Zirconium oxide presintered body and sintered body

By controlling the content difference of stabilizing elements and coloring elements in the zirconia composition, a specific laminated structure is formed, which solves the problem of warping of the zirconia laminated body during heat treatment, achieves the light transmittance and color gradient effect of natural teeth, and Suitable for dental restorative materials.

CN118742525APending Publication Date: 2024-10-01TOSOH CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380022180.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-18
Filing Date
2023-02-16
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing zirconia laminate is prone to warping problems during heat treatment, and it is difficult to achieve the light transmittance and color gradient effect of natural teeth.

Method used

By controlling the content difference of stabilizing elements and coloring elements in the zirconium oxide composition, a specific laminated structure is formed, ensuring the light transmittance and color tone gradient along the lamination direction, and suppressing warpage during heat treatment.

Benefits of technology

The zirconia sintered body and pre-sintered body have the impression of natural teeth in visual recognition, and have gradual light transmittance and color tone. At the same time, warpage is suppressed, making it suitable for dental restoration materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742525A_ABST
    Figure CN118742525A_ABST
Patent Text Reader

Abstract

Provided are: a sintered body which has light transmittance and a gradual change in color tone and which is capable of impressing an impression close to natural teeth when viewed; and a pre-sintered body which forms the sintered body. Even when subjected to a heat treatment such as sintering and pre-sintering, at least one of the zirconia pre-sintered body and the sintered body does not exhibit undesirable impressions, and the like, does not exhibit undesirable impressions, and does not exhibit undesirable impressions, even if subjected to a heat treatment such as sintering and pre-sintering. Warping can also be suppressed. This zirconia sintered body contains (i) a zirconia containing a stabilizing element, or (ii) a zirconia containing a zirconia containing a stabilizing element and a coloring element. The sintered body has three or more regions stacked in layers, and the content of at least one of a stabilizing element and a coloring element in two adjacent regions among the regions is different from each other; in the laminated regions, the difference between the content of the stabilizing element contained in the first region located at one end and the content of the stabilizing element contained in the second region located at the other end is 2.0 mol% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a pre-sintered body of zirconia and a sintered body of zirconia as a zirconia laminate. Background Art

[0002] The sintered body of zirconium oxide (ZrO2) is manufactured by molding, pre-sintering and sintering a raw material powder mainly containing zirconium oxide. The raw material powder is thermally shrunk and densified by heat treatment such as sintering and pre-sintering, but the behavior during heat treatment varies depending on the characteristics of the raw material powder, especially the composition of the raw material powder.

[0003] Zirconia accounts for the majority of the raw material powder. Nevertheless, even if the raw material powders differ in the content of additives by only less than 0.1 wt%, the thermal shrinkage behavior of the two powders is very different. When a molded body formed by stacking raw material powders having such a slight difference in composition is subjected to heat treatment, undesirable conditions such as peeling off or deformation of a portion of the layer may occur. Even if it is the same zirconium oxide, the above-mentioned undesirable conditions may occur when additives are added thereto. In order to avoid these undesirable conditions when the molded body is heat treated, special adjustments or treatments are required (for example, Patent Documents 1 and 2).

[0004] Patent Document 1 discloses that the composition and thermal shrinkage behavior of raw material powders are adjusted by coating with a dopant, and the powders are molded to obtain a sintered body without deformation and composed of laminates of different tones. Patent Document 2 discloses that a sintered body composed of laminates of different coloring element contents and having a change in color tone is obtained by laminating and molding the laminates while applying vibrations such as a boundary layer formed by mixing powders of upper and lower layers. However, in the laminates disclosed in Patent Documents 1 and 2, the zirconium oxide that occupies the majority of the raw material powder has the same composition, and the texture of these laminates mainly derived from the light-transmitting feeling of the zirconium oxide is also the same. Therefore, a different texture is formed compared to natural teeth that have a texture that varies due to the light-transmitting feeling.

[0005] Therefore, there is a demand for a zirconium oxide laminate having light transmittance and a gradation of color tone that can give an impression close to natural teeth. Patent Document 3 discloses a laminated body in which a plurality of zirconium oxide composition layers having different chemical compositions are laminated. Prior art literature Patent Literature

[0006] Patent Document 1: U.S. Patent Application Publication No. 2016 / 0157971 Patent Document 2: U.S. Patent Application Publication No. 2014 / 0328746 Patent Document 3: U.S. Patent Application Publication No. 2015 / 0173869 Summary of the invention Technical problem to be solved by the invention

[0007] In Patent Document 3, layers in which the amounts of yttrium and coloring elements are changed stepwise are stacked from the bottom layer to the top layer, thereby gradually changing the color tone and transmittance. However, when layers with different compositions are stacked to gradually change the color tone and transmittance, the composition of the bottom layer and the top layer is greatly different, so the shrinkage rate of the bottom layer and the top layer varies greatly. When a molded body with a large difference in shrinkage rate between the bottom layer and the top layer is heat treated, a pre-sintered body or a sintered body that is greatly warped toward the side with a larger shrinkage rate is obtained.

[0008] Therefore, the purpose of the present disclosure is to provide at least one of a pre-sintered body and a sintered body of zirconia, wherein the sintered body can give an impression close to natural teeth when visually identified and has light transmittance and a gradation of color tone, and the pre-sintered body can provide such a sintered body, which suppresses warping even after heat treatment such as sintering and pre-firing. Another object of the present disclosure is to provide at least any one of a pre-sintered body and a sintered body suitable as a dental restorative material, and a method for producing the same. Technical solutions for solving technical problems

[0009] The present inventors focused on the relationship between the content of the stabilizing element in the zirconium oxide composition contained in the bottom layer and the content of the stabilizing element in the zirconium oxide composition contained in the top layer, or the relationship between the shrinkage rate of the bottom layer and the shrinkage rate of the top layer, and found that by controlling them to a specific relationship, a sintered body can be obtained that not only has light transmittance and a layered structure with a gradually changing color tone like natural teeth, but also has suppressed warping, as well as a pre-sintered body that provides such a sintered body.

[0010] That is, the present invention is as described in the claims, and the gist of the present invention is as follows. [1] A sintered body of zirconium oxide, wherein: The zirconium oxide contains (i) zirconium oxide containing a stabilizing element, or (ii) zirconium oxide containing a stabilizing element and a coloring element. The sintered body has three or more regions stacked in layers, and the contents of at least one of a stabilizing element and a coloring element are different between two adjacent regions among the regions. In the stacked regions, a difference in content of the stabilizing element contained in a first region located at one end and a difference in content of the stabilizing element contained in a second region located at the other end is 2.0 mol % or less. [2] The sintered body according to [1], wherein the third region stacked in a layer between the first region and the second region includes one or more regions. [3] A sintered body according to [2], wherein the third region includes two or more regions, and the increase or decrease trend of at least either the light transmittance or the hue does not change along the stacking direction from the first region to the third region, or from the second region to the third region. [4] A sintered body of zirconium oxide, wherein: The zirconium oxide contains (i) zirconium oxide containing a stabilizing element, or (ii) zirconium oxide containing a stabilizing element and a coloring element. The sintered body has three or more regions stacked in layers, and the contents of at least one of a stabilizing element and a coloring element are different between two adjacent regions among the regions. In the stacked regions, the difference in shrinkage rate between the sintered body of the first region located at one end and the sintered body of the second region located at the other end (shrinkage rate difference) is 0.4% or less. [5] The sintered body according to [4], wherein the third region stacked in a layer between the first region and the second region includes one or more regions. [6] A sintered body according to [5], wherein the third region includes more than two regions, and the increase or decrease trend of at least either the light transmittance or the hue does not change along the stacking direction from the first region to the third region, or from the second region to the third region. [7] A pre-sintered body of a zirconium oxide composition, wherein: The zirconium oxide composition comprises (iii) a zirconium oxide composition containing a stabilizing element having a neck structure, or (iv) a zirconium oxide composition containing a zirconium oxide containing a stabilizing element having a neck structure and a coloring element, The pre-sintered body has three or more regions stacked in layers, and two adjacent regions among the regions have different contents of at least one of a stabilizing element and a coloring element. In the stacked regions, a difference in content of the stabilizing element contained in a first region located at one end and a difference in content of the stabilizing element contained in a second region located at the other end is 2.0 mol % or less. [8] The pre-sintered body according to [7], wherein the third region stacked in a layer between the first region and the second region includes one or more regions. [9] The pre-sintered body according to [8], wherein the third region includes two or more regions, and the increasing and decreasing trend of the color tone does not change along the stacking direction from the first region to the third region or from the second region to the third region.

[10] A pre-sintered body, which is a pre-sintered body of a zirconium oxide composition, wherein: The zirconium oxide composition comprises (iii) a zirconium oxide composition containing a stabilizing element having a neck structure, or (iv) a zirconium oxide composition containing a zirconium oxide containing a stabilizing element having a neck structure and a coloring element, The pre-sintered body has three or more regions stacked in layers, and two adjacent regions among the regions have different contents of at least one of a stabilizing element and a coloring element. In the stacked regions, the difference in shrinkage rate between the pre-sintered body in the first region located at one end and the pre-sintered body in the second region located at the other end (shrinkage rate difference) is 0.4% or less.

[11] The pre-sintered body according to

[10] , wherein the third region stacked in a layered manner on the first region and the second region includes one or more regions.

[12] The pre-sintered body according to

[11] , wherein the third region includes two or more regions, and the increasing and decreasing trend of the color tone does not change along the stacking direction from the first region to the third region or from the second region to the third region.

[13] The method for producing a sintered body according to any one of [1] to [6], wherein: The manufacturing method comprises the steps of laminating three or more layers of a powder composition containing a raw material powder of zirconium oxide to obtain a molded body, and sintering the molded body at a temperature of 1200° C. to 1600° C.; The raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and, when containing a coloring element, the coloring element.

[14] The method for producing a sintered body according to any one of [1] to [6], wherein: The manufacturing method comprises the steps of: laminating three or more layers of a powder composition of a raw material powder of zirconium oxide to obtain a molded body, and pre-firing the molded body at 800° C. or higher and lower than 1200° C. to obtain a pre-sintered body, wherein the raw material powder of zirconium oxide comprises zirconium oxide containing a stabilizing element and a coloring element when the coloring element is contained; and A step of sintering the pre-sintered body at a temperature of 1200°C to 1600°C.

[15] The method for producing a pre-sintered body according to any one of [7] to

[12] , wherein: The manufacturing method comprises the steps of stacking three or more layers of a powder composition of a raw material powder containing zirconium oxide to obtain a molded body, and pre-firing the molded body at a temperature of 800° C. to less than 1200° C., wherein the raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and a coloring element when the raw material powder contains a coloring element.

[16] A dental material comprising the sintered body according to any one of [1] to [6].

[17] A dental material comprising the pre-sintered body according to any one of [7] to

[12] . Effects of the Invention

[0011] According to the present disclosure, at least one of a pre-sintered body and a sintered body of zirconium oxide can be provided, wherein the sintered body can give an impression close to natural teeth when visually recognized and has light transmittance and a gradient of color tone, and the pre-sintered body can provide such a sintered body, which suppresses warping even after heat treatment such as sintering and pre-firing. In addition, according to the present disclosure, it is possible to provide at least any one of a pre-sintered body, a sintered body, and a method for producing the same that is suitable as a dental restorative material. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 This is a schematic diagram showing a cross section of a sintered body having a structure in which three zirconium oxide layers are stacked. Figure 2 This is a schematic diagram showing a cross section of a sintered body having a structure in which four zirconium oxide layers are stacked. Figure 3 It is a schematic diagram explaining the molding process of uniaxial press molding. Figure 4 It is a schematic diagram explaining the molding process of CIP treatment. Figure 5 It is a schematic diagram showing a method of measuring warpage. Figure 6 It is a schematic diagram showing a method for measuring three-point bending strength. Figure 7 Schematic diagram showing zirconium oxide having a neck structure. Figure 8 It is a schematic diagram explaining the molding process of uniaxial press molding when producing the laminated body in the example. Fig. 9 It is a schematic diagram explaining the molding process of the CIP treatment when producing the laminated body in the example. DETAILED DESCRIPTION

[0013] Hereinafter, a sintered body and a pre-sintered body of zirconium oxide according to one embodiment of the present disclosure will be described in detail. It should be noted that the description of the constituent elements described below is an example for explaining one embodiment of the present disclosure, and the present disclosure is not limited to these contents.

[0014] In the present specification, the laminate may include any of a sintered body, a pre-sintered body and a molded body. The laminate of the present embodiment may be, for example, a sintered body as a dental restoration, or a pre-sintered body as a precursor thereof. For example, in the present embodiment, when the laminate is a sintered body, the sintered body has a structure in which a region including "zirconium oxide containing a stabilizing element (i.e., zirconium oxide in which a stabilizing element is solid-dissolved) and zirconium oxide containing a coloring element" is stacked in layers; when the laminate is a pre-sintered body, the pre-sintered body has a structure in which a region including "zirconium oxide containing a stabilizing element showing a necking structure and a zirconium oxide composition containing a coloring element" is stacked in layers; when the laminate is a molded body, the molded body has a structure in which a region including "a powder composition containing zirconium oxide containing a stabilizing element" and "a powder composition containing a coloring element" is stacked in layers. By stacking regions having different contents of at least one of the stabilizing element and the coloring element in a layered manner, light transmittance and color tone (for example, based on L * a * b * The color tone of the color system) changes along the direction in which the layers are stacked (hereinafter also referred to as the "stacking direction"), and it is possible to form a gradation of light transmittance and color tone. It should be noted that in the present disclosure, it is stipulated that regions are "stacked in layers", which means that: in the sintered body or pre-sintered body, there are multiple regions containing zirconium oxide with different compositions due to different contents of stabilizing elements and coloring elements, and these multiple regions exist along the stacking direction. In the present disclosure, there is no stipulation that a "layer stacking" state must be achieved in which the interface between layers can be visually identified and the stacking state of each layer can be confirmed. In the sintered body or pre-sintered body of the present embodiment, it is not required to achieve a stacking state in which each layer can be visually identified. Even in a state without a visually recognizable interface, as long as it can be considered that there are multiple regions with different compositions along one direction, it can be said that the region referred to in the present disclosure is equivalent to "stacked in layers".

[0015] In addition, the pre-sintered body and the sintered body are obtained by laminating and molding a powder composition layer of raw material powder containing zirconium oxide, and pre-sintering or sintering the molded body, wherein the raw material powder of zirconium oxide contains zirconium oxide containing stabilizing elements and coloring elements in the case of containing coloring elements. The "region" in the sintered body and the pre-sintered body is formed by pre-sintering and sintering each powder composition layer in the molded body. That is, each "region" in the sintered body and the pre-sintered body substantially corresponds to each powder composition layer in the molded body. Therefore, in this specification, on the basis of explaining the stacked structure of stacked bodies such as sintered bodies and pre-sintered bodies, when explaining each layer constituting the stacked structure, sometimes the "region" in the sintered body and the pre-sintered body is referred to as the "layer" constituting the stacked structure of the sintered body and the pre-sintered body for explanation.

[0016] In addition, in this specification, when a plurality of preferred lower limits and preferred upper limits are listed as preferred ranges of conditions related to any element, these lower limits and upper limits may be any combination when explaining the preferred ranges of conditions. For example, when the preferred range of the thickness of a layer is described as having a lower limit of 1 mm or more, more preferably 2 mm or more, and on the other hand, having an upper limit of 20 mm or less, more preferably 15 mm or less, the preferred embodiment of the thickness of the layer is, for example, 1 mm or more and 20 mm or less, 1 mm or more and 15 mm or less, 2 mm or more and 20 mm or less, or 2 mm or more and 15 mm or less. Hereinafter, the sintered body will be described.

[0017] (Sintered body) The sintered body involved in this embodiment is: A sintered body of zirconium oxide, wherein The zirconium oxide contains (i) zirconium oxide containing a stabilizing element, or (ii) zirconium oxide containing zirconium oxide containing a stabilizing element and a coloring element. The zirconium oxide includes (i) zirconium oxide containing a stabilizing element. The zirconium oxide containing a stabilizing element (i) may further contain a coloring element. In this case, the zirconium oxide includes (ii) zirconium oxide containing the zirconium oxide containing a stabilizing element and a coloring element. Furthermore, the sintered body has three or more regions stacked in layers, and the contents of at least one of the stabilizing element and the coloring element are different in two adjacent regions among the regions. In the stacked regions, a difference in content of the stabilizing element contained in a first region located at one end and a difference in content of the stabilizing element contained in a second region located at the other end is 2.0 mol % or less. In addition, a sintered body according to another aspect of the present embodiment is: A sintered body of zirconium oxide, wherein The zirconium oxide contains (i) zirconium oxide containing a stabilizing element, or (ii) zirconium oxide containing zirconium oxide containing a stabilizing element and a coloring element. Furthermore, the sintered body has three or more regions stacked in layers, and the contents of at least one of the stabilizing element and the coloring element are different in two adjacent regions among the regions. In the stacked regions, the difference in shrinkage rate between the sintered body of the first region located at one end and the sintered body of the second region located at the other end (shrinkage rate difference) is 0.4% or less.

[0018] The sintered body is a laminated body including a sintered structure. In the present embodiment, the sintered structure is a structure mainly composed of zirconium oxide in the late stage of sintering. The sintered body of the present embodiment has a zirconium oxide layer including zirconium oxide containing a stabilizing element; or in the case of containing a coloring element, the sintered body of the present embodiment has a zirconium oxide layer including zirconium oxide containing a stabilizing element and zirconium oxide containing a coloring element (hereinafter, these zirconium oxide layers are also collectively referred to as "zirconium oxide layers"). The zirconium oxide layer is mainly composed of zirconium oxide grains containing a stabilizing element. Therefore, the sintered body of the present embodiment can be regarded as a zirconium oxide layer including zirconium oxide grains containing a stabilizing element; or in the case of containing a coloring element, it can also be regarded as a laminate having three or more zirconium oxide layers containing zirconium oxide and a coloring element, wherein the zirconium oxide layer contains zirconium oxide grains containing a stabilizing element. It should be noted that, in this specification, the zirconium oxide layer is also referred to as a sintered body layer.

[0019] <Layered structure> A sintered body having a structure in which three zirconium oxide layers (sintered body layers) are stacked will be described below. Figure 1 It is a schematic diagram showing an example of the stacked structure of the sintered body according to the present embodiment. Figure 1 A cross section of a sintered body (100) having a structure in which three zirconium oxide layers are stacked is shown. Figure 1 Each of the three layers in corresponds to each "region" described in this disclosure. Figure 1 In the diagram, the stacking direction is represented as the Y-axis direction, and the spreading direction of each layer (hereinafter also referred to as the "horizontal direction") is represented as the X-axis direction. The sintered body (100) comprises a first zirconium oxide layer (hereinafter also referred to as the "first layer") (11), a second zirconium oxide layer (hereinafter also referred to as the "second layer") (12), and a third zirconium oxide layer (hereinafter also referred to as the "third layer") (13), and has a structure in which the first layer (11), the third layer (13) and the second layer (12) are stacked in sequence. The zirconium oxide compositions of the layers (regions) represented by the first layer (11), the third layer (13), and the second layer (12) are the same within the respective layers (regions), but the zirconium oxide compositions between adjacent layers are different. Each layer (each region) of the first layer (11), the third layer (13) and the second layer (12) may further contain a coloring element in addition to zirconium oxide containing a stabilizing element. The coloring element may be contained in all three layers of the first layer (11), the third layer (13) and the second layer (12), or may be contained in only a part of the layers. When the first layer (11), the third layer (13) and the second layer (12) do not contain coloring elements, the contents of stabilizing elements in each layer (each region) shown in the first layer (11), the third layer (13) and the second layer (12) are different from those in the adjacent layers (adjacent regions). When all or part of the first layer (11), the third layer (13) and the second layer (12) contain coloring elements, the content of at least one of the stabilizing element and the coloring element in each layer (each region) represented by the first layer (11), the third layer (13) and the second layer (12) is different from that in the adjacent layers (adjacent regions).

[0020] by Figure 1 As an example, the three zirconium oxide layers shown contain coloring elements. Figure 1 The sintered body according to the present embodiment will be described in detail. The sintered body (100) comprises a first zirconium oxide layer (first layer) (11) containing zirconium oxide containing a stabilizing element and a coloring element, a second zirconium oxide layer (second layer) (12) containing zirconium oxide containing a stabilizing element and a coloring element, and a third zirconium oxide layer (third layer) (13) containing zirconium oxide containing a stabilizing element and a coloring element, and has a structure in which the first layer (11), the third layer (13) and the second layer (12) are stacked in sequence. Each layer (region) represented by the first layer (11), the third layer (13), and the second layer (12) has the same zirconium oxide composition in each layer (region). Figure 1 In the X direction, no change in light transmittance or color tone due to a difference in content of at least one of the stabilizing element and the coloring element was observed.

[0021] On the other hand, each layer (each region) represented by the first layer (11), the third layer (13), and the second layer (12) has a different composition of zirconium oxide in the mutually adjacent layers (adjacent regions). That is, the content of at least one of the stabilizing element and the coloring element is different between the mutually adjacent layers (adjacent regions). “The composition of zirconium oxide in adjacent layers is different” means, for example: the content of stabilizing elements in adjacent layers remains unchanged and only the content of coloring elements changes; the content of coloring elements in adjacent layers remains unchanged and only the content of stabilizing elements changes; the content of both stabilizing elements and coloring elements in adjacent layers changes. by Figure 1 Taking the example of , the content of at least any one of the stabilizing element and the coloring element contained in the zirconia layer of the third layer (13) is different from the content of at least any one of the stabilizing element and the coloring element contained in the adjacent first layer (11), and is different from the content of at least any one of the stabilizing element and the coloring element contained in the adjacent second layer (12). Each layer (each region) represented by the first layer (11), the third layer (13), and the second layer (12) may have a different content of at least one of the stabilizing element and the coloring element from the adjacent layers (adjacent regions), but in order to obtain the desired light transmittance and color tone change, it is preferred that the content of the stabilizing element and the coloring element be different from the adjacent layers (adjacent regions). That is, it is preferred that the content of the stabilizing element and the coloring element contained in the zirconium oxide layer of the third layer (13) be different from the content of the stabilizing element and the coloring element contained in the adjacent first layer (11), and also be different from the content of the stabilizing element and the coloring element contained in the adjacent second layer (12).

[0022] By forming a structure in which zirconium oxide layers containing zirconium oxide with different contents of at least one of a stabilizing element and a coloring element are stacked between adjacent layers, it is possible to Figure 1 In the Y direction, a sintered body is formed in which changes in light transmittance and color tone due to differences in the contents of the stabilizing element and the coloring element can be visually recognized. It should be noted that in Figure 1 In the sintered body (100), the first layer and the third layer or the third layer and the second layer are connected via an interface. However, the sintered body of this embodiment can also be stacked without a visually identifiable interface, and the interface between the layers is not limited to a linear interface.

[0023] The sintered body of the present embodiment may have a structure in which three or more layers of zirconium oxide layers containing stabilizing elements and coloring elements are stacked, or may have a structure in which four or more layers, or further five or more layers, are stacked. The increase in the number of layers makes the sintered body a stacked body in which subtle changes in texture can be visually confirmed. In the case of forming a texture closer to natural teeth, the sintered body of the present embodiment may be exemplified by a structure in which three or more layers and ten or less of zirconium oxide layers are stacked, further three or more layers and six or less layers are stacked, further four or more layers and seven or less layers are stacked, and further four or more layers and six or less layers are stacked. A zirconium oxide layer other than the first layer and the second layer (hereinafter also referred to as an "intermediate layer") may be provided between the first layer and the second layer, and the sintered body of the present embodiment may include a plurality of intermediate layers. That is, the third region (intermediate layer) stacked in a layered manner between the first region and the second region may include not only one region but also two or more regions. The stacking order of the intermediate layers is arbitrary. For example, in the case of having multiple intermediate layers (the intermediate layer adjacent to the first layer is referred to as the "third layer"; for the second or more intermediate layers, they are referred to as the "fourth layer", "fifth layer", etc. in the stacking direction starting from the intermediate layer adjacent to the third layer), the sintered body of the present embodiment preferably has a structure in which the zirconium oxide layers are stacked in such a manner that the content of at least any one of the stabilizing element and the coloring element changes constantly in the stacking direction, that is, a structure in which the zirconium oxide layers are stacked in such a manner that the above-mentioned content increases (or decreases). It should be noted that, in the present embodiment, the structure in which the intermediate layer is sandwiched between the first layer and the second layer refers to a structure in which the intermediate layer is located between the first layer and the second layer in the stacking direction. An example in which the first layer, the third layer, and the second layer are stacked in sequence is as follows: Figure 1 As explained in the following, Figure 2 The case where the intermediate layer has multiple layers will be described. It should be noted that in this embodiment, the first, second, third, etc. are numbers given for the convenience of description, and the arrangement and stacking state of the stacking order are not limited to Figure 1 , Figure 2 The situation shown.

[0024] Figure 2 It is a schematic diagram showing another example of the structure of the sintered body according to the present embodiment. Figure 2 The cross section of a sintered body (200) having a structure in which four zirconium oxide layers are stacked is shown. The sintered body (200) has a structure in which, in addition to a first layer (21) and a second layer (22), a third layer (23) and a fourth layer (24) are stacked as intermediate layers. In each layer (each region) of the first layer (21), the third layer (23), the fourth layer (24) and the second layer (22), in addition to zirconium oxide containing a stabilizing element, a coloring element may be further contained. The coloring element may be contained in all four layers of the first layer (21), the third layer (23), the fourth layer (24) and the second layer (22), or may be contained in only a part of the layers. When the first layer (21), the third layer (23), the fourth layer (24) and the second layer (22) do not contain coloring elements, the contents of stabilizing elements in each layer (each region) shown in the first layer (21), the third layer (23), the fourth layer (24) and the second layer (22) are different from those in the adjacent layers (adjacent regions). In addition, when all or part of the first layer (21), the third layer (23), the fourth layer (24) and the second layer (22) contain coloring elements, the content of at least one of the stabilizing elements and the coloring elements in each layer (each region) represented by the first layer (21), the third layer (23), the fourth layer (24) and the second layer (22) is different from that in the adjacent layers (adjacent regions).

[0025] Below, with Figure 2 The following description will take as an example a sintered body in which the four zirconium oxide layers contain a coloring element. The sintered body (200) comprises: a first zirconium oxide layer (first layer) (21) containing zirconium oxide containing a stabilizing element and a coloring element; a second zirconium oxide layer (second layer) (22) containing zirconium oxide containing a stabilizing element and a coloring element; a third zirconium oxide layer (third layer) (23) containing zirconium oxide containing a stabilizing element and a coloring element; and a fourth zirconium oxide layer (fourth layer) (24) containing zirconium oxide containing a stabilizing element and a coloring element, and has a structure in which the first layer (21), the third layer (23), the fourth layer (24) and the second layer (22) are stacked in sequence. Each layer (each region) represented by the first layer (21), the third layer (23), the fourth layer (24), and the second layer (22) has a different composition of zirconium oxide in mutually adjacent layers (adjacent regions). That is, the content of at least one of the stabilizing element and the coloring element is different between mutually adjacent layers (adjacent regions). The content of at least one of the stabilizing element and the coloring element contained in the zirconia layer of the third layer (23) is different from the content of at least one of the stabilizing element and the coloring element contained in the zirconia layer of the adjacent first layer (21), and is different from the content of at least one of the stabilizing element and the coloring element contained in the zirconia layer of the adjacent fourth layer (24). In addition, the content of at least one of the stabilizing element and the coloring element contained in the zirconia layer of the fourth layer (24) is different from the content of at least one of the stabilizing element and the coloring element contained in the zirconia layer of the adjacent third layer (23), and is also different from the content of at least one of the stabilizing element and the coloring element contained in the zirconia layer of the adjacent second layer (22). Each layer (each region) represented by the first layer (21), the third layer (23), the fourth layer (24), and the second layer (22) may have a different content of at least one of the stabilizing element and the coloring element from the adjacent layers (adjacent regions), but in order to obtain the desired light transmittance and color tone change, it is preferred that the content of the stabilizing element and the coloring element be different from the adjacent layers (adjacent regions). That is, it is preferred that the content of the stabilizing element and the coloring element contained in the zirconium oxide layer of the third layer (23) be different from the content of the stabilizing element and the coloring element contained in the adjacent first layer (21), and further, the content of the stabilizing element and the coloring element contained in the adjacent fourth layer (24) be different. In addition, it is preferred that the content of stabilizing elements and coloring elements contained in the zirconium oxide layer of the fourth layer (24) is different from the content of stabilizing elements and the content of coloring elements contained in the adjacent third layer (23), and also different from the content of stabilizing elements and the content of coloring elements contained in the adjacent second layer (22).

[0026] When the third region (intermediate layer) includes two or more regions, the zirconium oxide layers are preferably stacked so that at least one of the light transmittance and the color tone does not change in the increasing and decreasing trend in the stacking direction. That is, in the case of including a plurality of zirconium oxide layers such as the fourth layer and the fifth layer, it is preferred that the zirconium oxide layers be stacked in such a manner that the increasing and decreasing trend of at least one of the light transmittance and the color tone does not change along the stacking direction. It is particularly preferred that the zirconium oxide layers be stacked in such a manner that the content of at least one of the stabilizing element and the coloring element changes constantly in the stacking direction. Thus, a gradient of light transmittance and the color tone can be formed by the difference in the content of at least one of the stabilizing element and the coloring element. However, in the present disclosure, as described in the columns of <<First Mode>> and <<Second Mode>> of <Characteristics of the Laminated Structure> described later, the amount of stabilizing elements or the shrinkage rate of the layer located at one end (i.e., a region that becomes the uppermost layer or the lowermost layer in the stacking direction) and the layer located at the other end (i.e., another region that becomes the uppermost layer or the lowermost layer in the stacking direction) are set to similar values. Therefore, in the present disclosure, in the case of a sintered body in which four or more zirconium oxide layers are stacked, the increase or decrease trend of at least one of the light transmittance and the color tone of any one of the layers located at one end or the other end along the stacking direction is sometimes opposite to the increase or decrease trend of the other layers. However, such a mode is also included in the present disclosure. This method will be described more specifically as shown in the following (a) and (b). (a) When the third region includes two or more regions, the composition of the layer may be such that the increase or decrease trend of at least one of the light transmittance and the color tone along the stacking direction does not change from the first region to the third region. Figure 2 In the composition of the layers, the following composition can be used: from the first layer (corresponding to the first region) (21) to the third layer (23) and the fourth layer (24) as the intermediate layer (corresponding to the third region), the increasing and decreasing trend of at least one of the light transmittance and the hue does not change. In this way, a gradient of light transmittance and hue close to that of natural teeth can be formed. The second layer (corresponding to the second region) (22) is stacked on the fourth layer (24). The second layer (22) is a layer that exhibits a value close to the content of the stabilizing element of the first layer, or a value close to the shrinkage rate of the first layer. By stacking the second layer (22) that is close to at least one of the content of the stabilizing element and the shrinkage rate of the first layer in this way, sometimes the increasing and decreasing direction of at least one of the light transmittance and the hue from the first layer (21) to the fourth layer (24) is reversed. However, in such a case, when processing into the shape of a dental product such as a crown shape, for example, it is sufficient to adjust the crown shape in a stacked range that forms the desired gradient. (b) When the third region includes two or more regions, the composition of the layer may be such that the increase or decrease trend of at least one of the light transmittance and the color tone along the stacking direction does not change from the second region to the third region. Figure 2In the composition of the layers, the following composition can be used: from the second layer (corresponding to the second region) (22) to the fourth layer (24) and the third layer (23) as the intermediate layer (corresponding to the third region), the increasing and decreasing trend of at least one of the light transmittance and the hue does not change. Thus, a gradient of light transmittance and hue close to that of natural teeth can be formed. The first layer (corresponding to the first region) (21) is stacked below the third layer (23). The first layer (21) is a layer that exhibits a value close to the content of the stabilizing element of the second layer, or a value close to the shrinkage rate of the second layer. Therefore, by stacking the first layer (21) that is close to at least one of the content of the stabilizing element and the shrinkage rate of the second layer, sometimes the increasing and decreasing direction of at least one of the light transmittance and the hue from the second layer (22) to the third layer (23) is reversed. However, in such a case, when processing into the shape of a dental product such as a crown shape, for example, it is sufficient to adjust the crown shape in a stacked range that forms the desired gradient.

[0027] <Features of the laminated structure> Preferred embodiments of the sintered body of the present disclosure include a sintered body described in the following embodiment (A) and a sintered body described in the following embodiment (B).

[0028] <<Method (A)>> In the sintered body of the present embodiment, the difference between the content of the stabilizing element contained in the first region located at one end and the content of the stabilizing element contained in the second region located at the other end in the stacked regions is 2.0 mol % or less. use Figure 1 The method (A) is described below. Figure 1 In the Y-axis direction (stacking direction), the content of the stabilizing element contained in the first region located at one end (for example, the first layer (11)) and the second region located at the other end (for example, the second layer (12)) is set to a close value (specifically, less than 2.0 mol%). Thus, the difference in shrinkage between the first layer and the second layer in the stacking direction of the sintered body is balanced, and the warping of the sintered body can be suppressed. As a result, the sintered body of this embodiment has light transmittance close to that of natural teeth, gradation of color tone, suppressed warping, and less deformation. In the present embodiment, only the relationship between the first region (e.g., the first layer (11)) located at one end and the second region (e.g., the second layer (12)) located at the other end is specified, but if the shrinkage rate of the regions (layers) located at the two end portions is adjusted, the warping of the sintered body can be effectively suppressed. Therefore, for each layer of the intermediate layer arranged between the first layer (11) and the second layer (12), a zirconium oxide layer having an arbitrary composition can be stacked. In the sintered body of the present embodiment, the difference between the content of the stabilizing element contained in the first region and the content of the stabilizing element contained in the second region is 2.0 mol% or less, preferably 1.8 mol% or less, 1.5 mol% or less, or 0.8 mol% or less. The difference between the content of the stabilizing element contained in the first region and the content of the stabilizing element contained in the second region is preferably small, for example, 0 mol% or more, more than 0 mol%, 0.1 mol% or more, or 0.3 mol% or more. The difference can be 0 mol% or more and 2.0 mol% or less, 0 mol% or more and 1.5 mol% or less, more than 0 mol% and 1.8 mol% or less, or more than 0 mol% and 1.5 mol% or less.

[0029] In the present embodiment, the content of the stabilizing element in each region (layer) is the molar ratio of the stabilizing element in terms of oxide to the total of zirconium oxide and the stabilizing element in terms of oxide. The oxide conversion of the stabilizing element is as follows: yttrium is Y2O3, calcium is CaO, magnesium is MgO, cerium is CeO2, praseodymium is Pr6O 11 , neodymium is set to Nd2O3, terbium is set to Tb4O7, erbium is set to Er2O3, and ytterbium is set to Yb2O3. For example, when yttrium and erbium are included as stabilizing elements, the content (mol%) of the stabilizing elements is calculated by (Y2O3+Er2O3) / (ZrO2+Y2O3+Er2O3)×100.

[0030] <<Method (B)>> In the sintered body of the present embodiment, the difference in shrinkage rate between the first region at one end and the second region at the other end in the stacked regions (shrinkage rate difference) is 0.4% or less.

[0031] use Figure 1 The method (B) is described below. Figure 1 In the Y-axis direction (stacking direction), the shrinkage rates of the sintered bodies of the first region (e.g., the first layer (11)) located at one end and the second region (e.g., the second layer (12)) located at the other end are set to close values ​​(specifically, less than 0.4%). Thus, the difference in shrinkage between the first layer and the second layer in the stacking direction of the sintered body is balanced, and the warping of the sintered body can be suppressed. As a result, the sintered body of this embodiment has light transmittance close to that of natural teeth, gradation of color tone, suppressed warping, and less deformation. In the present embodiment, only the relationship between the first region (e.g., the first layer (11)) located at one end and the second region (e.g., the second layer (12)) located at the other end is specified, but if the shrinkage rate of the regions (layers) located at the two end portions is adjusted, the warping of the sintered body can be effectively suppressed. Therefore, for each layer of the intermediate layer arranged between the first layer (11) and the second layer (12), a zirconium oxide layer having an arbitrary composition can be stacked. In the sintered body of the present embodiment, the difference between the shrinkage rate of the sintered body in the first region and the shrinkage rate of the sintered body in the second region is 0.4% or less, preferably 0.36% or less, 0.3% or less, or 0.2% or less. The difference between the shrinkage rate of the sintered body in the first region and the shrinkage rate of the sintered body in the second region is preferably small, for example, 0% or more, more than 0%, 0.01% or more, or 0.02% or more. The difference may be 0% or more and 0.4% or less, more than 0% and 0.36% or less, 0.01% or more and 0.2% or more and 0.02% or less.

[0032] <<<Measurement method of shrinkage ratio>>> The shrinkage rates of the first region (eg, the first layer (11)) located at one end and the second region (eg, the second layer (12)) located at the other end are determined as follows. A raw material powder of zirconium oxide having the same composition as the first layer (11) and the second layer (12) is filled into a mold, and after being molded by uniaxial pressing (hereinafter also referred to as "uniaxial pressing"), a cold isostatic pressing (hereinafter also referred to as "CIP") treatment is performed to form a powder composition layer as a sample for measuring shrinkage. The powder composition layer is pre-sintered at 800°C or higher and lower than 1200°C, and then sintered at 1200°C or higher and lower than 1600°C to obtain a zirconium oxide layer. The shrinkage of the zirconium oxide layer is determined by the method described in the column [Method for evaluating shrinkage] below.

[0033] This is further described in detail below. The sample for measuring the shrinkage rate may be prepared under the following conditions. [Samples for shrinkage measurement] Mold diameter: Φ25mm Powder mass: 4g Molding pressure: Uniaxial pressing: 49MPa + CIP treatment: 196MPa Molding process: Powder for evaluation is placed in a mold → flattened → uniaxial pressing →CIP treatment

[0034] In the above sample preparation, Figure 3 A diagram schematically showing the molding process of uniaxial press molding is shown. Figure 4 A diagram schematically showing a molding process of a CIP treatment is shown. exist Figure 3 , the process of pressurizing the powder by “(a) charging the powder into the mold (32) (31) → (b) leveling the powder → (c) uniaxial pressing (33)” is shown. exist Figure 4 In the figure, the powder (41) after uniaxial pressing is placed in a high-pressure container, the high-pressure container is filled with a solvent such as water (42), and the powder is isotropically pressurized by water pressure (CIP treatment).

[0035] The obtained sample for measuring shrinkage was pre-fired under the following conditions and then sintered. [Pre-calcination and sintering conditions] The pre-calcination is performed at 800° C. or higher and lower than 1200° C., and the sintering is performed at 1200° C. or higher and 1600° C. or lower. More detailed conditions can be appropriately selected. Preferably, in the present disclosure, the pre-calcination is performed under the following conditions, and then the sintering is performed. Pre-sintering: from room temperature to 300°C at 15°C / hour, keep at 300°C for 5 hours, from 300°C to 700°C at 15°C / hour, keep at 700°C for 1 hour, from 700°C to 1000°C at 50°C / hour, keep at 1000°C for 2 hours, and then cool in the furnace. Sintering: 100°C / hour from room temperature to 1500°C, maintained at 1500°C for 2 hours, and then cooled in the furnace.

[0036] The shrinkage rate of the sintered body of the sample for shrinkage rate measurement obtained as described above was measured. [Evaluation method of shrinkage rate] The diameter of the sintered body of the sample for measuring shrinkage (hereinafter also referred to as "sample diameter") is measured with a vernier caliper. The sample diameter is measured at four points using a vernier caliper, and the average of the measured values ​​is taken as the sample diameter. The shrinkage rate was calculated according to the following formula (1). Shrinkage rate (%) = (mold diameter: Φ25mm-sample diameter) / mold diameter: Φ25mm×100...(1) For example, if the sample diameter is 24 mm, the shrinkage is (25-24) / 25×100=4%.

[0037] <Composition of Zirconia Layer> The sintered body of the present embodiment includes a zirconium oxide layer, and the zirconium oxide layer contains zirconium oxide containing a stabilizing element and a coloring element in the case of containing a coloring element. The zirconium oxide layer is a layer with zirconium oxide as the main component, and the zirconium oxide is zirconium oxide containing a stabilizing element. The sintered body and zirconium oxide layer (sintered body layer) of the present embodiment not only contain zirconium oxide containing a stabilizing element and a coloring element, but may also contain unavoidable impurities such as hafnium oxide (HfO2). The content of hafnium oxide as an unavoidable impurity varies greatly depending on the raw material ore and the manufacturing method, and can be exemplified as less than 2.0% by mass. In the present embodiment, the calculation of the values ​​related to the composition, such as the calculation of the content and density, can be calculated by treating the hafnium oxide as zirconium oxide (ZrO2).

[0038] In the sintered body of the present embodiment, the zirconium oxide is preferably zirconium oxide in a state where zirconium oxide is sintered after heat treatment of zirconium oxide sol, more preferably zirconium oxide in a state where zirconium oxide is sintered after heat treatment of zirconium oxide sol obtained by hydrolysis of a zirconium compound, and further preferably zirconium oxide in a state where zirconium oxide is sintered after heat treatment of zirconium oxide sol obtained by hydrolysis of zirconium oxychloride. The zirconium oxide contained in the zirconium oxide layer may be sintered zirconium oxide, that is, zirconium oxide crystal grains.

[0039] <<Stabilizing elements>> The stabilizing element may be any element that has the function of inhibiting the phase transition of zirconium oxide. The stabilizing element may include at least one of an element that does not have the function of coloring zirconium oxide but has the function of inhibiting the phase transition (hereinafter, also referred to as a "non-coloring stabilizing element") and an element that has the function of coloring zirconium oxide and has the function of inhibiting the phase transition (hereinafter, also referred to as a "coloring stabilizing element"), and may be a non-coloring stabilizing element or a coloring stabilizing element, and preferably contains at least a non-coloring stabilizing element. Specific examples of the stabilizing element include one or more selected from yttrium (Y), calcium (Ca), magnesium (Mg), cerium (Ce), praseodymium (Pr), neodymium (Nd), terbium (Tb), erbium (Er) and ytterbium (Yb). Examples of the non-coloring stabilizing element include one or more selected from the group consisting of yttrium, calcium, magnesium, and cerium, preferably at least one of yttrium and cerium, and more preferably yttrium. Examples of the coloring stabilizing element include one or more selected from praseodymium, neodymium, terbium, erbium, and ytterbium, and preferably at least one of terbium and erbium. Preferred stabilizing elements include at least one selected from yttrium, terbium and erbium, further yttrium, terbium and erbium, further yttrium and at least one of terbium and erbium, further erbium and yttrium, further yttrium. The stabilizing element is contained in zirconium oxide, and is dissolved in zirconium oxide. In addition, the sintered body of the present embodiment preferably does not contain undissolved stabilizing elements, that is, does not contain stabilizing elements that are not dissolved in zirconium oxide. In the present embodiment, "does not contain undissolved stabilizing elements" means that in the XRD measurement and XRD spectrum analysis described later, no XRD peak derived from the stabilizing element is confirmed; as long as the XRD peak derived from the stabilizing element is not confirmed, the undissolved stabilizing element is allowed.

[0040] In the sintered body of the present embodiment, the content of the stabilizing element in the zirconia containing the stabilizing element contained in each layer (corresponding to each region) can be, for example, a lower limit of 1.5 mol% or more, 2.5 mol% or more, 3.0 mol% or more, 3.5 mol% or more, or 4.0 mol% or more, and an upper limit of 7.0 mol% or less, 6.0 mol% or less, or 5.0 mol% or less. These upper and lower limits can be any combination. Therefore, the content of the stabilizing element in the zirconia containing the stabilizing element contained in each layer (corresponding to each region) of the present embodiment can be 1.5 mol% or more and 7.0 mol% or less, 2.5 mol% or more and 6.0 mol% or more, or 3.0 mol% or more and 6.0 mol% or less.

[0041] For example, Figure 1 Taking the sintered body as an example, the content of the stabilizing element in the zirconia containing the stabilizing element contained in the first layer (corresponding to the first region) (11) and the second layer (corresponding to the second region) (12) is preferably 1.5 mol% or more or 2.5 mol% or more, and the upper limit is preferably 6.0 mol% or less or 5.5 mol% or less. These upper and lower limits may be any combination. Therefore, in the present embodiment, the content of the stabilizing element in the zirconia containing the stabilizing element contained in the first layer (corresponding to the first region) (11) and the second layer (corresponding to the second region) (12) is 1.5 mol% or more and 6.0 mol% or 2.5 mol% or more and 5.5 mol% or less. Figure 1 The content of the stabilizing element in the zirconia containing the stabilizing element contained in the third layer (corresponding to the third region) (13) in the sintered body is, for example, preferably 2.5 mol% or more or 3.0 mol% or more, and the upper limit is preferably 7.0 mol% or less or 6.0 mol% or less. These upper and lower limits may be any combination. Therefore, the content of the stabilizing element in the zirconia containing the stabilizing element contained in the third layer (corresponding to the third region) (13) of the present embodiment is 2.5 mol% or more and 7.0 mol% or less, or 3.0 mol% or more and 6.0 mol% or less. exist Figure 1 In the embodiment of the present invention, the difference in the content of the stabilizing element in the adjacent layers is preferably 0.01 mol% or more, more preferably 0.2 mol% or more, more preferably 0.3 mol% or more, more preferably 0.5 mol% or more, more preferably 0.7 mol% or more, more preferably 1.0 mol% or more, and more preferably 1.2 mol% or more. The larger the difference in the content of the stabilizing element, the greater the difference in the light transmittance between the zirconia layers. On the other hand, there is a tendency that the warping becomes larger. If the difference in the content of the stabilizing element in the adjacent layers is less than 2.5 mol%, further less than 2.0 mol%, and further less than 1.7 mol%, the change in the light transmittance of the sintered body is likely to become the same as the change in the light transmittance of a natural tooth. The difference in the content of the stabilizing element in adjacent layers may be exemplified by 0.01 mol% to less than 2.5 mol%, 0.2 mol% to 2.0 mol%, 0.3 mol% to 1.7 mol%, further 0.5 mol% to 1.7 mol%, or 1.2 mol% to 1.7 mol%.

[0042] In addition, Figure 2 Taking the sintered body as an example, the content of the stabilizing element in the zirconia containing the stabilizing element contained in the first layer (corresponding to the first region) (21) and the second layer (corresponding to the second region) (22), for example, the respective lower limits are preferably greater than 1.5 mol% or greater than 2.5 mol%, and the upper limits are preferably less than 7.0 mol% or less than 6.0 mol%. These upper and lower limits may be any combination. Therefore, in the present embodiment, the content of the stabilizing element in the zirconia containing the stabilizing element contained in the first layer (corresponding to the first region) (21) and the second layer (corresponding to the second region) (22) is preferably greater than 1.5 mol% and less than 7.0 mol%, or greater than 2.5 mol% and less than 6.0 mol%. Figure 2 The content of the stabilizing element in the zirconia containing the stabilizing element contained in the third layer (corresponding to the third region) (23) and the fourth layer (corresponding to the third region) (24) of the intermediate layer in the sintered body is, for example, preferably 2.0 mol% or more or 2.5 mol% or more, and the upper limit is preferably 6.0 mol% or less or 5.5 mol% or less. These upper and lower limits may be any combination. Therefore, the content of the stabilizing element in the zirconia containing the stabilizing element contained in the third layer (corresponding to the third region) (23) and the fourth layer (corresponding to the third region) (24) of the present embodiment is preferably 2.0 mol% or more and 6.0 mol% or less, or 2.5 mol% or more and 5.5 mol% or less. exist Figure 2In the embodiment of the present invention, the difference in the content of the stabilizing element in the adjacent layers is preferably 0.01 mol% or more, more preferably 0.2 mol% or more, more preferably 0.3 mol% or more, more preferably 0.5 mol% or more, more preferably 0.7 mol% or more, more preferably 1.0 mol% or more, and more preferably 1.2 mol% or more. The larger the difference in the content of the stabilizing element, the greater the difference in the light transmittance between the zirconia layers. On the other hand, there is a tendency that the warping becomes larger. If the difference in the content of the stabilizing element in the adjacent layers is 2.5 mol% or less, less than 2.5 mol%, further 2.0 mol% or less, and further 1.7 mol% or less, the change in the light transmittance of the sintered body is likely to become the same as the change in the light transmittance of a natural tooth. The difference in the content of the stabilizing element in adjacent layers can be exemplified by 0.01 mol% to 2.5 mol%, 0.01 mol% to less than 2.5 mol%, 0.2 mol% to 2.0 mol%, 0.3 mol% to 1.7 mol%, further 0.5 mol% to 1.7 mol%, or 1.2 mol% to 1.7 mol%.

[0043] The stabilizing element content of the sintered body is obtained by the following formula, and varies depending on the thickness of each zirconium oxide layer. Stabilizing element content of sintered body = (thickness of the first layer / height of the sintered body) × content of stabilizing elements in the first layer + (thickness of the second layer / height of the sintered body) × content of the stabilizing element in the second layer +…… + (thickness of the nth layer / height of the sintered body) × content of the stabilizing element in the nth layer In the present embodiment, as described above, the content of the stabilizing element is the molar ratio of the stabilizing element to the total of zirconium oxide and the stabilizing element. In calculating the content of the stabilizing element, the content of each stabilizing element may be obtained by performing the above-mentioned oxide conversion.

[0044] <<Coloring Elements>> The coloring element in the present embodiment is an element having the function of coloring zirconium oxide. As a specific coloring element, at least any one of transition metal elements and lanthanide rare earth elements can be exemplified, preferably one or more selected from iron (Fe), cobalt (Co), nickel (Ni), manganese (Mn), titanium (Ti), praseodymium (Pr), neodymium (Nd), europium (Eu), gadolinium (Gd), terbium (Tb), erbium (Er) and ytterbium (Yb), more preferably one or more selected from iron, cobalt, manganese, titanium, praseodymium, gadolinium, terbium and erbium, and more preferably one or more selected from iron, cobalt, titanium, terbium and erbium. The coloring element contained in the sintered body of the present embodiment is at least one of the coloring elements contained in the state of oxide (hereinafter, also referred to as "oxide coloring elements") and coloring stabilizing elements, etc., which are contained in the state of solid solution in zirconium oxide. As preferred oxide coloring elements, one or more selected from iron, cobalt, nickel, manganese and titanium can be cited, and one or more selected from iron, cobalt and titanium are more preferred. The sintered body of this embodiment may contain two or more coloring elements, for example, two or more and five or less, and further three or more and four or less coloring elements. The sintered body of this embodiment preferably contains at least a coloring stabilizing element, more preferably contains at least one of terbium and erbium, and further preferably contains at least terbium and erbium. The type and content of the coloring element contained in each zirconium oxide layer can be appropriately selected in consideration of the shrinkage rate of each layer and the like. Regarding the content of the coloring element of the sintered body of the present embodiment, the lower limit is more than 0% by mass, preferably more than 0.01% by mass, more than 0.03% by mass, or more than 0.04% by mass, in terms of the mass ratio of the coloring element after oxide conversion to the mass of the sintered body of the present embodiment; in addition, the upper limit is preferably less than 2.0% by mass, less than 0.8% by mass, or less than 0.3% by mass. These upper and lower limits can be any combination. Therefore, the content of the coloring element of the sintered body of the present embodiment, in terms of the mass ratio of the coloring element after oxide conversion to the mass of the sintered body of the present embodiment, can be, for example, more than 0% by mass and less than 2.0% by mass, more than 0.01% by mass and less than 1.2% by mass, more than 0.03% by mass and less than 0.8% by mass, or more than 0.04% by mass and less than 0.3% by mass. For example, when yttrium (non-coloring stabilizing element) and erbium (coloring stabilizing element) are contained as stabilizing elements, and aluminum oxide and cobalt (oxide coloring elements) are contained, the content (mass %) of the coloring elements is calculated by (Co3O4+Er2O3) / (ZrO2+Y2O3+Er2O3+Co3O4+Al2O3)×100. 11, neodymium is set to Nd2O3, terbium is set to Tb4O7, erbium is set to Er2O3, ytterbium is set to Yb2O3, iron is set to Fe2O3, cobalt is set to Co3O4, nickel is set to NiO, manganese is set to Mn3O4 and titanium is set to TiO2.

[0045] Regarding the content of the coloring element in the sintered body layer of the present embodiment, the content of the coloring element in terms of the mass ratio of the oxide-converted coloring element to the mass of the sintered body of the present embodiment is preferably, for example, a lower limit of more than 0 mass%, more than 0.01 mass%, more than 0.03 mass%, or more than 0.04 mass%; in addition, the upper limit is preferably less than 2.0 mass%, less than 1.2 mass%, less than 0.8 mass%, or less than 0.3 mass%. These upper and lower limits can be any combination. Therefore, in terms of the mass ratio of the coloring element in terms of the oxide-converted coloring element to the mass of the sintered body of the present embodiment, examples include more than 0 mass% and less than 2.0 mass%, more than 0.01 mass% and less than 1.2 mass%, more than 0.03 mass% and less than 0.8 mass%, or more than 0.04 mass% and less than 0.3 mass%. For example, Figure 1 Taking the sintered body as an example, the content of the coloring element in the zirconium oxide containing the coloring element contained in the first layer (corresponding to the first region) (11) and the second layer (corresponding to the second region) (12) can be, for example, 0.01 mass% or more, 0.05 mass% or more, or 0.1 mass% or more, and the upper limit can be 2.0 mass% or less or 1.2 mass% or less. These upper and lower limits can be any combination. Therefore, the content of the coloring element in the zirconium oxide containing the coloring element contained in the first layer (corresponding to the first region) (11) and the second layer (corresponding to the second region) (12) of the present embodiment can be 0.01 mass% or more and 2.0 mass% or 0.05 mass% or more and 1.2 mass% or less. Figure 1 The content of the coloring element in the zirconium oxide containing the coloring element contained in the third layer (corresponding to the third region) (13) in the sintered body is preferably 0.001 mass % or more or 0.1 mass % or more, and the upper limit is more preferably 2.0 mass % or less or 1.2 mass % or less. These upper and lower limits can be any combination. Therefore, the content of the coloring element in the zirconium oxide containing the coloring element contained in the third layer (corresponding to the third region) (13) of the present embodiment is 0.001 mass % or more and 2.0 mass % or 0.1 mass % or more and 1.2 mass % or less. exist Figure 1In the embodiment of the present invention, the difference in the content of the coloring element in the adjacent layers is preferably 0.002 mass %, 0.005 mass %, 0.01 mass %, 0.015 mass % or more, or 0.02 mass %. There is a tendency that the greater the difference in the content of the coloring element, the greater the difference in the color tone between the zirconium oxide layers. On the other hand, there is also a situation where the warping becomes larger. If the difference in the content of the coloring element in the adjacent layers is 1 mass % or less, further 0.8 mass % or less, and further 0.5 mass % or less, the color tone change of the sintered body is likely to become the same as the color tone change of natural teeth. The difference in the content of the coloring element in the adjacent layers is preferably 0.002 mass % or more and 1 mass %, 0.005 mass % or more and 0.8 mass %, 0.01 mass % or more and 0.5 mass %, 0.015 mass % or more and 0.5 mass % or less, or 0.02 mass % or more and 0.5 mass %.

[0046] In addition, Figure 2 Taking the sintered body as an example, the content of the coloring element in the zirconium oxide containing the coloring element contained in the first layer (corresponding to the first region) (21) and the second layer (corresponding to the second region) (22) is preferably 0.01 mass% or more, 0.05 mass% or more, or 0.1 mass% or more, and the upper limit is preferably 2.0 mass% or less or 1.2 mass% or less. These upper and lower limits can be any combination. Therefore, in the present embodiment, the content of the coloring element in the zirconium oxide containing the coloring element contained in the first layer (corresponding to the first region) (21) and the second layer (corresponding to the second region) (22) is 0.01 mass% or more and 2.0 mass% or 0.05 mass% or more and 1.2 mass% or less. As Figure 2 The content of the coloring element in the zirconium oxide containing the coloring element contained in the third layer (corresponding to the third region) (23) and the fourth layer (corresponding to the third region) (24) of the intermediate layer in the sintered body is preferably 0.001 mass % or more or 0.1 mass % or more, and the upper limit is preferably 2.0 mass % or less or 1.2 mass % or less. These upper and lower limits can be any combination. Therefore, the content of the coloring element in the zirconium oxide containing the coloring element contained in the third layer (corresponding to the third region) (23) and the fourth layer (corresponding to the third region) (24) of the present embodiment is 0.001 mass % or more and 2.0 mass % or 0.1 mass % or more and 1.2 mass % or less. exist Figure 2In the embodiment of the present invention, the difference in the content of the coloring element in the adjacent layers is preferably 0.001 mass %, 0.002 mass %, 0.005 mass %, 0.01 mass %, 0.05 mass % or 0.1 mass %. There is a tendency that the greater the difference in the content of the coloring element, the greater the difference in the color tone between the zirconium oxide layers. On the other hand, there is also a situation where the warping becomes larger. If the difference in the content of the coloring element in the adjacent layers is 1 mass % or less, further 0.8 mass % or less, and further 0.5 mass % or less, the color tone change of the sintered body is easy to become the same as the color tone change of natural teeth. The difference in the content of the coloring element in the adjacent layers is preferably 0.002 mass % or more and 1 mass %, 0.005 mass % or more and 0.8 mass %, 0.01 mass % or more and 0.5 mass %, 0.015 mass % or more and 0.5 mass % or less, or 0.02 mass % or more and 0.5 mass %.

[0047] The sintered body of the present embodiment may contain aluminum oxide, and preferably at least one zirconium oxide layer contains aluminum oxide. The aluminum oxide content of the sintered body of the present embodiment can be 0% by mass or more, as measured by the ratio of the mass of aluminum oxide to the mass of the sintered body, and can be 0% by mass or more and 0.15% by mass or less, further 0% by mass or more and 0.10% by mass or less, and further 0% by mass or more and 0.07% by mass or less. In the case of containing aluminum oxide, for example, the lower limit of the aluminum oxide content exceeds 0% by mass, preferably 0.005% by mass or more or 0.01% by mass or more; the upper limit of the aluminum oxide content can be 0.15% by mass or less, 0.10% by mass or less, or 0.07% by mass or less. These upper and lower limits can be any combination. Therefore, the aluminum oxide content can be, for example, more than 0% by mass and less than 0.15% by mass, 0.005% by mass or more and 0.10% by mass or less, or 0.01% by mass or more and 0.07% by mass or less. The alumina content of each zirconia layer can be exemplified as being in the same range as above. The alumina content of each zirconia layer sometimes affects the thermal shrinkage behavior in the pre-sintering stage. The alumina content of each zirconia layer is arbitrary, and the alumina content of each zirconia layer can be different, but preferably the alumina content is equal. In the case where the alumina content of the zirconia layers is different from each other, for example, it can be exemplified that the lower limit of the difference in alumina content of adjacent zirconia layers exceeds 0 mass%, and further is 0.005 mass% or more, and the upper limit of the difference in alumina content of adjacent zirconia layers is 0.15 mass% or less, 0.1 mass% or less, 0.03 mass% or less, or 0.01 mass% or less. These upper and lower limits can be any combination. Therefore, the difference in alumina content of adjacent zirconia layers can be exemplified as exceeding 0 mass% and 0.15 mass% or less, exceeding 0 mass% and 0.1 mass% or less, exceeding 0 mass% and 0.03 mass% or less, or 0.005 mass% or more and 0.01 mass% or less. For example, in the case of a zirconium oxide layer composed of zirconium oxide containing aluminum oxide (Al2O3), a non-coloring stabilizing element of yttrium (Y2O3) and a coloring stabilizing element of erbium (Er2O3), the aluminum oxide content can be calculated as {Al2O3 / (ZrO2+Y2O3+Er2O3+Al2O3)}×100 (mass %). The sintered body of the present embodiment preferably does not substantially contain silicon dioxide (SiO 2 ), and more preferably contains silicon dioxide below the detection limit.

[0048] The sintered body of the present embodiment preferably includes at least a zirconium oxide layer containing zirconium oxide whose crystal phase is at least one of tetragonal (T phase) and cubic (C phase), more preferably includes at least a zirconium oxide layer containing zirconium oxide whose main phase is tetragonal, and further preferably includes a zirconium oxide layer containing zirconium oxide whose main phase is tetragonal and a zirconium oxide layer containing zirconium oxide whose main phase is cubic. It should be noted that the "main phase" in the present embodiment refers to the crystal phase with the largest proportion (ratio of the integrated intensity of the peak) in the crystal phase of zirconium oxide. The existence ratio can be obtained from the XRD spectrum of the sintered body surface. As measurement conditions of the XRD pattern of the sintered body surface, the following conditions can be exemplified. Radiation source: Cu Kα ray Measurement mode: Continuous scanning Scanning speed: 4° / min Measuring range: 2θ = 26° to 33° Accelerating voltage and current: 40mA and 40kV Divergence longitudinal limiting slit: 10mm Divergence / entrance slit: 1° Light receiving slit: open Detector: Semiconductor detector (D / teX Ultra) Filter: Ni filter Goniometer radius: 185mm The obtained XRD spectrum is smoothed and background-subtracted, and the profile is fitted using a segmented pseudo-Voigt function to obtain the ratio of tetragonal and cubic crystals (ratio of the integrated intensity of the peak), and the crystalline phase with a high ratio is used as the main phase. The measurement and fitting of the XRD spectrum can be performed by a general powder X-ray diffraction device (e.g., Ultima IV, manufactured by RIGAKU) and an analysis program attached to the X-ray diffraction device (e.g., comprehensive powder X-ray analysis software PDXLVer.2.2, manufactured by RIGAKU).

[0049] <Characteristics of sintered body and each zirconia layer constituting the sintered body (each sintered body layer)> Figure 1 The sintered body (100) shows the thickness of the first layer, the third layer, and the second layer to the same extent. However, the thickness of each layer of the sintered body of the present embodiment (also referred to as "layer thickness") may be different from each other, and the thickness of any of the first to third layers may be thicker. For example, as the layer thickness of the first to third layers, the lower limit of the layer thickness may be 1 mm or more, further 2 mm or more, further 3 mm or more, and the upper limit of the layer thickness may be 20 mm or less, further 15 mm or less, and further 10 mm or less. These upper and lower limits may be any combination. Therefore, as the layer thickness of the first to third layers, for example, 1 mm or more and 20 mm or less, further 2 mm or more and 15 mm or less, and further 3 mm or more and 10 mm or less may be cited. More specifically, in Figure 1 In the sintered body, the first layer preferably has a thickness of 0.5 mm to 10 mm, the second layer preferably has a thickness of 0.5 mm to 10 mm, and the third layer preferably has a thickness of 1 mm to 20 mm. In addition, Figure 2 In the sintered body, the first layer preferably has a thickness of 0.5 mm to 10 mm, and the second layer preferably has a thickness of 0.5 mm to 10 mm. The thickness of each layer in the intermediate layer is preferably 1 mm to 10 mm.

[0050] The shape of the sintered body of this embodiment can be any shape corresponding to the purpose, as long as it is at least one selected from spherical, elliptical, disc-shaped, cylindrical, cubic, rectangular and polyhedral; or a shape suitable for dental materials represented by dental restoration materials such as crowns, bridges, onlays and inlays; or any shape suitable for other purposes. In addition, in this embodiment, the spherical shape can include nearly spherical shapes other than a perfect sphere, such as a roughly spherical shape, and the polyhedral shape can include nearly polyhedral shapes other than a polyhedron, such as a roughly polyhedral shape. The size of the sintered body of the present embodiment is arbitrary, and examples thereof include a length of 10 mm or more and 120 mm or less, a width of 12 mm or more and 120 mm or less, and a height of 6 mm or more and 40 mm or less. In addition, the thickness of the sintered body in the stacking direction of the sintered body of the present embodiment, that is, the height of the sintered body, is arbitrary, and examples thereof include a thickness of 4 mm or more and 40 mm or less, and further a thickness of 5 mm or more and 30 mm or less.

[0051] <<Warp and deformation of sintered body>> The sintered body of the present embodiment preferably has a warpage (hereinafter also referred to as "warpage") measured using a thickness gauge (hereinafter also referred to as "feeler gauge") in accordance with JIS B 7524:2008 of 1.0 mm or less. The sintered body having a structure with three or more zirconium oxide layers is sintered to have a shape that is warped in the stacking direction (or in the opposite direction to the stacking direction). When such a sintered body is placed on a horizontal plate, a gap is formed between the sintered body and the horizontal plate. The warpage in the present embodiment is a value measured using a feeler gauge. The warpage of the sintered body of the present embodiment is preferably less than 0.3 mm, less than 0.2 mm, less than 0.1 mm, or less than 0.05 mm. The sintered body preferably has no warpage (warpage is 0 mm), but the sintered body of the present embodiment may also have a warpage that cannot be measured with a feeler gauge (warpage is more than 0 mm). The sintered body of the present embodiment may exemplify a warpage of more than 0 mm, and further more than 0.01 mm. The warpage is preferably less than 0.06 mm, more preferably less than 0.05 mm, and further preferably less than the measurement limit (less than 0.03 mm). The warpage can be measured by the maximum value of the thickness of a feeler gauge that can be inserted into the gap formed in a state where the convex portion of the sintered body is arranged in contact with the horizontal plate. The warpage of the sintered body of the present embodiment can be 0 mm or more and 0.3 mm or less, 0 mm or more and 0.05 mm or less, 0 mm or more and less than 0.03 mm, or more than 0 mm and less than 0.03 mm.

[0052] Figure 5Schematic diagram showing a method for measuring warpage. The sintered body (500) shows a cross section of a disk-shaped sample, showing a sintered body in a state of warpage in the stacking direction (Y-axis direction). Figure 5 In the figure, the warpage of the sintered body (500) is emphasized for illustration. Figure 5 As shown, when measuring the warpage, the convex part of the sintered body (500) with a concave-convex shape is arranged in such a way that the convex part is in contact with the horizontal plate (51). As a result, a gap is formed between the surface where the sintered body (500) and the horizontal plate (51) are in contact (hereinafter also referred to as the "bottom surface") and the horizontal plate (51). A feeler gauge is inserted into the gap, and the warpage can be measured with the maximum value of the thickness of the feeler gauge that can be inserted. Figure 5 In the figure, the feeler gauge (52A) is shown as being located below the bottom surface of the sintered body (500) and inserted into the gap; on the other hand, the feeler gauge (52B) is shown as not being located below the bottom surface of the sintered body (500) and not being inserted into the gap. Figure 5 The feeler gauge (52A) and the feeler gauge (52B) in the figure are feeler gauges with a thickness difference of one level (e.g., 0.01 mm) from each other, and the warpage of the sintered body (500) is the thickness of the feeler gauge (52A). Figure 5 , a figure showing both a feeler gauge (52A) and a feeler gauge (52B) inserted therein is shown, but the warpage can be measured by inserting the feeler gauges into the gap in order from the thinnest one (for example, after measuring with the feeler gauge (52A), it is removed and then the measurement is performed with the thicker feeler gauge (52B)).

[0053] The sintered body of the present embodiment preferably has a warpage (hereinafter also referred to as "deformation") of 1.0 or less, 0.5 or less, 0.2 or less, or 0.15 or less relative to the size of the sintered body. The deformation amount can be 0 or more, further 0.01 or more, and further 0.05 or more. The deformation amount may be 0 or more and 1.0 or less, 0 or more and 0.15 or less, 0.01 or more and 1.0 or less, or 0.05 or more and 0.15 or less. The deformation amount can be calculated by the following formula (2). Deformation amount = (warpage: mm) / (sintered body size: mm) × 100···(2) The size of the sintered body is the size of the sintered body in the direction perpendicular to the warping direction. Figure 5The sintered body (500) is along the stacking direction (Y-axis direction), so the size of the sintered body (500) is the size of the sintered body (53) in the horizontal direction (X-axis direction) perpendicular to the stacking direction. The size can be measured by a known measurement method using a vernier caliper or a micrometer. For example, in the case of a disc-shaped or cylindrical stack, the size of the sintered body represents the diameter of the sintered body. In the case of a disc-shaped or cylindrical stack, the size of the sintered body can be measured using a vernier caliper. For example, the diameter of the upper end and the diameter of the lower end can be measured at 4 points each, and the average value of the diameters of the upper end and the lower end can be obtained, and the average value of the obtained values ​​is used as the size of the stack. In the present embodiment, the warpage and deformation amounts are preferably values ​​measured using a disk-shaped sample as a measurement sample, and more preferably values ​​measured using a disk-shaped sample having a diameter of 5 mm to 120 mm. For example, when the diameter of the sintered body is 105 mm and the warpage is 0.2 mm, the deformation amount is 0.2 / 105×100=0.19.

[0054] <<Density of sintered body>> The lower limit of the density of the sintered body of the present embodiment measured by the method based on JIS R 1634 is 5.7 g / cm 3 Above or 5.9g / cm 3 The upper limit of density is 6.3 g / cm 3 Below or 6.1g / cm 3 These upper and lower limits may be any combination. Therefore, the density of the sintered body of this embodiment can be exemplified as 5.7 g / cm 3 Above and 6.3g / cm 3 Below, preferably 5.9 g / cm 3 Above and 6.1g / cm 3 The density in this range corresponds to 99% or more as a relative density, and is a density of a so-called dense sintered body having practical strength.

[0055] <<Color tone of sintered body or sintered body layer>> The color tone of the sintered body or each zirconium oxide layer (each sintered body layer) of the present embodiment can be determined by, for example, * a * b * The color tone of the sintered body or each zirconium oxide layer (each sintered body layer) of the present embodiment can be exemplified as: * a * b * Lightness L in the color system *The lower limit of L is 50 or above or 55 or above. * The upper limit value is below 80 or below 70; hue a * The lower limit of the value is -5 or above or -3 or above, the hue a * The upper limit value is 15 or less or 10 or less; and the hue b * The lower limit of 0 or more or 3 or more, hue b * The upper limit value is 45 or less or 35 or less. These upper limits and lower limits may be any combination. Therefore, the color tone of the sintered body or each zirconium oxide layer (each sintered body layer) of this embodiment can be exemplified as: L * a * b * Lightness L in the color system * 50 or more and 80 or less, or 55 or more and 70 or less, hue a * is greater than -5 and less than 15, or greater than -3 and less than 10, and the hue b * It is 0 or more and 45 or less, or 3 or more and 35 or less. When the color tone is within this range, the sintered body exhibits a color tone similar to that of natural teeth.

[0056] The sintered body of this embodiment has a change in color tone, so it is preferable that the chroma C between adjacent layers along the stacking direction is * Different. Chroma C * Is an indicator of brightness, represented by L * a * b * Hue a shown in the color system * and b * , through C * ={(a * ) 2 +(b * ) 2} 0.5 The chroma C between adjacent layers can be calculated as follows: * The absolute value of the difference (△C * ) has a lower limit of 0.1 or more, 0.3 or more, 1.0 or more, or 1.5 or more, and an absolute value (△C * ) has an upper limit of 20.0 or less, 15.0 or less, 10.0 or less, or 5.0 or less. These upper and lower limits may be any combination. * The absolute value of the difference (△C * ) can be exemplified as 0.1 to 20.0, 0.3 to 15.0, 1.0 to 10.0, or 1.5 to 5.0. * Within this range, a laminated body can be visually recognized as having a gradation of brightness close to that of natural teeth. Similarly, the brightness L between adjacent layers can be exemplified as * The absolute value of the difference (△L * ) has a lower limit of 1.0 or more, and further has a lower limit of 1.5 or more, and the absolute value (△L * ) has an upper limit of 30.0 or less, and further has an upper limit of 15.0 or less. These upper and lower limits may be any combination. Therefore, the sintered body of this embodiment can exemplify the brightness L between adjacent layers. * The absolute value of the difference (△L * ) is 1.0 or more and 30.0 or less, and further is 1.5 or more and 15.0 or less. Hue (L * 、a * and b * ) and C * It can be obtained using a colorimetric colorimeter (for example, ZE6000, manufactured by Nippon Denshoku Industries Co., Ltd.) equipped with an illumination and light receiving optical system in accordance with geometric conditions c of JIS Z 8722. * The specific measurement conditions are as follows in the method of measuring with a zero correction box on the measurement sample (so-called black background measurement). Regarding the color tone of the sintered body of this embodiment, any part of the sintered body is cut out in the horizontal direction and the measurement sample is processed into a sample thickness of 2.8±0.1mm for measurement. Light source: D65 light source Viewing angle: 2° Measurement method: SCI

[0057] <<Transmittance of sintered body or sintered body layer>> The sintered body of the present embodiment preferably includes at least a zirconium oxide layer having a sense of light transmission. It is further preferred that the zirconium oxide layer has a total light transmittance (hereinafter, also referred to as "total light transmittance") relative to the CIE standard light source D65 when the sample thickness is 1.0±0.1mm as follows: the lower limit of the total light transmittance is 15% or more, 20% or more, 30% or more, 32% or more, or 35% or more, and the upper limit of the total light transmittance is 50% or less, 45% or less, or 42% or less. These upper and lower limits can be any combination. Therefore, the sintered body of the present embodiment preferably has a zirconium oxide layer having a total light transmittance of, for example, 15% or more and 50% or less, further 20% or more and 45% or less, and further 32% or more and 42% or less. The wavelength of light absorbed by the sintered body of the present embodiment is different due to its color development. Therefore, as an indicator of light transmittance, the total light transmittance relative to light containing different wavelengths such as the CIE standard light source D65 is appropriate. In the sintered body of the present embodiment, the lower limit of the difference in total light transmittance between adjacent stacked zirconium oxide layers is preferably 1% or more or 1.5% or more, and the upper limit of the difference in total light transmittance is preferably 10% or less or 5% or less. These upper and lower limits may be any combination. Therefore, in the sintered body of the present embodiment, the difference in total light transmittance between adjacent stacked zirconium oxide layers is preferably, for example, 1% or more and 10% or less, or 1.5% or more and 5% or less.

[0058] The total light transmittance can be measured by a method based on JIS K 7361, and the CIE standard light source D65 is used as the incident light, and the value of the transmittance obtained by summing the diffuse transmittance and the linear transmittance relative to the incident light is obtained. An arbitrary part of the sintered body is cut out in the horizontal direction, and it is made into a sample with a thickness of 1.0±0.1mm and a surface roughness (Ra) ≤0.02μm. The sample is irradiated with light of the CIE standard light source D65 using a conventional turbidity meter (fog meter; for example, NDH4000, manufactured by Nippon Denshoku Industries), and the transmitted light is focused using an integrating sphere, thereby measuring the transmittance (diffuse transmittance and linear transmittance) of the sample, and it can be used as the total light transmittance.

[0059] <<Three-point bending strength of sintered body layer>> The three-point bending strength of each zirconium oxide layer (each sintered body layer) in the sintered body of the present embodiment is more preferably 500 MPa or more, 550 MPa or more, or 600 MPa or more as measured by a method based on JIS R 1601. The three-point bending strength can be exemplified as less than 1200 MPa, and further 1160 MPa or less. The preferred three-point bending strength is 500 MPa or more and less than 1200 MPa, 550 MPa or more and 1160 MPa or less, or 600 MPa or more and 1160 MPa or less. Figure 6 Schematic diagram showing the measurement of the three-point bending strength of the zirconium oxide layer (sintered body layer) (600). Figure 6 In the figure, the stacking direction is represented as the Y-axis direction, and the horizontal direction is represented as the X-axis direction. The test specimen for the three-point bending strength measurement is a rectangular parallelepiped sintered body made with the thickness as the stacking direction and the width and length as the horizontal directions. Figure 6As shown, the three-point bending strength can be measured by applying a load (61) perpendicularly to the length of the measurement sample (600). The measurement sample can be configured in such a way that the load (61) is applied to the middle of the distance between the fulcrums (62). In the measurement of the three-point bending strength, a columnar sintered body with a distance between the fulcrums of 30 mm, a width of 4 mm, and a thickness of 3 mm is used as the measurement sample, the crosshead speed is set to 0.5 mm / min, and the measurement is performed 10 times. The average value obtained is used as the three-point bending strength of the zirconium oxide layer (sintered body layer) involved in this embodiment.

[0060] Next, the pre-sintered body will be described below, focusing on the differences from the above-mentioned sintered body.

[0061] (Pre-sintered body) The pre-sintered body involved in this embodiment is: A pre-sintered body of a zirconium oxide composition, wherein The zirconium oxide composition contains (iii) a zirconium oxide composition containing a stabilizing element having a neck structure, or contains (iv) a zirconium oxide composition containing a zirconium oxide containing a stabilizing element having a neck structure and a coloring element. Furthermore, the pre-sintered body has three or more regions stacked in layers, and the contents of at least one of the stabilizing element and the coloring element are different in two adjacent regions among the regions. In the stacked regions, a difference in content of the stabilizing element contained in a first region located at one end and a difference in content of the stabilizing element contained in a second region located at the other end is 2.0 mol % or less. In addition, the pre-sintered body according to another aspect of the present embodiment is: A pre-sintered body of a zirconium oxide composition, wherein The zirconium oxide composition contains (iii) a zirconium oxide composition containing a stabilizing element having a neck structure, or contains (iv) a zirconium oxide composition containing a zirconium oxide containing a stabilizing element having a neck structure and a coloring element. Furthermore, the pre-sintered body has three or more regions stacked in layers, and the contents of at least one of the stabilizing element and the coloring element are different in two adjacent regions among the regions. In the stacked regions, the difference in shrinkage rate between the pre-sintered body in the first region located at one end and the pre-sintered body in the second region located at the other end (shrinkage rate difference) is 0.4% or less.

[0062] The pre-sintered body is a laminated body including a structure having a neck structure (so-called pre-sintered particles). The pre-sintered body can be processed as needed and provided as a precursor of a sintered body. It is also called a preliminary sintered body, a soft sintered body, or a semi-sintered body. The necking structure is the structure of zirconium oxide after heat treatment below the sintering temperature, which is a structure formed by chemical adhesion between zirconium oxide particles. Figure 7 As shown, the zirconium oxide (71) contained in the zirconium oxide composition layer of the pre-sintered body can be confirmed as a part of the particle shape of the zirconium oxide in the powder composition. In this embodiment, the structure having the neck structure is a structure composed of zirconium oxide in the initial stage of sintering. This is different from the sintered structure, that is, the structure composed of zirconium oxide grains in the later stage of sintering. Therefore, the pre-sintered body of the present embodiment can be regarded as a stack of three or more zirconium oxide composition layers including "zirconium oxide particles with a neck structure containing zirconium oxide containing a stabilizing element"; or in the case of containing a coloring element, the pre-sintered body of the present embodiment can also be regarded as a stack of three or more zirconium oxide composition layers including zirconium oxide and a coloring element, wherein the zirconium oxide contained in the zirconium oxide composition layer includes zirconium oxide particles with a neck structure containing zirconium oxide containing a stabilizing element. The pre-sintered body has a zirconium oxide composition layer containing zirconium oxide with a neck structure and a stabilizing element instead of the zirconium oxide layer; or, in the case of containing a coloring element, has a zirconium oxide composition layer containing zirconium oxide with a neck structure and a stabilizing element and a coloring element (hereinafter, these zirconium oxide composition layers are collectively referred to as "zirconium oxide composition layers" or "composition layers"). With Figure 1 or Figure 2 In the pre-sintered body, the stabilizing element and the coloring element may be in the state of solid solution in the zirconium oxide, or in the state of oxide or its precursor. It should be noted that, in the present specification, the zirconium oxide composition layer is also referred to as a pre-sintered body layer.

[0063] <Features of the laminated structure> Preferred embodiments of the pre-sintered body of the present disclosure include a pre-sintered body described in the following embodiment (C) and a pre-sintered body described in the following embodiment (D).

[0064] <<Method (C)>> In the pre-sintered body of the present embodiment, the difference in the content of the stabilizing element contained in the first region located at one end and the content of the stabilizing element contained in the second region located at the other end among the stacked regions is 2.0 mol % or less. use Figure 1 The method (C) is described below. Figure 1In the Y-axis direction (stacking direction), the contents of stabilizing elements contained in the first region (e.g., the first layer (11)) located at one end and the second region (e.g., the second layer (12)) located at the other end are set to close values ​​(specifically, less than 2.0 mol %). Thus, the difference in shrinkage between the first layer and the second layer is balanced with respect to the stacking direction Y of the pre-sintered body, and the warping of the pre-sintered body can be suppressed. As a result, the pre-sintered body of the present embodiment is a pre-sintered body with suppressed warping and less deformation. Moreover, such a pre-sintered body can effectively form a sintered body that has light transmittance close to that of natural teeth and a gradation of color tones when visually recognized, and has suppressed warping and less deformation. In this embodiment, only the relationship between the first region (e.g., the first layer (11)) located at one end and the second region (e.g., the second layer (12)) located at the other end is specified, but if the shrinkage rate of the regions (layers) located at the two end portions is adjusted, the warping of the pre-sintered body can be effectively suppressed. Therefore, for each layer of the intermediate layer arranged between the first layer (11) and the second layer (12), a zirconium oxide composition layer composed of an arbitrary composition can be stacked. In the pre-sintered body of the present embodiment, the difference between the content of the stabilizing element contained in the first region and the content of the stabilizing element contained in the second region is 2.0 mol% or less, preferably 1.8 mol% or less, more preferably 1.5 mol% or less, and further preferably 0.8 mol% or less. The difference between the content of the stabilizing element contained in the first region and the content of the stabilizing element contained in the second region is preferably small, for example, 0 mol% or more, more than 0 mol%, 0.1 mol% or more, or 0.3 mol% or more. The difference between the content of the stabilizing element contained in the first region and the content of the stabilizing element contained in the second region can be exemplified by 0 mol% or more and 2.0 mol% or less, more than 0 mol% and 1.8 mol% or less, 0.1 mol% or more and 1.5 mol% or more, or 0.3 mol% or more and 0.8 mol% or less.

[0065] <<Method (D)>> In the pre-sintered body of the present embodiment, the difference in shrinkage rate between the first region at one end and the second region at the other end in the stacked regions (shrinkage rate difference) is 0.4% or less.

[0066] use Figure 1 The method (D) is explained below. Figure 1 In the Y-axis direction (stacking direction), the shrinkage rates of the pre-sintered bodies of the first region (e.g., the first layer (11)) located at one end and the second region (e.g., the second layer (12)) located at the other end are set to close values ​​(specifically, less than 0.4%). Thus, the difference in shrinkage between the first layer and the second layer is balanced with respect to the stacking direction Y of the pre-sintered body, and the warping of the pre-sintered body can be suppressed. As a result, the pre-sintered body of the present embodiment is a pre-sintered body with suppressed warping and less deformation. Moreover, such a pre-sintered body can effectively form a sintered body that has light transmittance close to that of natural teeth and a gradation of color tones when visually recognized, and has suppressed warping and less deformation. In the present disclosure, only the relationship between the first region (e.g., the first layer (11)) located at one end and the second region (e.g., the second layer (12)) located at the other end is specified, but if the shrinkage rate of the regions (layers) located at the two end portions is adjusted, the warping of the pre-sintered body can be effectively suppressed. Therefore, for each layer of the intermediate layer arranged between the first layer (11) and the second layer (12), a zirconium oxide composition layer composed of an arbitrary composition can be stacked. In the pre-sintered body of the present embodiment, the difference between the shrinkage rate of the pre-sintered body in the first region and the shrinkage rate of the pre-sintered body in the second region is preferably 0.4% or less, 0.36% or less, 0.3% or less, or 0.2% or less. The difference between the shrinkage rate of the pre-sintered body in the first region and the shrinkage rate of the pre-sintered body in the second region is preferably small, for example, 0% or more, more than 0%, 0.01% or more, or 0.02% or more. The difference between the shrinkage rate of the pre-sintered body in the first region and the shrinkage rate of the pre-sintered body in the second region can be 0% or more and 0.4% or less, more than 0% and 0.36% or less, 0.01% or more and 0.3% or less, or 0.02% or more and 0.2% or less.

[0067] <<<Measurement method of shrinkage ratio>>> The shrinkage rates of the first region (eg, the first layer (11)) located at one end and the second region (eg, the second layer (12)) located at the other end are determined as follows. A raw material powder of zirconium oxide having the same composition as the first layer (11) and the second layer (12) is filled into a mold, and CIP treatment is performed after uniaxial press molding, thereby forming a powder composition layer as a sample for measuring shrinkage. The powder composition layer is pre-sintered at 800°C or higher and lower than 1200°C to obtain a zirconium oxide composition layer. The shrinkage of the zirconium oxide composition layer is determined by the method described in the [Evaluation method of shrinkage] described in the column << (B) method>> under the above (sintered body). In addition, when the shrinkage rate of the pre-sintered body is obtained, the method for preparing the sample and the pre-sintering conditions for measuring the shrinkage rate are as described above.

[0068] <Composition of Zirconia Composite Layer> The zirconium oxide contained in the calcined body is preferably a zirconium oxide formed by heat-treating zirconium oxide sol at a temperature lower than the sintering temperature, more preferably a zirconium oxide formed by heat-treating zirconium oxide sol obtained by hydrolyzing a zirconium compound at a temperature lower than the sintering temperature, and further preferably a zirconium oxide formed by heat-treating zirconium oxide sol obtained by hydrolyzing zirconium oxychloride at a temperature lower than the sintering temperature. The content of the stabilizing element in the zirconia containing the stabilizing element contained in the first composition layer (corresponding to the first region), the content of the stabilizing element in the zirconia containing the stabilizing element contained in the second composition layer (corresponding to the second region), and the content of the stabilizing element in the zirconia containing the stabilizing element contained in the composition layer of the third composition layer or the intermediate layer (corresponding to the third region) may be the same as the stabilizing element contents of the above-mentioned first layer, second layer and third layer (intermediate layer), respectively. The content of the stabilizing element in each composition layer in the pre-sintered body is arbitrary as long as it is the same as that of the sintered body layer of the present embodiment described above. More preferably, the pre-sintered body includes at least a zirconium oxide composition layer containing zirconium oxide having a main phase of tetragonal or cubic crystals.

[0069] <Characteristics of the Pre-sintered Body and Each Zirconium Oxide Composition Layer Constituting the Pre-sintered Body (Each Pre-sintered Body Layer)> The pre-sintered body preferably has a warpage of less than 1.0 mm, less than 0.5 mm, less than 0.3 mm, less than 0.2 mm, less than 0.1 mm or less than 0.05 mm. The pre-sintered body preferably has no warpage (warpage is 0 mm), but may also have a warpage that cannot be measured with a feeler gauge (warpage is more than 0 mm). The warpage of the pre-sintered body can be exemplified as more than 0 mm, and further more than 0.01 mm. The warpage is preferably less than 0.06 mm, more preferably less than 0.05 mm, and further preferably less than the measurement limit (less than 0.03 mm). The warpage of the pre-sintered body can be 0 mm or more and less than 0.3 mm, 0 mm or more and less than 0.05 mm, 0 mm or more and less than 0.03 mm, more than 0 mm and less than 0.03 mm. The deformation amount of the pre-sintered body is preferably 1.0 or less, 0.5 or less, 0.2 or less, or 0.15 or less. The deformation amount can be 0 or more, further 0.01 or more, and further 0.05 or more. The deformation amount can be 0 or more and 1.0 or less, 0 or more and 0.15 or less, 0.01 or more and 1.0 or less, or 0.05 or more and 0.15 or less.

[0070] The lower limit of the density of the pre-sintered body is 2.4 g / cm 3 Above or 3.1g / cm 3The upper limit of density is 3.7 g / cm 3 Below or 3.5g / cm 3 These upper and lower limits may be any combination. Therefore, the density of the pre-sintered body can be exemplified as 2.4 g / cm 3 Above and 3.7g / cm 3 Below, preferably 3.1 g / cm 3 Above and 3.5g / cm 3 The density in this range corresponds to a relative density of 40% to 60%. The pre-sintered body may be a laminated body having a strength suitable for processing such as CAD / CAM processing. The density of the pre-sintered body is determined from the mass determined by mass measurement and the volume determined by size measurement. The color tone of the zirconium oxide composition layer contained in the preliminary sintered body may be different from that of the sintered body (sintered body layer) obtained by sintering the preliminary sintered body.

[0071] The pre-sintered body and each composition layer (each pre-sintered body layer) are opaque, and the total light transmittance is 0%. However, in consideration of measurement errors, the total light transmittance can be exemplified as being 0% or more and 0.2% or less. The pre-sintered body and each composition layer (each pre-sintered body layer) only need to have a strength that is not prone to defects during processing such as CAD / CAM or cutting. For example, the Vickers hardness is 25 HV or more and 150 HV (= kgf / mm 2 ) or less, or 30HV or more and 130HV or less. The determination of Vickers hardness can be carried out using a conventional Vickers hardness tester (e.g., Q30A, manufactured by Qness) equipped with a diamond regular quadrangular pyramid indenter. During the determination, the indenter is statically pressed into the surface of the test sample, and the diagonal length of the indentation mark formed on the surface of the test sample is visually determined. The obtained diagonal length can be used to obtain the Vickers hardness by the following formula. Hv=F / {d 2 / 2sin(α / 2)} In the above formula, Hv is the Vickers hardness (HV), F is the measurement load (1 kgf), d is the diagonal length of the indentation mark (mm), and α is the angle between the opposing surfaces of the indenter (136°). As the measurement conditions of the Vickers hardness, the following conditions can be mentioned. Test sample: disc-shaped with a thickness of 2.0±0.5mm Measuring load: 1kgf Before measurement, the measurement sample may be pre-treated by cutting out an arbitrary portion of the pre-sintered body in the horizontal direction and grinding the measurement surface with #800 water-resistant abrasive paper to remove irregularities exceeding 0.1 mm.

[0072] The laminate of the present embodiment can be used for known uses of zirconium oxide such as decorative components, structural materials, and optical materials, but when the laminate is a sintered body, it can be suitable for use as a dental material such as a denture (e.g., a crown, a bridge, etc.), and a dental material including the sintered body of the present embodiment can be made. In addition, when the laminate is a pre-sintered body, it can be suitable for use as a precursor of a dental material such as a denture (e.g., a crown, a bridge, etc.), and can be provided as a dental restorative material such as a blank, a disk, a block, a mill blank, and their precursors. The laminate of the sintered body or pre-sintered body of the present embodiment can be used as a dental material. Next, a method for producing various laminated bodies (specifically, a sintered body, a pre-sintered body, and a molded body) according to the present embodiment will be described below.

[0073] (Method for producing sintered body and pre-sintered body) The method for producing the sintered body according to the present embodiment is as follows. A method for producing a sintered body, comprising: laminating three or more layers of a powder composition containing a raw material powder of zirconium oxide to obtain a molded body, and sintering the molded body at a temperature of 1200° C. to 1600° C.; The raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and, when containing a coloring element, the coloring element. In addition, another method for producing the sintered body according to the present embodiment is as follows. A method for producing a sintered body, comprising: laminating three or more layers of a powder composition containing a raw material powder of zirconium oxide to obtain a molded body, and pre-firing the molded body at 800° C. or higher and lower than 1200° C. to obtain a pre-sintered body; as well as A step of sintering the pre-sintered body at a temperature of 1200°C to 1600°C.

[0074] In addition, the method for producing the pre-sintered body according to the present embodiment is as follows. A method for producing a pre-sintered body, comprising: laminating three or more layers of a powder composition containing a raw material powder of zirconium oxide to obtain a molded body, and pre-calcining the molded body at a temperature of 800° C. or higher and lower than 1200° C. The raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and, when containing a coloring element, the coloring element.

[0075] The method for producing the molded body produced to produce the sintered body or the pre-sintered body is as follows. A method for producing a molded body, comprising: laminating three or more layers of a powder composition containing a raw material powder of zirconium oxide to produce a molded body; The raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and, when containing a coloring element, the coloring element. It should be noted that, in the present specification, the powder composition layer is also referred to as a molded body layer.

[0076] Regarding the molded body used in the production method of the present embodiment, main features different from the above-mentioned sintered body will be described below. The molded body provided in the manufacturing method of this embodiment is formed by stacking three or more layers of powder composition layers including raw material powder of zirconium oxide containing a stabilizing element, or, when containing a coloring element, including raw material powder of zirconium oxide containing a stabilizing element and zirconium oxide containing a coloring element.

[0077] The compact is a laminated body in which powder composition layers are laminated, and the compact can be provided as a pre-sintered body or a precursor of a sintered body. The molded body has a powder composition layer containing a powder composition of zirconium oxide containing a stabilizing element instead of a zirconium oxide layer, or, when containing a coloring element, has a powder composition layer containing a powder composition of zirconium oxide containing a stabilizing element and a coloring element (hereinafter, these powder composition layers are collectively referred to as "powder layers"). With Figure 1 or Figure 2 The stacked structure shown is equivalent to the structure. Therefore, the molded body can also be regarded as a laminated body having three or more layers of powder containing zirconium oxide, wherein the powder of zirconium oxide contains a stabilizing element. In the molded body, the stabilizing element and the coloring element may be in a state of solid solution in zirconium oxide, or in a state of an oxide or a precursor thereof. As a precursor, one or more selected from sulfides, chlorides, nitrates, sulfates, hydroxides and oxyhydroxides may be exemplified, and one or more selected from chlorides, hydroxides and oxyhydroxides may be further exemplified. In addition, the coloring element preferably contains at least an oxide.

[0078] The zirconium oxide contained in the powder layer is preferably zirconium oxide obtained by heat-treating zirconium oxide sol, more preferably zirconium oxide obtained by heat-treating zirconium oxide sol obtained by hydrolyzing a zirconium compound, and further preferably zirconium oxide obtained by heat-treating zirconium oxide sol obtained by hydrolyzing zirconium oxychloride.

[0079] The zirconium oxide contained in the powder layer is preferably zirconium oxide powder. The lower limit of the average particle size of the zirconium oxide powder is preferably 0.3 μm or more or 0.4 μm or more, and the upper limit of the average particle size is preferably 0.7 μm or less or 0.5 μm or less. These upper and lower limits may be any combination. Therefore, the average particle size of the zirconium oxide powder is preferably, for example, 0.3 μm or more and 0.7 μm or less, or 0.4 μm or more and 0.5 μm or less.

[0080] The BET specific surface area of ​​the zirconium oxide powder is preferably 7.5 m 2 / g or more and 15m 2 / g or less. When the BET specific surface area is less than this range, the sintering speed becomes too slow; on the other hand, when the BET specific surface area exceeds this range, the sintering speed becomes too fast. In either case, it is difficult to densify in normal pressure sintering, especially in air sintering. Since there is a tendency to promote densification even in the case of sintering with a fast heating rate, the lower limit of the BET specific surface area is preferably 8m 2 / g or more, 9m 2 / g or above, or 9.5m 2 / g or more, and the upper limit of the BET specific surface area is preferably 15m 2 / g or less, 13m 2 / g or less, or 11m 2 / g or less. These upper and lower limits may be any combination. Therefore, the BET specific surface area of ​​the zirconium oxide powder is preferably 8m 2 / g or more and 15m 2 / g or less, 9m 2 / g or more and 13m 2 / g or less, or 9.5m 2 / g or more and 11m 2 / g or less. In the present embodiment, the BET specific surface area is a BET specific surface area measured in accordance with JIS R 1626, and may be measured by a BET five-point method based on a carrier gas method using nitrogen as an adsorption gas. Specific measurement conditions for the BET specific surface area include the following conditions.

[0081] [Measurement conditions of BET specific surface area] Adsorption medium: N2 Adsorption temperature: -196℃ Pretreatment conditions: Degassing treatment at 250°C for more than 1 hour in the atmosphere The BET specific surface area can be measured using a conventional apparatus (for example, TRISTAR II 3020, manufactured by Shimadzu Corporation).

[0082] The coloring element contained in the powder layer is preferably in at least one of a state of being mixed with the zirconium oxide powder and a state of being solid-dissolved in the zirconium oxide. Alternatively, the coloring element powder and the zirconium oxide powder may be mixed.

[0083] The molded body may contain a binder. By containing a binder, the shape retention of the molded body is improved. The binder contained in the molded body can use a known binder used for molding ceramics, preferably an organic binder. As an organic binder, it is one or more selected from polyvinyl alcohol, polyvinyl butyral, wax and acrylic resin, preferably one or more selected from polyvinyl alcohol and acrylic resin, and more preferably an acrylic resin. In the present embodiment, the acrylic resin is a polymer containing at least any one of acrylate and methacrylate. As a specific acrylic resin, one or more selected from polyacrylic acid, polymethacrylic acid, acrylic copolymer and methacrylic acid copolymer, and their derivatives can be exemplified. As a specific binder of the acrylic resin, an acrylic resin used for ceramic powder can be exemplified, and further one or more selected from AS-1100, AS-1800 and AS-2000 can be exemplified (all product names. Manufactured by Toagosei Co., Ltd.).

[0084] The content of the stabilizing element in the zirconia containing the stabilizing element contained in the first powder layer, the content of the stabilizing element in the zirconia containing the stabilizing element contained in the second powder layer, and the content of the stabilizing element in the zirconia containing the stabilizing element contained in the third powder layer may be the same as the stabilizing element contents of the above-mentioned first layer, second layer, and third layer (middle layer), respectively. The contents of the stabilizing element and the coloring element in each powder layer in the molded body are arbitrary as long as they are the same as those of the sintered body of the present embodiment described above.

[0085] In the case where each powder layer contains a binder, from the viewpoint of suppressing defects during molding, the lower limit of the content of the binder in each powder layer is preferably 1.5% by mass or more, 1.5% by mass or more, 2.0% by mass or more, or 2.5% by mass or more, and the upper limit is preferably 8.0% by mass or less, 6.0% by mass or less, or 5.5% by mass or less. These upper and lower limits can be any combination. Therefore, the content of the binder in each powder layer is, for example, preferably 1.5% by mass or more and 8.0% by mass or less, 2.0% by mass or more and 6.0% by mass or less, or 2.5% by mass or more and 5.5% by mass or less. The binder content is the mass ratio of the binder to the mass of the substance after removing the binder from the powder composition in the powder layer ({binder / (powder composition-binder)}×100). For example, when manufacturing a powder composition, the total mass of the constituent components of the powder composition other than the binder (for example, stabilizing elements, zirconium oxide and aluminum oxide after oxide conversion) is calculated, and then the mass ratio of the target binder to the total mass is calculated to manufacture the powder composition.

[0086] From the perspective of operability, the powder composition contained in the powder layer is preferably zirconium oxide powder, a coloring element when containing a coloring element, and a powder in a granulated state of a binder when containing a binder (hereinafter also referred to as "granulated powder"), and more preferably a granulated powder granulated into granules by spray drying or the like (hereinafter also referred to as "powder particles"). The particle size of the granulated powder is arbitrary, and as the average aggregation diameter (hereinafter, also referred to as the "average particle diameter"), the lower limit can be 1 μm or more or 5 μm or more, and the upper limit can be 150 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. These upper and lower limits can be any combination. Therefore, with respect to the particle size of the granulated powder, as the average aggregation diameter, 1 μm or more and 150 μm or less, 1 μm or more and 100 μm or less, 5 μm or more and 50 μm or less, or 5 μm or more and 30 μm or less can be exemplified. As other embodiments, 20 μm or more and 50 μm or less can be exemplified. In the present embodiment, the average aggregation diameter is a diameter corresponding to the cumulative 50% in the volume particle size distribution measurement. The volume particle size distribution is a value that can be measured using a general-purpose device (eg, MT3100II, manufactured by Microtrac BEL), and is the volume diameter of approximately spherical particles. As a pretreatment, the granulated powder may be sieved with a sieve having an opening of 125 μm before measurement, and the granulated powder that has passed the sieve may be measured.

[0087] The molded body preferably includes at least a powder layer containing zirconium oxide having a tetragonal or cubic crystal as a main phase.

[0088] The molded body preferably has a warpage of less than 1.0 mm, less than 0.3 mm, less than 0.2 mm, less than 0.1 mm, or less than 0.05 mm. The molded body preferably has no warpage (warpage is 0 mm), but may also have a warpage that cannot be measured with a feeler gauge (warpage is more than 0 mm). The molded body may exemplify a warpage of more than 0 mm, and further more than 0.01 mm. The warpage is preferably less than 0.06 mm, more preferably less than 0.05 mm, and further preferably less than the measurement limit (less than 0.03 mm). The warpage of the molded body may be 0 mm or more and less than 0.06 mm, 0 mm or more and less than 0.05 mm, 0 mm or more and less than 0.03 mm, or more than 0 mm and less than 0.03 mm. The deformation amount of the molded body is preferably 1.0 or less, 0.5 or less, 0.2 or less, or 0.15 or less. The deformation amount can be 0 or more, further 0.01 or more, and further 0.05 or more. The deformation amount can be 0 or more and 1.0 or less, 0 or more and 0.15 or less, 0.01 or more and 1.0 or less, or 0.05 or more and 0.2 or less.

[0089] The lower limit of the density of the molded product can be exemplified as 2.4 g / cm 3 Above or 3.1g / cm 3 The upper limit of the density can be exemplified as 3.7 g / cm 3 Below or 3.5g / cm 3 These upper and lower limits may be any combination. Therefore, the density of the molded body can be exemplified as 2.4 g / cm 3 Above and 3.7g / cm 3 Below, or 3.1g / cm 3 Above and 3.5g / cm 3 The density in this range corresponds to a relative density of 40% to 60%. It should be noted that the density of the molded body may be approximately the same as that of the pre-sintered body. The density of the molded body was determined from the mass determined by mass measurement and the volume determined by size measurement.

[0090] The color tone of the zirconium oxide powder composition layer (molded body layer) contained in the molded body may be different from that of the sintered body (sintered body layer) obtained by sintering the molded body, or may not have a change in color tone. The molded body and each powder layer are opaque, and the total light transmittance is 0%. However, in consideration of measurement errors, the total light transmittance can be exemplified as being 0% or more and 0.2% or less.

[0091] The molded body may have a strength sufficient to prevent cracks or chips from occurring during calcination or sintering.

[0092] The molded body is obtained by stacking the powder composition and molding it. Each powder composition can be obtained by mixing zirconium oxide powder and a binder in the case of containing a binder in a desired arbitrary ratio using a known method. Preferably, the molding is press molding. For example, a powder composition having a composition corresponding to the bottom layer is filled in a molding die as the bottom layer. Afterwards, a powder composition having a composition corresponding to the composition of the adjacent layer of the bottom layer is filled on the bottom layer. In the case of a molded body having a structure stacked with more than 3 layers of powder layers, as long as the same operation is repeated, the necessary powder composition is stacked. After filling the powder composition having a composition corresponding to the composition of the top layer, uniaxial press molding is performed at an arbitrary pressure to obtain a preliminary molded body, which is subjected to CIP treatment to obtain a molded body. When stacking, there is no need to apply vibration using a vibrator to form a mixed layer between layers. In addition, uniaxial press molding is preferably performed after filling the powder composition having a composition corresponding to the top layer, and preferably not pressurized before filling the powder composition having a composition corresponding to the top layer.

[0093] The molding pressure of uniaxial pressure molding is preferably 15 MPa or more and 200 MPa or less, and more preferably 18 MPa or more and 100 MPa or less. Uniaxial pressure molding has a tendency to suppress the warping of the molded body as the molding pressure becomes higher. The pressure of CIP treatment can be 98 MPa or more and 392 MPa or less.

[0094] The molded body is treated at a temperature lower than the sintering temperature to form a pre-sintered body. A known method can be used for the pre-sintering method and pre-sintering conditions. As the holding temperature during pre-firing (hereinafter also referred to as "pre-firing temperature"), the lower limit may be 800°C or higher, 900°C or higher, or 950°C or higher, and the upper limit may be less than 1200°C, 1150°C or lower, or 1100°C or lower. These upper and lower limits may be any combination. Therefore, the pre-firing temperature may be, for example, 800°C or higher and less than 1200°C, preferably 900°C or higher and 1150°C or lower, and more preferably 950°C or higher and 1100°C or lower. The holding time at the calcination temperature (hereinafter also referred to as "calcination time") can be appropriately set according to the size of the molded body to be calcined, the characteristics of the calcination furnace, etc., and the lower limit is preferably 0.5 hours or more, more preferably 0.5 hours or more, and the upper limit is preferably 5 hours or less, more preferably 3 hours or less. These upper and lower limits can be any combination. Therefore, the calcination time is, for example, 0.5 hours or more and 5 hours or less, or 0.5 hours or more and 3 hours or less. It should be noted that the temperature increase, the temperature increase rate during the temperature increase, and the holding time at the increased temperature may be divided into a plurality of stages to increase the temperature. For example, pre-sintering can be performed under the following conditions: from room temperature to 300°C at 15°C / hour, maintained at 300°C for 5 hours, from 300°C to 700°C at 15°C / hour, maintained at 700°C for 1 hour, from 700°C to 1000°C at 50°C / hour, maintained at 1000°C for 2 hours. The atmosphere in the calcining step (hereinafter also referred to as "calcining atmosphere") is preferably an atmosphere other than a reducing atmosphere, more preferably at least one of an oxygen atmosphere and an air atmosphere, and still more preferably an air atmosphere.

[0095] In the manufacturing method of this embodiment, any one of the molded body and the pre-sintered body (hereinafter, they are also collectively referred to as "molded body, etc.") is treated at 1200° C. to 1600° C. Thus, the molded body, etc. becomes a sintered body. Before sintering, the molded body, etc. can be processed into any shape. The sintering method and sintering conditions can use known methods. As the sintering method, at least one selected from pressureless sintering, HIP treatment, SPS and vacuum sintering can be cited. In order to be widely used as an industrial sintering method, the sintering method is preferably pressureless sintering, and more preferably pressureless sintering under an atmospheric atmosphere. The sintering method is preferably only pressureless sintering, and more preferably pressure-sintering after pressureless sintering is not performed. Thus, the sintered body can be obtained as a pressureless sintered body. In the present embodiment, pressureless sintering refers to a method in which no external force is applied to the sintered object during sintering, and sintering is performed only by heating.

[0096] The lower limit of the holding temperature during sintering (hereinafter also referred to as "sintering temperature") is 1200°C or more, preferably 1300°C or more, 1400°C or more, 1430°C or more, or 1480°C or more, and the upper limit is 1650°C or less, preferably 1580°C or less, 1560°C or less, 1560°C or less, or 1560°C or less. These upper and lower limits may be any combination. Therefore, the sintering temperature is, for example, 1200°C or more and 1650°C or less, 1300°C or more and 1580°C or less, 1400°C or more and 1560°C or less, 1430°C or more and 1560°C or less, or 1480°C or more and 1560°C or less. In another embodiment, the sintering temperature is 1450°C or more and 1650°C or less, preferably 1500°C or more and 1650°C or less, and more preferably 1550°C or more and 1650°C or less. As the heating rate until the sintering temperature is reached, the lower limit can be 50°C / hour or more, 100°C / hour or more, or 150°C / hour or more, and the upper limit can be 800°C / hour or less or 700°C / hour or less. These upper and lower limits can be any combination. Therefore, the heating rate until the sintering temperature is reached is, for example, 50°C / hour or more and 800°C / hour or less, 100°C / hour or more and 800°C / hour or less, 150°C / hour or more and 800°C / hour or less, or 150°C / hour or more and 700°C / hour or less. As the holding time at the sintering temperature (hereinafter, also referred to as "sintering time".), it varies according to the sintering temperature, the size of the molded body, the characteristics of the sintering furnace, etc., but the preferred lower limit is more than 1 hour, and the upper limit is less than 5 hours, less than 3 hours or less than 2 hours. These upper and lower limits can be any combination. Therefore, the sintering time is, for example, more than 1 hour and less than 5 hours, more preferably more than 1 hour and less than 3 hours, and further preferably more than 1 hour and less than 2 hours. For example, sintering may be performed under the conditions of heating from room temperature to 1500° C. at 100° C. / hour and maintaining at 1500° C. for 2 hours. The sintering atmosphere (hereinafter also referred to as "sintering atmosphere") is preferably an atmosphere other than a reducing atmosphere, more preferably at least one of an oxygen atmosphere and an air atmosphere, and still more preferably an air atmosphere. The air atmosphere can be mainly composed of nitrogen and oxygen, with an oxygen concentration of about 18 to 23% by volume. Preferred sintering conditions in the sintering step include normal pressure sintering in an air atmosphere. Example

[0097] Hereinafter, the present disclosure will be described in more detail based on examples, but the present disclosure is not limited to these examples.

[0098] (BET specific surface area) The BET specific surface area was measured by a BET five-point method using an automatic specific surface area measuring device (device name: TriStar II 3020, manufactured by Shimadzu Corporation) in accordance with JIS R 1626. The measurement conditions are as follows. Adsorption medium: N2 Adsorption temperature: -196℃ Pretreatment conditions: Degassing treatment at 250°C for more than 1 hour in an air atmosphere

[0099] (Average particle diameter) The average particle diameter is measured by particle size distribution measurement using a Microtrac particle size distribution analyzer (device name: MT3100II, manufactured by Microtrac BEL) by a laser diffraction / scattering method. The measurement conditions are as follows. Light source: semiconductor laser (wavelength: 780nm) Voltage: 3mW Refractive index of zirconium oxide: 2.17 Calculation mode: MT3000 As a pretreatment, the granulated powder was sieved with a sieve having an opening of 125 μm before the measurement, and the granulated powder that passed through the sieve was measured.

[0100] (Warping and deformation) A disk-shaped molded body, a pre-sintered body or a sintered body was used as a measurement sample, and the respective deformation amounts were calculated from the following formula (3). Deformation = (warpage: mm) / (size: mm)×100···(3)

[0101] The method for calculating the deformation amount is further explained in detail. The conditions for producing the laminate are as follows. [Laminated body] Mould diameter: Φ110mm Powder mass: 470 g (total mass of layered powder) Molding pressure: Uniaxial pressing: 49MPa + CIP treatment: 196MPa Molding process: Load the raw material powder that forms the first layer into the mold → flatten → Load the raw material powder that forms the second layer into the mold → flatten → (repeat later) → uniaxial pressing → CIP treatment

[0102] In the preparation of the above-mentioned laminate, Figure 8 A diagram schematically showing the molding process of uniaxial press molding is shown. Fig. 9 A diagram schematically showing a molding process of a CIP treatment is shown. exist Figure 8 In the figure, the powder composition is pressurized by "(a) loading the powder composition (81) into the mold (82) → (b) flattening the powder composition → (c) (the second layer is also formed in the same way and repeated later), (d) uniaxial pressing (83)". exist Fig. 9 , a uniaxially pressed powder (laminated body) (91) is placed in a high-pressure container, the high-pressure container is filled with a solvent (92), and the powder is isotropically pressurized (CIP treatment).

[0103] By undergoing the CIP treatment, a molded body for measuring the warpage and deformation amount was obtained. The molded body was calcined under the following conditions to obtain a sintered body for measuring the warpage and deformation. The molded body was calcined and sintered under the following conditions to obtain a sintered body for measuring the warpage and deformation. [Pre-calcination and sintering conditions] Pre-sintering: from room temperature to 300°C at 15°C / hour, keep at 300°C for 5 hours, from 300°C to 700°C at 15°C / hour, keep at 700°C for 1 hour, from 700°C to 1000°C at 50°C / hour, keep at 1000°C for 2 hours, and then cool in the furnace. Sintering: 100°C / hour from room temperature to 1500°C, maintained at 1500°C for 2 hours, and then cooled in the furnace.

[0104] The warpage of the laminated bodies of the molded body, the pre-sintered body, and the sintered body was measured by Figure 5 The measurement method shown is used. The measurement sample is arranged in such a way that the convex part of the measurement sample is in contact with the horizontal plate. A feeler gauge (product name: 75A19, manufactured by Nagai Gauge Manufacturing Co., Ltd.) is inserted into the gap formed between the horizontal plate and the bottom surface to measure the warpage. The measurement is performed by inserting a feeler gauge arranged parallel to the horizontal plate into the gap formed between the horizontal plate and the bottom surface of the measurement sample, and measuring the feeler gauge thickness as the maximum thickness of the feeler gauge that can be inserted into the gap, and the feeler gauge thickness is taken as the warpage. It should be noted that the warpage is measured by a single feeler gauge or a combination of feeler gauges, starting from a feeler gauge thickness of 0.03 mm and sequentially at intervals of 0.01 mm. Regarding the dimensions of the measurement sample, the diameter of the upper end and the diameter of the lower end were measured at four points each using a vernier caliper, and the average value of the upper and lower end diameters was determined.

[0105] (Zirconium oxide powder A1) As the zirconium oxide powder A1, commercially available zirconium oxide powder Zpex Smile (manufactured by TOSOH Corporation) was used.

[0106] The zirconium oxide powder A1 was subjected to uniaxial press molding at a pressure of 49 MPa and CIP treatment at a pressure of 196 MPa to obtain a powder layer (molded body layer) of the zirconium oxide powder A1. The obtained powder layer (molded body layer) was calcined and sintered under the following conditions to obtain a zirconium oxide layer (sintered body layer). [Pre-calcination and sintering conditions] Pre-sintering: from room temperature to 300°C at 15°C / hour, keep at 300°C for 5 hours, from 300°C to 700°C at 15°C / hour, keep at 700°C for 1 hour, from 700°C to 1000°C at 50°C / hour, keep at 1000°C for 2 hours, and then cool in the furnace. Sintering: 100°C / hour from room temperature to 1500°C, maintained at 1500°C for 2 hours, and then cooled in the furnace.

[0107] The zirconium oxide layer (sintered body layer) of the zirconium oxide powder A1 was measured for three-point bending strength (MPa), total light transmittance (%), color tone (L * 、a * and b * ).

[0108] <Three-point bending strength (MPa)> As mentioned above, the three-point bending strength is determined by Figure 6 The assays shown were performed.

[0109] <Total light transmittance (%)> The total light transmittance of the sample was measured by a method based on JIS K 7361. The sample was irradiated with standard light source D65, and the light beam passing through the sample was detected by an integrating sphere to measure the total light transmittance. A conventional haze meter (device name: haze meter NDH4000, manufactured by NIPPON DENSOKU) was used for the measurement. As a measurement sample, an arbitrary portion of the sintered body was cut out in the horizontal direction, and both surfaces of the sample were mirror-polished to a sample thickness of 1.0±0.1 mm and a surface roughness (Ra) of 0.02 μm or less.

[0110] <L * 、a * and b * > The color tone was measured using a colorimeter (device name: ZE6000, manufactured by Nippon Denshoku Industries Co., Ltd.) The measurement conditions were as follows. As hue and C * As for the specific measurement conditions, in a method of placing a zero correction box on a measurement sample and performing measurement (so-called black background measurement), the measurement is performed under the following conditions. Light source: D65 light source Viewing angle: 2° Measurement method: SCI After cutting out an arbitrary portion of the sintered body in the horizontal direction, the measurement surface of the sample was mirror-polished to a sample thickness of 2.8±0.1 mm and a surface roughness (Ra) of 0.02 μm or less.

[0111] The evaluation results of the properties of the zirconium oxide layer (sintered body layer) using the zirconium oxide powder A1 are shown in Table 1-2.

[0112] (Zirconium oxide powder A2) The zirconium oxychloride aqueous solution was hydrolyzed to obtain a hydrated zirconium oxide sol. Yttrium chloride and erbium oxide were added to the hydrated zirconium oxide sol so that the yttrium concentration was 5.05 mol% in terms of Y2O3 and the erbium concentration was 0.15 mol% in terms of Er2O3, and then dried at 180°C. The dried zirconium oxide sol was calcined at 1160°C for 2 hours, washed with pure water, and dried in the air at 110°C. α-alumina, iron oxide as an oxide coloring element, and pure water were mixed therein to prepare a slurry, which was treated in a ball mill for 22 hours to obtain a slurry containing the following powder: the powder contained 0.05 mass% of aluminum oxide and 0.085 mass% of iron as an oxide coloring element in terms of iron oxide, and the remainder was zirconium oxide containing 5.05 mol% of yttrium and 0.15 mol% of erbium. An acrylic binder was added to the obtained slurry so that the mass ratio of the binder to the mass of the powder in the slurry was 3 mass %, and the slurry was spray-dried at 180° C. in the air to obtain zirconium oxide powder A2. The BET specific surface area of ​​the obtained zirconium oxide powder was 10.1 m 2 / g, and the average particle diameter is 44μm.

[0113] (Zirconium oxide powder A3~A6) Zirconium oxide powders A3 to A6 were obtained by the same method as that of the zirconium oxide powder A2, except that sintering was performed at 1130° C. and yttrium chloride, erbium oxide, α-alumina, and iron oxide were used to have the compositions shown in Table 1-1. The compositions of the zirconium oxide powders A1 to A6 are shown in Table 1-1.

[0114] Zirconium oxide layers (sintered layers) using the zirconium oxide powders A2 to A6 were prepared by the same method as described in the above (Zirconium oxide powder A1) column, and the properties of the zirconium oxide layers (sintered layers) were evaluated. The evaluation results are shown in Table 1-2.

[0115] (Zirconium oxide powder B1) As the zirconium oxide powder B1, commercially available zirconium oxide powder Zpex4 (manufactured by TOSOH Corporation) was used.

[0116] (Zirconium oxide powder C1) As the zirconium oxide powder C1, commercially available zirconium oxide powder Zpex (manufactured by TOSOH Corporation) was used.

[0117] (Zirconium oxide powder B2~B11, C2~C4) Zirconia powders B2 to B11 and C2 to C4 having the compositions shown in Table 1-1 were prepared by the same method as for the zirconia powder A2, except that the type and content of the stabilizing element and the type and content of the coloring element were changed as shown in Table 1-1.

[0118] (Zirconium oxide powder B8 to B11) Zirconium oxide powders B8 to B11 were prepared by the same method as the zirconium oxide powder A2, except that sintering was performed at 1125° C. and yttrium chloride, erbium oxide, α-alumina, iron oxide, cobalt oxide, and titanium oxide were used to have the compositions shown in Table 1-1. Sintered body layers were also prepared using zirconium oxide powders B1 to B11 and C1 to C4, and the properties of the sintered body layers were evaluated. The evaluation results are shown in Table 1-2. The ppm in Table 1-2 is ppm by mass.

[0119] [Table 1-1]

[0120] [Table 1-2]

[0121] (Measurement of shrinkage of layers using various zirconium oxide powders) Using the above-mentioned zirconium oxide powders A1 to A6, B1 to B11 and C1 to C4, various sample layers of powder layer (molded body layer), zirconium oxide composition layer (pre-sintered body layer) and zirconium oxide layer (sintered body layer) were prepared under the following conditions, and their shrinkage rates were measured. [Sample layer for shrinkage measurement] Mold diameter: Φ25mm Powder mass: 4g Molding pressure: Uniaxial pressing: 49MPa + CIP treatment: 196MPa Molding process: Put the raw material powder for evaluation into the mold → flatten → uniaxial pressing → CIP treatment

[0122] The sample layer was prepared as described above by Figure 3 and Figure 4 The molding process shown is carried out. The sample layer of the molded body layer including the obtained powder layer (powder composition layer) was pre-fired under the following conditions to obtain a sample layer of the zirconium oxide composition layer (pre-sintered body layer). The sample layer of the zirconium oxide composition layer (pre-sintered body layer) was sintered under the following conditions to obtain a sample layer of the zirconium oxide layer (sintered body layer). [Pre-calcination and sintering conditions] Pre-sintering: from room temperature to 300°C at 15°C / hour, keep at 300°C for 5 hours, from 300°C to 700°C at 15°C / hour, keep at 700°C for 1 hour, from 700°C to 1000°C at 50°C / hour, keep at 1000°C for 2 hours, and then cool in the furnace. Sintering: 100°C / hour from room temperature to 1500°C, maintained at 1500°C for 2 hours, and then cooled in the furnace.

[0123] The shrinkage rate of each sample layer obtained as described above was measured. [Evaluation method of shrinkage rate] The diameter of the sample for shrinkage measurement (hereinafter also referred to as "sample diameter") was measured with a vernier caliper. The sample diameter was measured at four points using a vernier caliper, and the average of the measured values ​​was taken as the sample diameter. The shrinkage rate was calculated from the following formula (1). Shrinkage rate (%) = {(mold diameter: Φ25mm-sample diameter) / mold diameter: Φ25mm}×100...(1)

[0124] Table 2 shows the measurement results of the shrinkage rates of various sample layers of powder layers (molded body layers), zirconium oxide composition layers (pre-sintered body layers) and zirconium oxide layers (sintered body layers) made using the powders of zirconium oxide powders A1 to A6, B1 to B11 and C1 to C4.

[0125] [Table 2]

[0126] Example 1 (Molding body) After filling a mold with an inner diameter of 110 mm with zirconia powder A1 in an amount (21 g) to give a layer thickness of 1 mm when forming a pre-sintered body, the mold was tapped to form the (i)th powder layer (corresponding to Figure 2 The first layer (21) in the mold is filled with zirconia powder A2 in an amount (214 g) with a layer thickness of 10 mm when the pre-sintered body is formed on the (i)th powder layer, and then the mold is tapped to form the (ii)th powder layer (corresponding to Figure 2 The third layer (23) in the mold is filled with zirconium oxide powder C3 in an amount (214 g) with a layer thickness of 10 mm when the pre-sintered body is formed on the (ii) powder layer, and then the mold is tapped to form the (iii) powder layer (corresponding to Figure 2The fourth layer (24) in the (iii)th powder layer was filled with 21 g of zirconium oxide powder A1 in a layer thickness of 1 mm when the pre-sintered body was formed, and the mold was tapped to form the (iv)th powder layer (corresponding to Figure 2 Then, the fillers of the powder layers (i) to (iv) were subjected to uniaxial pressing at a pressure of 98 MPa. Then, CIP treatment was performed at a pressure of 196 MPa to obtain a laminated body comprising four layers, which was used as the molded body of this embodiment. (Pre-sintered body) The compact was calcined under the following calcination conditions to obtain a laminated body, which was used as a calcined body of this example. [Pre-burning conditions] Pre-sintering: from room temperature to 300°C at 15°C / hour, keep at 300°C for 5 hours, from 300°C to 700°C at 15°C / hour, keep at 700°C for 1 hour, from 700°C to 1000°C at 50°C / hour, keep at 1000°C for 2 hours, and then cool in the furnace. (Sintered body) The pre-sintered body was fired under the following sintering conditions to obtain a laminated body, which was used as a sintered body of this example. [Sintering conditions] Sintering: 100°C / hour from room temperature to 1500°C, maintained at 1500°C for 2 hours, and then cooled in the furnace.

[0127] The types of powders used in Example 1, the order of laminating the powders, and the conditions of Example 1 are shown in Table 3-1, and the evaluation results are shown in Table 3-2-1. The measurement results of the warpage of the sintered body of Example 1 were less than the measurement limit (0.03 mm). It should be noted that Table 3-2-1 and Table 3-2-2 are collectively referred to as Table 3-2.

[0128] (Examples 2 to 10) The laminates shown in Table 3-1 were prepared in the same manner as in Example 1 except that the types of powders used and the order of laminating the powders used were changed as shown in Table 3-1. The evaluation results are shown in Table 3-2 below.

[0129] [Table 3-1]

[0130] [Table 3-2-1]

[0131] [Table 3-2-2] In Table 3-2, the warpage measurement result recorded as "less than 0.03 mm" means less than the measurement limit of 0.03 mm, the deformation amount recorded as "less than 0.03 mm" in the molding and pre-burning column means less than the measurement limit of 0.03 mm, and the deformation amount recorded as "less than 0.04 mm" in the sintering column means less than the measurement limit of 0.04 mm.

[0132] (Comparative Examples 1 to 7) The laminated bodies shown in Table 4-1 were prepared in the same manner as in Example 1 except that the types of powders used and the lamination order of the powders used were changed as shown in Table 4-1 below. The evaluation results are shown in Table 4-2 below.

[0133] [Table 4-1]

[0134] [Table 4-2]

[0135] From the results of the embodiments, it can be seen that by setting the contents of stabilizing elements contained in the first region (e.g., the bottom layer) located at one end of the stack and the second region (e.g., the top layer) located at the other end to similar values ​​(specifically, less than 2.0 mol%), the warping of the sintered body can be suppressed, and a sintered body with light transmittance close to that of natural teeth, a gradient of color tone and little deformation can be produced. In addition, it can be seen from the results of the embodiments that by setting the shrinkage rates of the sintered body in the first region (for example, the bottom layer) located at one end of the stack and the second region (for example, the top layer) located at the other end to similar values ​​(specifically, less than 0.4%), the warping of the sintered body can be suppressed, and a sintered body with light transmittance close to that of natural teeth, a gradient of color tone and little deformation can be produced. It should be noted that the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2022-024064 filed on February 18, 2022 are incorporated herein by reference and introduced as a disclosure of the specification of the present disclosure. Description of Reference Numerals

[0136] 100, 200, 500, 600: zirconia sintered body 11, 21: First floor 12, 22: Second layer 13, 23: The third floor 24: Fourth floor 31: Powder composition 32: Mold 33: Uniaxial pressing 41: Powder formed by uniaxial pressing 42: Solvent 51: Horizontal plate 52A, 52B: Thickness gauge 53: Size of sintered body 61: Load 62: Distance between pivot points 71: Zirconia with necking structure 81: Powder composition 82: Mold 83: Uniaxial pressing 91: Powder formed by uniaxial pressing (laminated body) 92: Solvent

Claims

1. A sintered body of zirconium oxide, characterized in that: The zirconium oxide contains (i) zirconium oxide containing a stabilizing element, or (ii) zirconium oxide containing a stabilizing element and a coloring element. The sintered body has three or more regions stacked in layers, and the contents of at least one of a stabilizing element and a coloring element are different between two adjacent regions among the regions. In the stacked regions, a difference in content of the stabilizing element contained in a first region located at one end and a difference in content of the stabilizing element contained in a second region located at the other end is 2.0 mol % or less.

2. The sintered body according to claim 1, wherein The third region stacked in a layer between the first region and the second region includes one or more regions.

3. The sintered body according to claim 2, wherein The third region includes two or more regions, and the increasing and decreasing trend of at least one of light transmittance and color tone along the stacking direction does not change from the first region to the third region or from the second region to the third region.

4. A sintered body of zirconium oxide, characterized in that: The zirconium oxide contains (i) zirconium oxide containing a stabilizing element, or (ii) zirconium oxide containing a stabilizing element and a coloring element. The sintered body has three or more regions stacked in layers, and the contents of at least one of a stabilizing element and a coloring element are different between two adjacent regions among the regions. In the stacked regions, the difference in shrinkage between the first region located at one end and the second region located at the other end, that is, the shrinkage difference, is 0.4% or less.

5. The sintered body according to claim 4, wherein The third region stacked in a layer between the first region and the second region includes one or more regions.

6. The sintered body according to claim 5, wherein The third region includes two or more regions, and the increasing and decreasing trend of at least one of light transmittance and color tone along the stacking direction does not change from the first region to the third region or from the second region to the third region.

7. A pre-sintered body of a zirconium oxide composition, characterized in that: The zirconium oxide composition comprises (iii) a zirconium oxide composition containing a stabilizing element having a neck structure, or (iv) a zirconium oxide composition containing a zirconium oxide containing a stabilizing element having a neck structure and a coloring element, The pre-sintered body has three or more regions stacked in layers, and two adjacent regions among the regions have different contents of at least one of a stabilizing element and a coloring element. In the stacked regions, a difference in content of the stabilizing element contained in a first region located at one end and a difference in content of the stabilizing element contained in a second region located at the other end is 2.0 mol % or less.

8. The pre-sintered body according to claim 7, wherein The third region stacked in a layer between the first region and the second region includes one or more regions.

9. The pre-sintered body according to claim 8, wherein The third region includes two or more regions, and the increasing and decreasing tendency of the color tone along the stacking direction does not change from the first region to the third region or from the second region to the third region.

10. A pre-sintered body of a zirconium oxide composition, characterized in that: The zirconium oxide composition contains (iii) a zirconium oxide composition containing a stabilizing element having a neck structure, or contains (iv) a zirconium oxide composition containing a zirconium oxide containing a stabilizing element having a neck structure and a coloring element, The pre-sintered body has three or more regions stacked in layers, and two adjacent regions among the regions have different contents of at least one of a stabilizing element and a coloring element. In the stacked regions, the difference in shrinkage rate between the pre-sintered body in the first region located at one end and the pre-sintered body in the second region located at the other end, that is, the shrinkage rate difference is 0.4% or less.

11. The pre-sintered body according to claim 10, wherein The third region stacked in a layer between the first region and the second region includes one or more regions.

12. The pre-sintered body according to claim 11, wherein The third region includes two or more regions, and the increasing and decreasing tendency of the color tone along the stacking direction does not change from the first region to the third region or from the second region to the third region.

13. The method for producing a sintered body according to any one of claims 1 to 6, characterized in that: The manufacturing method includes a step of sintering a molded body formed by laminating three or more layers of a powder composition of a raw material powder containing zirconium oxide at a temperature of not less than 1200° C. and not more than 1600° C., wherein the raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and a coloring element when the coloring element is contained.

14. The method for producing a sintered body according to any one of claims 1 to 6, characterized in that: The manufacturing method comprises the steps of: pre-sintering a molded body formed by laminating three or more layers of a powder composition containing a raw material powder of zirconium oxide at a temperature of 800° C. or higher and lower than 1200° C. to obtain a pre-sintered body, wherein the raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and a coloring element when the coloring element is contained; and A step of sintering the pre-sintered body at a temperature of 1200°C to 1600°C.

15. The method for producing a pre-sintered body according to any one of claims 7 to 12, wherein: The manufacturing method comprises the step of calcining a molded body formed by laminating three or more layers of a powder composition containing a raw material powder of zirconium oxide at a temperature of 800° C. or higher and lower than 1200° C., The raw material powder of zirconium oxide contains zirconium oxide containing a stabilizing element and, when containing a coloring element, the coloring element.

16. A dental material, characterized in that: The present invention comprises the sintered body according to any one of claims 1 to 6.

17. A dental material, characterized in that: The present invention comprises the pre-sintered body according to any one of claims 7 to 12.

Citation Information

Patent Citations

  • Zirconia calcined body

    JP2020147495A

  • Zirconia composition, zirconia semi-sintered body and zirconia sintered body, as well as dental product

    US20180002235A1

  • Zirconia calcined body suitable for dental use

    WO2022004862A1