjusting the relevant parameters as shown in Table 1, the rest is the same as Example 10.

[0143] The relevant parameters and performances of each embodiment and each comparative example are shown in Table 1.

[0144]

[0145]

[0146] It can be seen from Examples 1 to 27 and Comparative Examples 1 to 7 that by using the positive electrode sheet and the negative electrode sheet within the scope of the present application, and adjusting the mass percentage of silicon elements and the value of A / B within the scope of the present application, the positive electrode material layer can have a suitable resistivity, the first positive electrode material layer and the current collector have a higher bonding force, and the lithium-ion battery has a higher volume energy density, nail penetration rate and more cycles, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance. In Comparative Example 1, the first positive electrode material layer is not provided, and the composition of the first positive electrode material layer of Comparative Examples 2 and 3 is not within the scope of the present application. In Comparative Examples 4 to 7, at least one of the values ​​of A / B or the mass percentage of silicon elements is not within the scope of the present application. The lithium-ion batteries of Comparative Examples 1, 3 to 7 cannot take into account the higher volume energy density, nail penetration rate and more cycles, which indicates that their comprehensive performance is poor. Since the resistivity of the first positive electrode material layer of Comparative Example 2 is too large, the lithium-ion battery cannot work, and no relevant performance data is measured.

[0147] The types of the first active material and the delithiation product of the first active material usually affect the energy density, safety performance and cycle performance of the lithium-ion battery. It can be seen from Examples 1 to 9 that the first active material within the scope of the present application is selected, and its delithiation product is as shown in Table 1, which can make the lithium-ion battery have a higher volume energy density, nail penetration rate and more cycles at the same time, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance at the same time.

[0148] The values ​​of A / B and A / C usually affect the energy density, safety performance and cycle performance of lithium-ion batteries. It can be seen from Examples 10 to 14 that by adjusting the values ​​of A / B and A / C within the scope of this application, the lithium-ion battery can have a higher volume energy density, nail penetration rate and more cycles, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance.

[0149] The mass percentage of silicon usually affects the energy density, safety performance and cycle performance of lithium-ion batteries. It can be seen from Examples 10, 15 to 17 that by adjusting the mass percentage of silicon within the scope of this application, the lithium-ion battery can have a higher volume energy density, nail penetration rate and more cycles, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance.

[0150] The mass percentage of the delithiation product of the first active material usually affects the energy density, safety performance and cycle performance of the lithium-ion battery. It can be seen from Example 1, Example 12 and Example 18 that by regulating the mass percentage of the delithiation product of the first active material within the scope of this application, the lithium-ion battery can have a higher volume energy density, nail penetration rate and more cycles, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance.

[0151] The mass percentage of inorganic materials usually affects the energy density, safety performance and cycle performance of lithium-ion batteries. It can be seen from Examples 19 to 23 that by adjusting the mass percentage of inorganic materials within the scope of this application, the lithium-ion battery can have a higher volume energy density, nail penetration rate and more cycles, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance.

[0152] The type of inorganic material usually affects the energy density, safety performance and cycle performance of lithium-ion batteries. It can be seen from Examples 19 to 23 that the use of inorganic materials within the scope of this application can make the lithium-ion battery have a higher volume energy density, nail penetration rate and more cycles, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance.

[0153] The type of the second active material usually affects the energy density, safety performance and cycle performance of the lithium-ion battery. It can be seen from Example 12, Example 26 to Example 27 that the selection of the second active material within the scope of the present application can make the lithium-ion battery have a higher volume energy density, nail penetration rate and more cycles, indicating that the lithium-ion battery has a higher energy density, better safety performance and cycle performance.

[0154] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method or article including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method or article.

[0155] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0156] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. An electrochemical device, comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode material layer, wherein the positive electrode material layer comprises a first positive electrode material layer and a second positive electrode material layer, wherein the first positive electrode material layer is disposed between the positive electrode current collector and the second positive electrode material layer; The first positive electrode material layer includes a first active material, and the delithiation product of the first active material includes Li 5- x FeO 4-y , Li 5-x CoO 4-y , Li 2-z MnO2、Li 1.2-r Ni 0.13 Fe 0.13 Mn 0.54 O2 or Li 1-t At least one of FePO4, wherein 4≤x≤5, 2≤y≤3, 1.6≤z≤2, 1≤r≤1.2, 0.8≤t≤1; The second positive electrode material layer includes a second active material, and the second active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate or lithium manganese oxide; The negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes silicon element, and based on the mass of the negative electrode material layer, the mass percentage of the silicon element is 1% to 50%; The mass of the delithiation product of the first active material in the positive electrode sheet is A mg / 1540 mm 2 The mass of silicon in the negative electrode is B mg / 1540 mm 2 , 29%≤A / B≤230%.

2. The electrochemical device according to claim 1, wherein: 39%≤A / B≤200%.

3. The electrochemical device according to claim 1, wherein The delithiation product of the first active material includes LiFeO2, CoO2, MnO2, Ni 0.13 Fe 0.13 Mn 0.54 At least one of O2, FePO4, FeO2, Fe2O3 or FeO.

4. The electrochemical device according to claim 1, wherein Based on the mass of the first positive electrode material layer, the mass percentage of the delithiation product of the first active material is 30% to 96%.

5. The electrochemical device according to any one of claims 1 to 4, wherein: The mass of the second active material in the positive electrode sheet is C mg / 1540 mm 2 , 0.45%≤A / C≤6%.

6. The electrochemical device according to claim 5, wherein: 0.9%≤A / C≤4.5%.

7. The electrochemical device according to any one of claims 1 to 4, wherein: Based on the mass of the negative electrode material layer, the mass percentage of the silicon element is 1% to 20%.

8. The electrochemical device according to claim 5, which satisfies at least one of the following characteristics: (1) 1mg / 1540mm 2 ≤A≤14mg / 1540mm 2 ; (2) 3mg / 1540mm 2 ≤B≤12mg / 1540mm 2 ; (3) 200mg / 1540mm 2 ≤C≤300mg / 1540mm 2 .

9. The electrochemical device according to any one of claims 1 to 4, wherein: The first positive electrode material layer further includes an inorganic material, and the inorganic material includes at least one of aluminum oxide, lithium lanthanum zirconium oxide, lithium lanthanum titanate, lithium aluminum titanium phosphate, antimony-doped tin oxide or titanium oxide; Based on the mass of the first positive electrode material layer, the mass percentage of the inorganic material is 5% to 60%.

10. The electrochemical device according to any one of claims 1 to 4, wherein: The specific capacity of the first positive electrode material layer is 130 mAh / g to 780 mAh / g.

11. The electrochemical device according to claim 10, wherein: The specific capacity of the first positive electrode material layer is greater than or equal to the specific capacity of the second positive electrode material layer.

12. The electrochemical device according to any one of claims 1 to 4, wherein: The first active material includes at least one of the following compounds: Li5QO4 or Li5QO6, Q includes at least one of Ni, Co, Fe, Sn or Mn, and the valence state of the Q element is lower than its own highest oxidation valence state; Li q Fe 0.5(1+q) PO4,1≤q≤5; Li 2-a-b-c-d Ni a R b Mr c M d O 2-f ,0≤a<0.35,0<b<0.5,0.3<c≤0.6,0≤d<0.05,0.7<a+b+c+d <0.9, 0≤f<0.2, R includes at least one of Fe or Co, and M includes at least one of Mg, Al, Ti, V, Cr, Cu, Y, Zr, Nb, Mo, La or W; Li 1+e Mn 1-p X p O 2-s Y s ,-0.1<e<0.2,0≤p<0.2,0≤s<0.2,X is Fe、Co、Ti、Zn、 At least one of Mg, Al, V, Cr or Zr, and Y includes at least one of S, N, F, Cl or Br.

13. The electrochemical device according to claim 10, wherein: The first active material includes Li5FeO4, Li5CoO4, Li2MnO2, Li 1.2 Ni 0.13 Fe 0.13 Mn 0.54 At least one of O2 or LiFePO4.

14. The electrochemical device according to any one of claims 1 to 4, wherein: The negative electrode material layer includes a negative electrode active material, and the negative electrode active material includes at least one of silicon, silicon carbon or silicon oxygen.

15. The electrochemical device according to claim 14, wherein: The negative electrode active material further comprises at least one of graphite, hard carbon, soft carbon or mesophase micro carbon beads.

16. The electrochemical device according to any one of claims 1 to 4, wherein: The resistivity of the positive electrode material layer is ρΩ·m, 44≤ρ≤155.

17. An electronic device comprising the electrochemical device according to any one of claims 1 to 16.

Citation Information

Cited By

  • Electrochemical device and electronic device

    WO2026012016A1