Co / Ni-MOF-derived lithium-sulfur battery diaphragm modification material and preparation method thereof
The lithium-sulfur battery separator modification material derived from Co/Ni-MOF uses ultrasound-assisted synthesis and heat treatment technology to form a polar and highly conductive composite material, which solves the problem of polysulfide shuttle effect in lithium-sulfur batteries and significantly Improved battery cycle stability and energy density.
Patent Information
- Application Number
- CN202411164644.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-01
Smart Images

Figure CN118738759A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery separator materials, and in particular to a Co / Ni-MOF-derived lithium-sulfur battery separator modification material and a preparation method thereof. Background Art
[0002] With the continuous development of technology, traditional lithium-ion batteries can no longer meet the market's growing demand for energy density, so the development of a new generation of high-energy storage batteries is particularly urgent. Lithium-sulfur batteries have attracted much attention due to their high theoretical energy density and low cost. However, the shuttle effect of lithium polysulfide in the sulfur reduction reaction, the slow redox kinetics leading to low sulfur utilization and poor cycle stability, and the uneven lithium deposition / dissolution leading to dendrite growth are still important factors affecting battery safety and life. Therefore, exploring reasonable and effective methods is extremely important to solve the above key problems.
[0003] The separator is an important component of lithium-sulfur batteries. Traditional polyolefin separators have poor inhibition of intermediate polysulfide (LIPS) shuttle effect, poor lithium ion migration number, slow conversion kinetics, etc. More and more scholars are solving these problems by modifying the separator.
[0004] In order to achieve physical adsorption and chemical anchoring of polysulfides to alleviate the irreversible capacity fading problem caused by the shuttle effect, the membrane is modified using the active sites of surface functional groups possessed by some materials rich in pore structures. Studies have shown that various carbon materials with high conductivity, large surface area and chemical stability, such as porous carbon, graphene, graphyne and carbon nanotubes, are the main choices for modifying the membrane. However, the non-polar surface of carbon materials has a weak affinity for LiPSs, which means that they can only act as a physical barrier to prevent the diffusion of LiPSs and therefore cannot meet practical requirements. Therefore, polymer materials such as metal compounds and metal organic framework (MOFs) derivatives are needed to provide chemical interactions for anchoring LiPSs.
[0005] Based on this, the present application aims to design a Co / Ni-MOF-derived lithium-sulfur battery separator modification material, which utilizes the polarity of the nitrogen-doped carbon system and oxygen atoms to inhibit the dissolution of polysulfides in the electrolyte to a certain extent, thereby inhibiting the shuttling of polysulfides. Summary of the invention
[0006] The object of the present invention is to provide a Co / Ni-MOF-derived lithium-sulfur battery separator modification material and a preparation method thereof to inhibit the shuttling of polysulfides.
[0007] The present application discloses a Co / Ni-MOF-derived lithium-sulfur battery diaphragm modification material and a preparation method thereof, comprising the following steps: S1 used ultrasound-assisted synthesis of CoNi ZIFs precursor; S2 is a membrane-modified composite material obtained by heat treatment and chemical oxidation; S3 Weigh the membrane modified composite material, conductive carbon Super P, and polyvinylidene fluoride in proportion, put them in a mortar and stir them evenly; S4: N-methylpyrrolidone is added to the mixture of S3 to prepare a black slurry, which is ground until the slurry has almost no particle feeling, and then the slurry is coated on a separator (Celgard 2400); S5 The diaphragm prepared in S4 is vacuum dried in an oven, and the obtained modified diaphragm is made into a disk with a diameter of 16 mm, thereby obtaining a modified diaphragm.
[0008] Preferably, the preparation method of the CoNi ZIFs precursor in step S1 is: add Co(NO3)2·6H2O and Ni(NO3)2·6H2O to methanol and sonicate until fully dissolved; dissolve 2-methylimidazole in methanol and sonicate; mix the above solutions, stir at room temperature for 12 hours to obtain a new solution, and centrifuge at a speed of 8000 r / min to obtain a dark purple slurry, and wash three times with ethanol; finally, dry the product in an oven to obtain CoNi ZIFs.
[0009] Preferably, the method for preparing the membrane modified composite material in step S2 is: placing CoNi ZIFs in a crucible for heat treatment, raising the temperature to 300-400° C. at a rate of 1° C. / min in an air atmosphere, and reacting for 2-4 hours.
[0010] Preferably, the molar ratio of the membrane modified composite material, the conductive carbon Super P, and polyvinylidene fluoride in step S3 is 7:2:1.
[0011] Preferably, the drying temperature in step S5 is 60-80° C., and the reaction time is 8-14 hours.
[0012] Preferably, the preparation method of the Li2S6 solution for the visual adsorption experiment of the diaphragm material prepared in step S5 is as follows: S and Li2S powders are dissolved in a mixed solution of equal volumes of DOL and DME in a molar ratio of 1:5, and vigorously stirred at 70°C for 24 hours to obtain a Li2S6 solution.
[0013] The advantages of the present invention are that low-cost metal organic framework-derived bimetallic oxide / nitrogen-doped carbon nanosheets are designed and synthesized for lithium-sulfur batteries. (1) Nitrogen doping changes the local electron distribution in the carbon nanosheets, thereby greatly improving the conductivity and promoting the transmission of electrons / ions; (2) Cobalt oxide is used in lithium-sulfur batteries. On the basis of the 3D honeycomb structure, the improved separator allows rapid transmission of lithium ions while effectively suppressing the shuttle effect; (3) NiO has an ionic crystal structure, which makes NiO have certain conductive properties. At the same time, NiO can be used as a catalyst to promote the reaction rate or change the reaction path in chemical reactions. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1 Shown is a comparison diagram of Li2S6 adsorption of Example 1 and Comparative Example 1; Figure 2 Shown are cyclic voltammetry curves corresponding to different scan rates of the diaphragm battery of Example 1 and Comparative Example 1; Figure 3 Shown are the cycling performances of the materials of Example 1 and Comparative Example 1 at a current density of 0.2 C; In the figure: Figure 2 (a) Co3O4-NiO / NC-PP, Figure 2 (b) Co3O4 / NC-PP. DETAILED DESCRIPTION
[0016] The following will describe the technical solutions in the embodiments of the present invention in detail in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Example 1 S1 Co(NO3)2·6H2O and Ni(NO3)2·6H2O were weighed in a molar ratio of 1:1 and placed in a beaker containing methanol, and ultrasonically dispersed until fully dissolved; 2-methylimidazole was weighed in a mass volume ratio of 9g:10ml and dissolved in methanol, and ultrasonicated until completely dissolved; the above solutions were mixed, stirred at room temperature for 12h to obtain a new solution, centrifuged at 8000 r / min for 5min to obtain a dark purple slurry, and washed three times with ethanol; then dried in an oven at 60°C for 12h to obtain the precursor CoNi ZIFs; S2 CoNi ZIFs were placed in a crucible, and the temperature was raised to 350 °C at a rate of 1 °C / min in an air atmosphere for 2 h to obtain Co3O4-NiO / NC composite materials (diaphragm modified composite materials); S3 Weigh the membrane modified composite material, conductive carbon Super P, and polyvinylidene fluoride in a molar ratio of 7:2:1, place in a mortar and stir evenly; S4: N-methylpyrrolidone is added to the mixture of S3 to prepare a black slurry, which is ground until the slurry has almost no particle feeling, and then the slurry is coated on a separator (Celgard 2400); S5 The diaphragm prepared in S4 was vacuum dried in an oven at 60° C. for 10 h, and the obtained modified diaphragm was made into a disk with a diameter of 16 mm, thereby obtaining the modified diaphragm Co3O4-NiO / NC-PP. Comparative Example 1
[0018] Except that only the raw material Co(NO3)2·6H2O is weighed in step S1, the other steps are the same as those in Example 1; step S2 is to obtain the Co3O4-NC composite material; and finally the modified separator Co3O4 / NC-PP is obtained. Example 2
[0019] S1 Co(NO3)2·6H2O and Ni(NO3)2·6H2O were weighed in a molar ratio of 1:1 and placed in a beaker containing methanol, and ultrasonically dispersed until fully dissolved; 2-methylimidazole was weighed in a mass volume ratio of 10 g:15 ml and dissolved in methanol, and ultrasonicated until completely dissolved; the above solutions were mixed, stirred at room temperature for 12 h to obtain a new solution, centrifuged at 7500 r / min for 10 min to obtain a dark purple slurry, and washed three times with ethanol; then dried in an oven at 70°C for 10 h to obtain the precursor CoNi ZIFs; S2 CoNi ZIFs were placed in a crucible, and the temperature was raised to 350 °C at a rate of 1 °C / min in an air atmosphere for 2 h to obtain Co3O4-NiO / NC composite materials (diaphragm modified composite materials); S3 Weigh the membrane modified composite material, conductive carbon Super P, and polyvinylidene fluoride in a molar ratio of 7:2:1, place in a mortar and stir evenly; S4: N-methylpyrrolidone is added to the mixture of S3 to prepare a black slurry, which is ground until the slurry has almost no particle feeling, and then the slurry is coated on a separator (Celgard 2400); S5 The diaphragm prepared in S4 was vacuum dried in an oven at 60° C. for 12 h, and the obtained modified diaphragm was made into a disk with a diameter of 16 mm, thereby obtaining the modified diaphragm Co3O4-NiO / NC-PP. Example 3
[0020] S1 Co(NO3)2·6H2O and Ni(NO3)2·6H2O were weighed in a molar ratio of 1:1 and placed in a beaker containing methanol, and dispersed by ultrasonication until fully dissolved; 2-methylimidazole was weighed in a mass volume ratio of 9g:10ml and dissolved in methanol, and ultrasonication was performed until completely dissolved; the above solutions were mixed, stirred at room temperature for 12h to obtain a new solution, centrifuged at a speed of 8000 r / min for 5min to obtain a dark purple slurry, and washed three times with ethanol; then dried in an oven at 70°C for 10h to obtain the precursor CoNi ZIFs; S2 CoNi ZIFs were placed in a crucible, and the temperature was raised to 350 °C at a rate of 1 °C / min in an air atmosphere for 2 h to obtain Co3O4-NiO / NC composite materials (diaphragm modified composite materials); S3 Weigh the membrane modified composite material, conductive carbon Super P, and polyvinylidene fluoride in a molar ratio of 7:2:1, place in a mortar and stir evenly; S4: N-methylpyrrolidone is added to the mixture of S3 to prepare a black slurry, which is ground until the slurry has almost no particle feeling, and then the slurry is coated on a separator (Celgard 2400); S5 The diaphragm prepared in S4 was vacuum dried in an oven at 70°C for 10 h, and the obtained modified diaphragm was made into a disc with a diameter of 16 mm, so that the modified diaphragm Co3O4-NiO / NC-PP was obtained.
[0021] A visualized adsorption experiment was carried out on the prepared diaphragm material. The preparation method of the Li2S6 solution used in the experiment was as follows: S and Li2S powders were dissolved in a mixed solution of equal volumes of DOL and DME in a molar ratio of 1:5, and vigorously stirred at 70 °C for 24 hours to obtain a Li2S6 solution.
[0022] Weigh 2 mg of each of the diaphragm materials prepared in Example 1 and Comparative Example 1 and soak them in the prepared Li2S6 solution (4 mL) for 10 hours. At the same time, a comparative sample of the same volume of Li2S6 solution was prepared. The results are shown in Figure 1 As shown: When the material was first added, the material showed the same color as the control sample. After 10 hours, the solution with the added samples experienced different degrees of fading, among which the color of the Co3O4-NiO / NC sample was almost transparent, with the greatest degree of fading, and the Co3O4 / NC sample was not completely faded. The above shows that the Co3O4-NiO / NC sample has the best physical adsorption and chemical anchoring ability for polysulfides.
[0023] Cyclic voltammetry (CV) was used to test the electrochemical reactivity of button cells for the diaphragm materials prepared in Example 1 and Comparative Example 1. Figure 2 The results show that: Figure 2 As shown in a, in the voltage range of 1.7-2.8 V, the curve has two cathode peaks (2.27 V, 2.01 V), reflecting the reaction occurring during the discharge process - the reduction reaction of sulfur to lithium disulfide and then to solid lithium sulfide. The anode peak (2.42 V) indicates that lithium sulfide is oxidized to sulfur during the charging process. The results show that the Co3O4-NiO / NC electrode has a larger peak current and a narrower peak width, indicating that Co3O4-NiO / NC enhances the charge and discharge reaction kinetics of LiPS.
[0024] Then, the cycle performance of Example 1 and Comparative Example 1 was tested at a current density of 0.2 C. Figure 3 The results show that the initial capacity of the lithium-sulfur battery using Co3O4-NiO / NC-PP separator is 1021 mAh g –1 After 100 cycles of charge and discharge, the discharge capacity is 602 mAh g –1 , which is higher than that of the Co3O4 / NC-PP separator (initial capacity of 607 mAh g –1 ) lithium-sulfur battery, whose specific capacity is only 390 mAh g after 30 cycles –1 This indicates that Co3O4-NiO / NC can effectively inhibit the shuttle effect of polysulfides and promote the catalytic conversion of sulfur.
[0025] This implementation mode is only an exemplary description of this patent and does not limit its protection scope. Personnel in this field may also make partial changes to it. As long as it does not exceed the spirit of this patent, it shall be regarded as an equivalent replacement of this patent and shall be within the protection scope of this patent.
Claims
1. A Co / Ni-MOF-derived lithium-sulfur battery modified diaphragm material and a preparation method thereof, characterized in that: The steps include: S1 used ultrasound-assisted synthesis of CoNi ZIFs precursor; S2 is a membrane-modified composite material obtained by heat treatment and chemical oxidation; S3 Weigh the membrane modified composite material, conductive carbon Super P, and polyvinylidene fluoride in proportion, put them in a mortar and stir them evenly; S4: N-methylpyrrolidone is added to the mixture of S3 to prepare a black slurry, which is ground until the slurry has almost no particle feeling, and then the slurry is coated on a separator (Celgard 2400); S5 The diaphragm prepared in S4 is vacuum dried in an oven, and the obtained modified diaphragm is made into a disk with a diameter of 16 mm, thereby obtaining a modified diaphragm.
2. The method for preparing a diaphragm material according to claim 1, characterized in that: The preparation method of the CoNi ZIFs precursor in step S1 is as follows: Co(NO3)2·6H2O and Ni(NO3)2·6H2O are added to methanol and ultrasonicated until fully dissolved; 2-methylimidazole is dissolved in methanol and ultrasonicated; the above solutions are mixed, stirred at room temperature for 12 hours to obtain a new solution, and centrifuged at a speed of 8000 r / min to obtain a dark purple slurry, which is washed three times with ethanol; finally, the product is dried in an oven to obtain CoNi ZIFs.
3. The method for preparing a diaphragm material according to claim 1, characterized in that: The preparation method of the membrane modified composite material in step S2 is: placing CoNi ZIFs in a crucible for heat treatment, raising the temperature to 300-400° C. at a rate of 1° C. / min in an air atmosphere, and reacting for 2-4 hours.
4. The method for preparing a diaphragm material according to claim 1, characterized in that: The molar ratio of the membrane modified composite material, the conductive carbon Super P, and polyvinylidene fluoride in step S3 is 7:2:
1.
5. The method for preparing a diaphragm material according to claim 1, characterized in that: The drying temperature in step S5 is 60-80° C., and the reaction time is 8-14 hours.
6. The method for preparing a diaphragm material according to claim 1, characterized in that: The preparation method of the Li2S6 solution for the visual adsorption experiment of the diaphragm material prepared in step S5 is as follows: S and Li2S powders are dissolved in a mixed solution of equal volumes of DOL and DME in a molar ratio of 1:5, and vigorously stirred at 70°C for 24 hours to obtain a Li2S6 solution.