Solid state process for treating synthetic thermoplastic articles
By applying the coating composition under solid conditions of synthetic thermoplastic resin and decomposing it with heat to form cross-links, the problem of increased cost and complexity of additives in the existing technology is solved, and the efficient fireproof performance improvement of synthetic thermoplastic products is achieved, which is suitable for fiber and industrial production of fabrics.
Patent Information
- Application Number
- CN202380018630.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-25
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-01
AI Technical Summary
When it comes to improving the fire performance of synthetic thermoplastic products, commonly used additives add cost and processing complexity, have limited impact on droplets in standardized fire tests, and the cross-linking process is not suitable for industrial-scale fiber or fabric production. .
A solid-state method is used to apply the coating composition, including polyene compounds and free radical initiators, below the crystallization melting temperature of synthetic thermoplastic resins, and to form cross-links by thermal decomposition, avoiding the complexity of cross-linking in the molten state, and is applicable in industrial production.
Cross-linking is achieved in synthetic thermoplastic products, improving their performance in vertical flame tests, reducing or eliminating melting and droplets, and is suitable for the production of fibers and fabrics without affecting the size and shape of the products.
Smart Images

Figure BDA0004960994890000161
Abstract
Description
[0001] The present invention generally relates to a method of processing a synthetic thermoplastic article.
[0002] Synthetic thermoplastics such as aliphatic polyamides (commonly called "nylon"), polyesters, and polyacrylonitrile (PAN) are used, among other uses, to produce fibers and yarns, which are then knitted or woven to produce fabrics. Polyamide fabrics are known for their high strength and abrasion resistance. Polyamide, polyester, and polyacrylonitrile fabrics are used to make clothing, as well as protective gear for military, paramilitary, and law enforcement personnel. These fabrics are also used to make a variety of products for use within homes, offices, and / or other buildings; these include carpets, curtains, furniture upholstery, bedding, shower curtains, window treatments, wallpaper, and other decorative coverings, among others.
[0003] As a thermoplastic material, polymers such as polyamide, polyester, and PAN can and will heat soften and flow when heated to a sufficiently high temperature. In at least some of these applications, it is important that the article resists molten dripping when exposed to an open flame or other heat source. This is often a fire safety issue; the burning material of the molten dripping can propagate flames and drip onto people or animals, causing injury or death. This concern is reflected in various standard burn tests, such as ASTM D6413-11, the EN 13501-1 Single Burning Item Test, and the British Standard BS5867 Part 2-B test, which evaluate the formation of droplets under specified ignition conditions.
[0004] Many strategies have been devised to improve the performance of thermoplastic articles in standardized fire tests. These typically include the addition of various additives such as char formers, organophosphorus compounds, organohalogen compounds, hydrated minerals, red phosphorus, and borates. All of these have disadvantages. They increase cost; require additional processing steps; and affect physical and / or aesthetic properties. In some cases, they pose exposure or environmental risks. Most have little effect on melting and / or dripping.
[0005] Molded nylon parts can be cross-linked by compounding thermoplastic nylon with polyene compounds (such as triallyl cyanurate, triallyl isocyanurate and trimethylolpropane trimethacrylate) and then irradiating the composite in the mold. For example, see Pramanik et al., Radiation Physics and Chemistry 79 (2009) 199-205. Although in principle melting and / or dripping can be reduced by cross-linking thermoplastic polymers, this process is not suitable for industrial-scale fiber or fabric production. Similarly, polymers have been cross-linked or branched using combinations of such polyene compounds and various free radical initiators. For example, this is described in WO 2019 / 152264 and Yang et al. in Polymer Test 27 (2008) 957-963. These methods are carried out in the melt. They are not suitable for industrial fiber or yarn production because a large amount of gel is produced. These gels clog the spinneret and cause fiber breakage during spinning and / or subsequent drawing steps.
[0006] The present invention is a solid-state method for processing a synthetic thermoplastic article comprising a synthetic thermoplastic component, wherein the synthetic thermoplastic component comprises at least one synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C. The method comprises:
[0007] a) applying a coating composition to at least one surface of an article and in contact with at least one polyamide and / or polyester component of the article at a temperature below the crystalline melting temperature of the synthetic thermoplastic resin, wherein the coating composition comprises i) at least one polyene compound having from 2 to 6 vinyl groups and an equivalent weight per vinyl group of up to 125 grams per equivalent, and (ii) at least one free radical initiator, wherein a sufficient amount of the coating composition is applied to the article to provide at least 0.04 kilograms of the polyene compound and at least 0.005 kilograms of the peroxy or azo free radical initiator per kilogram of the synthetic thermoplastic component in the article; and
[0008] b) heating the coated article to a temperature of at least 70°C but below the crystalline melting temperature of the synthetic thermoplastic resin to decompose the peroxy or azo free radical initiator to form free radicals and produce crosslinks in the aliphatic synthetic thermoplastic resin.
[0009] Very surprisingly, the applicant has found that crosslinking can be produced in a synthetic thermoplastic resin by locally applying a coating composition followed by a solid-state (i.e., below the crystalline melting temperature of the synthetic thermoplastic resin) heating step. The ability to crosslink in this manner provides very substantial advantages. It is no longer necessary to melt blend the crosslinking agent (polyene and free radical initiator) into the synthetic thermoplastic resin before producing the article. Therefore, no special grades of resin are required and the composite costs of producing them are avoided. The radiation treatment step described by Pramanik et al. in Radiation Physics and Chemistry 79 (2009) 199-205 becomes unnecessary and can therefore be removed. Simple and inexpensive coating and heating equipment can be used. The process is suitable for both continuous and batch operations and can therefore generally be carried out on existing production lines.
[0010] In practice, the process allows synthetic thermoplastic articles produced using melt processing methods such as melt spinning, extrusion, blow molding, etc. to be modified in a simple manner to produce therein (or at least on the treated surface) properties more similar to those of cross-linked thermosetting polymers that would otherwise be inaccessible to melt processing operations. A particular advantage is that the treated products generally reduce or even eliminate melting and / or dripping when exposed to a flame in a vertical flame test. This is an important benefit when the article is a fabric or sheet that constitutes or forms part of personal clothing, protective equipment, and construction, furniture or decorative products.
[0011] The process of the present invention generally does not affect the size or geometry of the article, and changes in size and shape due to the process may be negligible or even non-existent.
[0012] In a second aspect, the present invention is a solid state method for reducing melting and / or dripping of a fabric comprising fibers of a synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C alone or in admixture with fibers of a polymer other than a synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C, the melting temperature of the fibers being at least 100°C as measured according to ASTM D7138-16, the method comprising:
[0013] a) applying a coating composition to at least one surface of a fabric at a temperature below the melting temperature of the fiber, wherein the coating composition comprises i) 30 to 99.9 weight percent, based on the weight of the coating composition, of at least one polyene compound having from 2 to 6 vinyl groups and an equivalent weight per vinyl group of up to 125 grams per equivalent, and (ii) at least one free radical initiator, wherein a sufficient amount of the coating composition is applied to the article to provide at least 0.04 kilograms of the polyene compound and at least 0.005 kilograms of the peroxy or azo free radical initiator per kilogram of fabric; and
[0014] b) heating the coated fabric to a temperature of at least 70°C but below the melting temperature of the fibers for a period of 1 minute to 2 hours.
[0015] The fabric remains soft after treatment; notably, the fibers or filaments do not aggregate to form large clumps. The tactile properties (sometimes expressed as "hand") show little change. The airflow remains essentially unchanged or changes only slightly.
[0016] Another advantage of the present invention is that the coating composition may also include other components that provide beneficial effects. These components may include, for example, plasticizers, fabric softeners, dyes, hydrophobic and / or oleophobic treatments, and many other treatments.
[0017] The process is particularly suitable for treating aliphatic polyamide, polyester and / or PAN fabrics. For example, the aliphatic polyamide, polyester and / or PAN fabrics may include aliphatic polyamide, polyester or PAN fibers alone, or a blend of aliphatic polyamide, polyester and / or PAN fibers with each other and / or with fibers of at least one other polymer other than polyamide, polyester or PAN, the fibers of such other polymer having a melting temperature of at least 100° C. as measured according to ASTM D 7138-16.
[0018] The article to be treated includes at least one synthetic thermoplastic component, the synthetic thermoplastic component including at least one synthetic thermoplastic resin having a crystalline melting temperature of at least 100° C. Examples of such synthetic thermoplastic resins include polyamides, polyesters, and PAN. In some embodiments, the synthetic thermoplastic resin accounts for at least 50%, at least 75%, or at least 90% of the total weight of the synthetic thermoplastic component.
[0019] In some embodiments, the synthetic thermoplastic resin is or includes a polyamide. Polyamide is aliphatic, i.e., has no aromatic groups. It is a thermoplastic organic polymer having repeating units connected by amide bonds. The molecular weight of each amide group is preferably at most 500 g / mol, preferably at most 300 g / mol. The crystalline melting temperature of the polyamide is at least 100° C., preferably at least 150° C., measured by the capillary method of ISO3146:2000. The polyamide can be a polymer of α,ω-amino acid, a copolymer of a dicarboxylic acid and a diamine, a polymer of a cyclic lactam, or a combination of any two or more thereof. Examples of useful polyamides include nylon 4, nylon 6, nylon 8, nylon 9, nylon 10, nylon 12, nylon 4 / 6, nylon 5 / 6, nylon 6 / 6, nylon 6 / 9, nylon 10 / 10, and nylon 10 / 12.
[0020] In other embodiments, the synthetic thermoplastic resin is or includes a polyester. The polyester may or may not contain aromatic groups. It is a thermoplastic polymer having repeating units connected by ester bonds. The molecular weight of each ester group is preferably at most 500 g / mol, preferably at most 300 g / mol. The crystalline melting temperature of the polyester is at least 100° C., preferably at least 150° C., measured by the capillary method according to ISO 3146:2000. The polyester may be, for example but not limited to, polyethylene terephthalate, poly(ethylene terephthalate), poly(butylene terephthalate), poly(ethylene adipate-co-terephthalate), poly(butylene adipate-co-terephthalate), poly(ethylene succinate), poly(l,4-cyclohexylene-dimethylene terephthalate) and poly(butylene succinate).
[0021] In other embodiments, the synthetic thermoplastic resin is or includes poly(acrylonitrile).
[0022] In addition to the synthetic thermoplastic resin, the synthetic thermoplastic component may also contain other materials. These materials may include, for example but not limited to, other polymers mixed into the synthetic thermoplastic resin or forming a dispersion with the synthetic thermoplastic resin; fillers and reinforcing agents; rheology modifiers; impact modifiers; plasticizers; colorants; various thermoplastic processing aids such as lubricants; preservatives; fungicides; antioxidants and ultraviolet stabilizers, etc.
[0023] The article may include one or more components that do not contain a synthetic thermoplastic resin. For example, these other components may be adhesively, mechanically, magnetically or otherwise secured to the synthetic thermoplastic component. For example, the article may be a multilayer structure having one or more layers of a synthetic thermoplastic resin and one or more other layers that do not contain any synthetic thermoplastic resin.
[0024] Articles of particular interest include fabrics having at least one fiber of a synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C, particularly one or more of aliphatic polyamide fibers, polyester fibers and PAN fibers. Such fabrics comprise fibers and / or yarns of a synthetic thermoplastic resin which may be woven, knitted, tangled, knotted, felted, melt-bonded or glued together. The fibers or yarns of a synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C may be blended with other fibers or yarns of other materials other than synthetic thermoplastic resins having a crystalline melting temperature of at least 100°C. Such other fibers may be or include, for example, fibers of materials such as cotton, elastomeric polyurethanes (including spandex), cellulose, wool, silk, aramid, polypropylene, polyacetate, cellulose esters (such as rayon), and the like. The fibers have a melting temperature of at least 100°C, preferably at least 150°C, according to ASTM D7138-16 Method A (if a mixture of two or more different fibers) or Method B (if a monocomponent fiber). The fabric may be in the form of a roll having a width of 100 mm or more (e.g. 300 mm to 7 meters or more), and / or may constitute all or part of a finished article, such as clothing, curtains, bedding, carpets, wallpaper, or the like.
[0025] In step a) of the process, a coating composition is applied to at least one surface of the article and is contacted with at least one synthetic thermoplastic component in the article. The coating composition includes i) at least one polyene compound having 2 to 6 vinyl groups, each vinyl equivalent being up to 150 g / equivalent, and (ii) at least one free radical initiator. The coating composition is advantageously in the form of a liquid or dispersion having a liquid phase containing dispersed solids at a temperature at which it is applied to the article. If it is a dispersion, the polyene compound and the free radical initiator can each be independently present in a liquid phase or a solid phase, or partially in both. The liquid phase of the dispersion can be, for example, a polyene compound or a free radical initiator, or both; alternatively or in addition, the liquid phase can be or include a carrier or other functional component. In some embodiments, the coating composition is a dispersion of solid radial initiator-free particles in a liquid phase, comprising a liquid polyene compound and optionally one or more other liquid components, such as a carrier and / or other liquid functional components.
[0026] Polyene compounds contain 2 to 6 vinyl groups per molecule. For the purposes of the present invention, "vinyl" is a -CHR=CHR group, wherein each R is independently hydrogen, a linear, branched or cyclic alkyl group having up to 6 carbon atoms, or a phenyl group. Vinyl is preferably allyl, i.e. part of a larger group of the form -CH2-CHR=CHR, and / or enone, i.e. part of a larger group of the form -C(O)-CHR=CHR. R is preferably hydrogen in each case.
[0027] In some embodiments, each polyene compound (if more than one) contains from 2 to 4 vinyl groups per molecule, and in particular embodiments contains 2 or 3 vinyl groups per molecule.
[0028] The equivalent weight per vinyl group of each polyene compound may be up to 125 g / equivalent.
[0029] Examples of suitable polyene compounds include, for example, various compounds corresponding to esters of acrylic acid or methacrylic acid and polyhydric alcohols. These compounds include, for example, 1,4-butanedioldiacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, cyclohexane dimethanol diacrylate, alkoxylated hexanediol diacrylate, neopentyl glycol diacrylate, diacrylate), propoxylatedneopentyl glycol diacrylate, trimethylolpropanetriacrylate, ethoxylated trimethylolpropanetriacrylate, propoxylated trimethylolpropanetriacrylate, glycerine triacrylate, ethyloxylated and / or propoxylated glycerine triacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate or pentaerythritol tetraacrylate.tri-ortetraacrylate), erythritol di-, tri-or tetraacrylate, acrylated polyester oligomer, bisphenol A diacrylate, acrylated bisphenol A diglycidyl ether, ethoxylated bisphenol A diacrylate, and the like, and corresponding compounds in which the acrylate groups are replaced by methacrylate groups. Other suitable acrylate compounds include tris(2-hydroxyethyl)isocyanurate triacrylate and acrylated urethane oligomers.
[0030] Other suitable polyene compounds are compounds having two or more allyl groups. Examples of these compounds include polyallyl ethers of polyols and polyallyl esters of polycarboxylic acids.
[0031] Suitable polyallyl ethers include, for example, 1,4-butanediol diallylether, 1,5-pentanediol diallyl ether, 1,6-hexanediol diallyl ether,6-hexanediol diallyl ether、neopentyl glycol diallyl ether、diethylene glycol diallyl ether、triethylene glycol diallyl ether、tetraethylene glycol diallyl ether、polyethylene glycol diallyl ether、dipropylene glycol diallyl ether、tripropylene glycol diallyl ether、cyclohexane dimethanol diallylether、alkoxylated hexanediol diallyl ether、neopentyl glycol diallyl ether、propoxylated neopentyl glycol diallyl ether ether), trimethylolpropane di-or triallyl ether, ethoxylated trimethylolpropane di-or triallyl ether, propoxylated trimethylolpropane di-or triallyl ether, glycerine di-or triallyl ether, ethyloxylated and / or propoxylated glycerine di-or triallyl ether, pentaerythritol di-, tri- or tetraallyl ether, erythritol diallyl ether, erythritol triallyl ether or erythritol tetraallyl ether. di-,tri-or tetraallyl ether), acrylated polyester oligomer, bisphenol A diacrylate, acrylated bisphenol A diglycidyl ether, ethoxylated bisphenol A diallylether, etc.
[0032] Examples of suitable polyallyl esters include diallyl maleate, diallyl fumarate, diallyl phthalate, diallyl terephthalate, diallyl succinate, di- or triallyl citrate, and the like.
[0033] Other useful polyene compounds include triallyl cyanurate and triallyl isocyanurate (TAIC).
[0034] The free radical initiator is one or more compounds which react thermally and / or decompose under the conditions of step b) of the process to generate free radicals. Free radical initiators which are solid at 22°C are preferred, as are those which have a 10-hour half diffusion temperature measured in toluene of at least 30°C to 70°C (as reported by the manufacturer), in particular a 10-minute half diffusion temperature of 80°C to 120°C. The free radical initiator preferably has a solubility in water of no more than 1 g / l of water and a solubility in toluene of at least 25 g / l of toluene.
[0035] Azo free radical initiators have been found to be particularly useful. Azo free radical initiators include the moiety RN=N-R', wherein R and R' are organic groups that form carbon nitrogen bonds with the corresponding adjacent nitrogens. Examples of azo radical initiators include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylpentanenitrile), 4,4'-azobis(4-cyanovaleric acid), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 2,2'-azobis(2-methylbutyronitrile).
[0036] Other useful free radical initiators include, for example, 1) acyl peroxides such as acetyl or benzoyl peroxide, 2) alkyl peroxides such as cumyl, dicumyl, lauroyl or t-butyl peroxide, 3) hydroperoxides such as t-butyl or cumyl hydroperoxide, 4) peresters such as t-butyl perbenzoate, 5) other organic peroxides including acyl alkylsulfonyl peroxides, dialkyl peroxydicarbonates, diperoxyketals, or ketone peroxides, 6) cyclic ketones and 1,2,4-trioxepane, such as described in U.S. Pat. No. 8,334,348, 7) azide compounds, 8) various tetrazines, and 9) various persulfate compounds such as potassium persulfate.
[0037] The polyene compound may comprise, for example, 30% to 99.9% of the total weight of the coating composition. In particular embodiments, the polyene compound comprises at least 35%, at least 40%, at least 45%, or at least 50% of the total weight of the coating composition. In other specific embodiments, the polyene compound comprises up to 99.5%, up to 99%, up to 95%, up to 80%, up to 70%, or up to 50% of the total weight of the coating composition.
[0038] The free radical initiator comprises, for example, 0.1% to 50% of the total weight of the coating composition. In certain embodiments, the polyene compound comprises at least 0.5%, at least 1%, at least 2%, at least 3%, or at least 4% of the total weight of the coating composition. In other specific embodiments, the polyene compound comprises up to 25%, up to 15%, up to 10%, up to 7.5%, or up to 6% of the total weight of the coating composition.
[0039] In some embodiments, the polyene compound and the free radical initiator together comprise at least 35%, at least 45%, at least 50%, at least 60%, or at least 75%, and up to 100%, up to 98%, or up to 90% of the total weight of the coating composition.
[0040] In some embodiments, the coating composition further comprises at least one vinyl terminated polysiloxane. The polysiloxane may have, for example, a vinyl content of at least 0.05 mmol / g, at least 0.1 mmol / g, and up to 2 mmol / g, preferably up to 1 mmol / g, or up to 0.5 mmol / g. The polysiloxane may contain at least 2 vinyl groups or at least 3 vinyl groups per molecule, up to 10 vinyl groups per molecule, and a nominal viscosity (as reported by the manufacturer) of 6 to 1000 cSt. Such vinyl terminated polysiloxane products are available from AB Specialty Silicones as An When present, such vinyl terminated polysiloxanes may comprise, for example, at least 5%, at least 10%, or at least 20%, and up to 69.9%, up to 60%, up to 50% of the total weight of the coating composition.
[0041] In a specific embodiment, the coating composition includes 30 to 60% by weight, especially 35 to 65% by weight of a polyene compound, 2 to 10% by weight of a free radical initiator and 25 to 75% by weight of one or more vinyl terminated polysiloxanes, the vinyl content of which is as described above. These three components can together account for, for example, 45% to 100% or 70% to 100% of the total weight of the coating composition.
[0042] The coating composition may include other ingredients other than the above-mentioned polyene compound, free radical initiator and vinyl terminated polysiloxane, which may serve as a carrier (ie, provide or supplement the liquid phase) and / or perform other specific functions.
[0043] Useful carriers or carrier mixtures are liquid at 22°C, or are materials that are solid at 22°C but have a melting point of 70°C or less, preferably 50°C or less. The boiling point of the carrier is preferably at least 100°C, more preferably at least 125°C, and even more preferably at least 150°C. Examples of useful carriers are (i) aliphatic monoalcohols or aliphatic monocarboxylic acids having 14 to 30 carbon atoms; (ii) esters of fatty acids and fatty alcohols, the esters having 18 to 48 carbon atoms, preferably 20 to 36 carbon atoms; (iii) polyethers having one or more hydroxyl groups; (iv) non-vinyl-terminated polysiloxanes, which may be linear, branched or cyclic; (v) polysiloxane-poly(alkylene glycol) copolymers; (vi) waxes, such as polyethylene wax, beeswax, lanolin, carnauba wax, candelilla wax, carnauba wax, sugar cane wax, jojoba wax, cuticle wax, coconut wax, petroleum wax, paraffin wax, etc.; (vii) fluorinated polymers, (viii) solid vegetable oils and / or animal oils or fats; (viii) another organic oligomer or polymer having a pure phase melting or softening temperature of up to 100°C, or (ix) various plasticizers.
[0044] Aliphatic monoalcohols include fatty alcohols, including saturated fatty alcohols, such as 1-dodecanol, 1-tetradecanol, 1-hexadecanol, 1-octadecyl alcohol, and the like, and fatty alcohols having one or more carbon-carbon unsaturated sites in the fatty alcohol chain. Useful esters of fatty acids and fatty alcohols include, for example, hexyl octadecanoate, octadecyl octadecyl ester, octadecyl ester, hexadecyl ester, and the like. The fatty acid and / or fatty alcohol portion of the ester may contain one or more carbon-carbon unsaturated sites.
[0045] Suitable polyethers are polymers of one or more cyclic ethers, such as propylene oxide, tetramethylene glycol, and the like. The molecular weight is high enough to produce polymers with a melting temperature of up to 100°C. The polyether may contain one or more hydroxyl groups. It may be linear or branched. The polyether may contain terminal alkyl ester groups. Specific examples of suitable polyethers include poly(ethylene oxide), monoalkyl esters of poly(ethylene oxide), poly(propylene oxide), monoalkyl esters of poly(propylene oxide), ethylene oxide-propylene oxide copolymers and their monoalkyl esters, poly(tetrahydrofuran), and the like.
[0046] Useful polysiloxanes include, for example, poly(dimethylsiloxane) and copolymers thereof. The polysiloxane may be linear, branched or cyclic. Useful siloxane-poly(alkylene glycol) copolymers include, for example, poly(dimethylsiloxane-poly(ethylene glycol) copolymers which may have a block or graft structure. Particularly preferred polysiloxanes include octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and linear or branched polydimethylsiloxane (PDMS) oils, polymethylhydrogensiloxane (PMHS) oils, and other liquid cyclomethicones.
[0047] Paraffin or beeswax are particularly preferred wax carriers. Stearyl alcohol and cetyl alcohol are particularly preferred alcohol carriers and are solid at 22°C.
[0048] Plasticizers include phthalates, trimellitates, adipates, maleates, benzoates, terephthalates, various fatty acid esters, epoxidized vegetable oils, sulfonamides, organic phosphates, alkyl citrates, acetylated monoacylglycerides, and the like.
[0049] The carrier can provide certain functional properties to the cured composition. In some embodiments, the carrier provides increased hydrophobicity and / or oleophobicity to the cured composition. It can also perform a plasticizing function. The carrier should not increase flammability.
[0050] The carrier may also include low molecular weight organic compounds having a boiling temperature below 100°C and having no polymerizable unsaturation (i.e., not a monomer as described above). These low molecular weight organic compounds include, for example, liquid polyethers and polyether monoalkyl esters, such as PPG-14 monobutyl ester; liquid alkanes, such as n-hexane, n-pentane, n-heptane, heneicosane, docosane, tricosane, tetracosane, pentacosane, hexacosane, heptacosane, octacosane, nonacosane, triacontan, etc.; liquid alcohols, such as n-propanol, isopropanol, n-butanol, tert-butanol, methanol, and ethanol; fluorinated alkanes, such as perfluorohexane, perfluoroheptane, perfluorododecane-pinene, perfluorodecane-octane, perfluorododecane, etc.; chlorinated alkanes and chlorinated aromatic hydrocarbons. compounds such as isopentyl chloride, isobutyl chloride and benzyl chloride; alkanediols and polyalkylene glycols such as ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol and 1,4-butylene glycol; liquid esters such as diisopropyl sebacate and glyceryl tripalmitate; ketones such as acetone and methyl ethyl ketone; liquid fatty acids such as stearic acid, oleic acid, palmitic acid, lauric acid, etc.; 1-naphthylamine; biphenyl; benzophenone; diphenylamine; 1,2-diphenylethane; maleic anhydride; pyrazine; thymol; glycerol; sorbitol or other sugars; and dibenzylidene sorbitol.
[0051] The carrier, if present, may comprise up to 64.9% of the total weight of the coating composition. However, if present, such a carrier is preferably present in significantly lower amounts. Preferred upper limits are up to 50%, up to 25% or up to 10%.
[0052] Other examples of such other ingredients include one or more free radical curable monomers having exactly one free radical polymerizable group per molecule and a molecular weight of up to 500. Examples of such monomers have at least one hydrocarbon group having at least eight carbon atoms and / or at least one siloxane group directly or indirectly bonded to a polymerizable group. The hydrocarbon group may be partially fluorinated or perfluorinated. The free radical polymerizable group may be any group that polymerizes in a free radical polymerization, but is preferably a vinyl, acrylate, methacrylate or chlorosilane group. At 30° C., the solubility of the monomer in water is preferably no more than 2 parts by weight per 100 parts by weight of water, more preferably no more than 1 part by weight, and even more preferably no more than 0.25 parts by weight. At 30° C., the solubility of water in the monomer is preferably no more than 2 parts by weight per 100 parts by weight of monomer, more preferably no more than 1 part by weight, and most preferably no more than 0.25 parts by weight. Examples of such monomers are further described in WO 2015 / 127479. Specific examples of monomers include, but are not limited to, one or more of the following: octyl acrylate, octyl methacrylate, decyl acrylate, decyl methacrylate, lauryl acrylate, lauryl methacrylate, octadecyl acrylate, octadecyl methacrylate, 2-perfluorohexyl ethyl acrylate, 2-perfluorooctyl ethyl acrylate, 2-perfluorodecyl ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate, 2-(perfluorooctyl)ethyl methacrylate, lauryl methacrylate, stearyl methacrylate, 2-(perfluorooctyl)ethyl methacrylate, 2-perfluorodecyldimethylchlorosilane, vinyl siloxane, and vinyl naphthalene.
[0053] The coating composition may also include one or more blowing agents. Suitable blowing agents include physical (endothermic) types that are liquid at 22°C but volatilize under the conditions of the curing step, and physical types that decompose or otherwise react to form gases under the conditions of the curing reaction. If an organic physical blowing agent is present, it should be used in small amounts so that the curable composition contains no more than 10%, preferably no more than 5%, more preferably no more than 2%, still more preferably no more than 1%, and even more preferably no more than 0.25% (by weight) of organic compounds having a boiling temperature below 100°C. Chemical blowing agents preferably generate carbon dioxide or nitrogen; these include the so-called azo types, peroxy blowing agents such as peroxy esters, peroxy carbonates, etc., and certain carbamate and citrate compounds.
[0054] The curable composition can be prepared by simply mixing the ingredients. The order of addition is generally not important as long as the free radical initiator is not exposed to temperatures at which it decomposes. The preferred method of forming the composition is to combine them in any order at a temperature of 10°C to 50°C and stir.
[0055] The coating composition is applied to the article and contacted with at least one synthetic thermoplastic component of the article. It can be applied using any of a number of convenient methods, such as by rolling, brushing, spraying, dipping the article into the composition, applying a puddle and scraping the composition onto the surface of the article using, for example, an air knife or a scraper, etc. A particularly useful method of application, particularly in a continuous industrial process, is to roll it onto the article using a roller. In this case, the curing composition is applied to a roller in any convenient manner and transferred to the substrate by contacting the substrate with the roller.
[0056] The application temperature (i.e., the temperature of the article at the time of application) is below the crystalline melting temperature of the synthetic thermoplastic resin, or in the case of a fabric, below the melting temperature of the fiber as measured by the applicable method of ASTM D-7138-16. It is important that the article remains solid throughout the process. The application temperature is preferably no greater than 70°C, more preferably no greater than 50°C or no greater than 35°C. A particularly preferred application temperature is from 10°C to 35°C.
[0057] The amount of coating applied may be expressed in terms of weight of the article and / or the surface area to which the coating composition is applied.
[0058] In certain embodiments, the amount of the coating composition is sufficient to provide 0.04 kg to 0.75 kg of polyene compounds per kg of synthetic thermoplastic components in the article and 0.005 kg to 0.05 kg of peroxy or azo free radical initiators per kg of synthetic thermoplastic components in the article. If the coating composition is applied to multiple sides of the article, the above weight is applicable to the combined weight of polyene compounds and peroxy or azo free radical initiators in all applied coatings. The amount of the coating composition can be sufficient to provide at least 0.05 kg, 0.06 kg, at least 0.075 kg or at least 0.9 kg of polyene compounds and at least 0.006 kg of peroxy or azo free radical initiators per kg of synthetic thermoplastic components in the article. In some embodiments, the amount of the coating composition is selected to provide up to 0.6 kg, up to 0.4 kg, or up to 0.3 kg of polyene compound and up to 0.04 kg or up to 0.03 kg of peroxy or azo free radical initiator per kg of synthetic thermoplastic component in the article. The total weight of the coating composition can be, for example, 0.05 kg to 1 kg, particularly 0.075 kg to 0.5 kg of coating composition per kg of synthetic thermoplastic component in the article.
[0059] The coated article is then heated to decompose the peroxy or azo free radical initiator, form free radicals, and produce crosslinks in the synthetic thermoplastic resin having a crystalline melting temperature of at least 100° C. The heating step is preferably carried out in an oxygen-deficient atmosphere. For purposes of the present invention, an oxygen-deficient atmosphere refers to a gas containing up to 1 mol % of molecular oxygen (O2). The oxygen-deficient atmosphere may contain no more than 0.1 mol % of molecular oxygen. The oxygen-deficient atmosphere may contain at least 98 mol %, preferably at least 99 mol %, and more preferably at least 99.9 mol % of an inert gas such as nitrogen, argon, carbon dioxide, steam, helium, or any mixture of two or more thereof.
[0060] The temperature in this heating step is at least 70°C but below the crystalline melting temperature of the synthetic thermoplastic resin or, for fabrics, below the fiber melting temperature as determined by the applicable method of ASTM D7138-16. During the heating step, the article remains in a solid state with no or negligible change in its original dimensions and geometry. Preferably, the temperature is at least 80°C or at least 90°C, up to 150°C or up to 125°C.
[0061] The heating step is preferably carried out in the substantial absence of ionizing radiation, such as no more than 1 kGy, no more than 0.1 kGy, no more than 0.01 kGy of ultraviolet radiation, electron beam radiation, or other ionizing radiation. It is particularly preferred that during the heating step, the article is not exposed to such ionizing radiation unless present due to natural background radiation.
[0062] The atmospheric pressure during the heating step can be negative pressure, atmospheric pressure or superatmospheric pressure. Superatmospheric pressures such as 689 kPa to 6895 kPa gauge (100 to 1000 psi gauge) are beneficial.
[0063] The heating step can be continued for a period of time, such as at least one minute, at least 15 minutes, or at least 30 minutes. Usually, a time of more than 2 hours is not required, but it can be used if more cross-linking is required or the article is larger or thicker. During the heating step, the free radical initiator generates free radicals. The free radicals and the polyene cross-link the synthetic thermoplastic resin. The cross-link density usually increases with the increase of the heating time.
[0064] Crosslinking generally results in changes in the physical and / or thermal properties of the polyamide and / or polyester components of the article. The crosslinked synthetic thermoplastic component may exhibit one or more of i) non-melting behavior characteristic of thermosetting resins; ii) delayed ignition, and / or iii) reduced dripping when exposed to an open flame.
[0065] Mechanical properties may also be altered by cross-linking. Fabrics treated according to the present invention typically show a significant reduction in melt dripping when subjected to flame tests such as ASTM D6413-11, EN 13501-1 Single Burning Event Test, and British Standard BS5867 Part 2-B Test. Fabrics treated according to the present invention typically show negligible changes in properties such as airflow, "hand", drape, etc.
[0066] Various optional components of the coating composition or their reaction products may remain with the treated article, forming a coating thereon and / or in some cases permeating into the synthetic thermoplastic component of the article. Certain carriers, if present, may remain in the treated article and impart functional properties thereto. The vinyl terminated polysiloxane may be polymerized and / or grafted onto the synthetic thermoplastic resin under the conditions of step (b) to impart elasticity.
[0067] The following examples are intended to illustrate the present invention but not to limit its scope. Unless otherwise indicated, all parts and percentages are by weight.
[0068] Example 1
[0069] The coating composition was prepared by combining in a high shear mixer 47.5 parts of triallyl isocyanurate, 47.5 parts of a vinyl terminated polysiloxane polymer having a nominal viscosity of 500 cSt and a vinyl content of 0.15 mmol / g, and 5 parts of azobisiso(butyronitrile).
[0070] The coating composition was applied to each side of each of the following fabrics using a gravure coater at about 35° C. to 40° C. The total weight of the two coatings was about 0.3 kg per kg of fabric. The application amount of triallyl isocyanurate was about 0.1425 kg / kg of fabric, and the application amount of azobisiso(butyronitrile) was about 0.015 kg / kg of fabric.
[0071] Fabric A: 98:2 blend of nylon 6,6 and spandex, camouflage colour, fabric weight 144 g / m².
[0072] - Fabric B: 100% Nylon 6,6, Camouflage colour, fabric weight 48 g / m².
[0073] Fabric C: 100% nylon 6,6, grey, fabric weight 50 g / m².
[0074] - Fabric D: 100% acrylic, fabric weight 287 g / m².
[0075] The fiber melting temperatures of fabrics A, B and C are all above 150° C. as measured according to ASTM D7138-16. The crystalline melting temperature of nylon 6,6 itself is greater than 150° C.
[0076] After coating, the fabric was heat treated in an autoclave under 400 psig (2.76 MPa) nitrogen (oxygen content <100 ppm) at 100°C for 1 hour to produce crosslinks in the nylon.
[0077] Samples of treated and untreated fabrics were evaluated for air permeability on a DA Atlas M021A air permeability tester and for water repellency using the AATCC TM-022 spray test.
[0078] The treated fabrics were also subjected to a vertical flame dripping test as follows: A 3 inch (7.62 cm) x 12 inch (30.48 cm) fabric sample was suspended vertically. A 1.5 inch (3.81 cm) high flame was placed below the lower end of the sample, ignited for 12 seconds, and then removed. The sample was observed for flammability and melting / dripping during the burning process.
[0079] Under the conditions of the vertical flame dripping test, each of the untreated fabrics melted and formed drips. After treatment, no melting or dripping was observed in any of the fabric samples.
[0080] Additionally, all fabrics showed a large increase in water repellency, with fabric A increasing from 0 to 70 and fabrics B and C increasing from 0 to 100. All fabrics showed a small decrease in air permeability.
[0081] Example 2
[0082] The coating composition was prepared by combining in a high shear mixer 47 parts of triallyl isocyanurate, 25 parts of a vinyl terminated polysiloxane polymer having a nominal viscosity of 500 cSt and a vinyl content of 0.15 mmol / g, 24 parts of a poly(dimethylsiloxane) having a nominal viscosity of 1000 cSt, and 3 parts of azobisiso(butyronitrile).
[0083] The coating composition was applied to each side of fabrics A and B using a gravure coater at about 23°C. The total weight of the two coatings was about 0.3 kg per kg of fabric. Triallyl isocyanurate was applied in an amount of about 0.14 kg per kg of fabric and azobisiso(butyronitrile) was applied in an amount of about 0.009 kg per kg of fabric. After coating, the fabrics were heat treated in an autoclave at 100°C for 30 minutes under 400 psig (2.76 MPa) nitrogen (oxygen content <100 ppm) to produce crosslinks in the nylon.
[0084] The treated and untreated fabric samples were evaluated for air permeability, water repellency and performance in the vertical flame dripping test.
[0085] As mentioned above, under the conditions of the vertical flame dripping test, each of the untreated fabrics melted and formed drips. After treatment, no melting or dripping was observed in any of the fabric samples, even after 20 wash cycles.
[0086] The water spray rating of fabric A increased from zero to 60 and dropped to 50 after 20 wash cycles. The air permeability of untreated fabric A was 7.2 standard cubic feet per minute (3.49 L / s) and remained essentially the same after treatment. After 20 wash cycles, the air permeability of the treated fabric dropped to 4.2 CFM (1.98 L / s).
[0087] After treatment, the water spray repellency rating of fabric B increased from 0 to 60. After treatment, the air permeability decreased from 23.3 CFM (11.0 L / s) to 17.1 CFM (8.07 L / s), and further decreased to 12.8 CFM (6.04 L / s) after 20 wash cycles.
[0088] Example 3
[0089] Separate samples of Fabric A were treated on each side with one of the following coating compositions and heat treated for 30 minutes to produce crosslinks in the fabric in the manner described in the previous examples.
[0090] Composition 3A: 37 parts triallyl isocyanurate, 20 parts vinyl terminated polysiloxane polymer with a nominal viscosity of 500 cSt and a vinyl content of 0.15 mmol / g, 19.5 parts poly(dimethylsiloxane) with a nominal viscosity of 1000 cSt, 2.5 parts azobisiso(butyronitrile), and 20 parts melamine cyanurate.
[0091] Composition 3B: 37 parts triallyl isocyanurate, 20 parts vinyl terminated polysiloxane polymer with a nominal viscosity of 500 cSt and a vinyl content of 0.15 mmol / g, 19.5 parts poly(dimethylsiloxane) with a nominal viscosity of 1000 cSt, 2.5 parts azobisiso(butyronitrile), and 20 parts melamine polyphosphoric acid.
[0092] In each case, the amount of triallyl isocyanurate applied was about 0.111 kg per kg of fabric and the amount of azobisiso(butyronitrile) was about 0.0075 kg per kg of fabric.
[0093] None of the treated samples showed melting or dripping during the flame test. The air permeability of the untreated sample was 7.2 CFM (11.0 L / s), while the samples treated with compositions 3A and 3B only slightly decreased to 6.2 CFM (2.83 L / s) and 6.8 CFM (3.21 L / s), respectively. The water resistance rating in each case was 50.
[0094] Example 4
[0095] The coating composition was prepared by mixing 46.5 parts of triallyl isocyanurate, 46.5 parts of a vinyl terminated polysiloxane polymer having a nominal viscosity of 500 cSt and a vinyl content of 0.15 mmol / g, and 5 parts of azobisiso(butyronitrile) in a high shear mixer.
[0096] The coating composition was applied to a poly(ethylene terephthalate) fabric weighing 139 g / m2 at about 23°C and heated for one hour in the manner described in the previous examples to produce crosslinks in the resin. Triallyl isocyanurate was applied in an amount of about 0.1395 kg per kg of fabric and azobisiso(butyronitrile) was applied in an amount of about 0.015 kg per kg of fabric. The melting temperature of the fabric was greater than 150°C as measured in accordance with ASTM D7138-16. Although the untreated fabric melted and dripped under a vertical flame test, the treated fabric did not melt or drip. The air permeability of the treated fabric was 373 CFM (176 L / s), while that of the untreated fabric was 397 CFM (187 L / s).
[0097] Comparative Examples A and B
[0098] Each side of fabrics A and B was coated with a coating composition and cured in the same general manner as described in the above examples. The coating composition is as generally described in US2017 / 0029663; it contains 38% octadecyl acrylate, 11% 1,6-hexanediol diacrylate, 5% dipentaerythritol pentaacrylate, 3% lauryl peroxide, and 43% non-vinyl terminated poly(dimethylsiloxane) with a nominal viscosity of 10CSt. The composition contains only 14% by weight of polyene (1,6-hexanediol and dipentaerythritol pentaacrylate). In each case, the total amount of polyene applied in the two coatings was about 0.048 kg per kg of fabric, and the total amount of dodecyl peroxide was about 0.009 kg per kg of fabric. The fabric treated in this way will both melt and drip when subjected to a vertical flame test. Large amounts of stearyl acrylate and poly(dimethylsiloxane) in the coating composition are believed to adversely affect the ability of the composition to introduce crosslinks into the fabric, even if substantial amounts of polyene and free radical initiator are provided in the coating.
[0099] Examples 5A-5C
[0100] Separate samples of fabric B were treated on each side with one of the following coating compositions at different coating weights as shown in the table below and heat treated for 30 minutes to produce crosslinking in the fabric in the manner described in the previous examples. The samples thus treated were subjected to the flame test, spray test and air permeability test described above, and the results are shown in the table.
[0101] Composition 5A: 92 parts of triallyl isocyanurate and 8 parts of lauroyl peroxide.
[0102] Composition 5B: 94 parts of triallyl isocyanurate and 6 parts of lauroyl peroxide.
[0103] Composition 5C: 96 parts of triallyl isocyanurate and 4 parts of lauroyl peroxide.
[0104] surface
[0105]
[0106] *This is not an example of the present invention.
[0107] The data in the table show the effect of the amount of free radical initiator used. Applications below 0.005 kg per kg of fabric produce undesirable results. Even an application of 0.005 kg provides marginal benefits in Sample 5B, although an equivalent amount of applied free radical initiator provides good results when the total coating weight is higher.
[0108] Example 6
[0109] Fabric D was coated on each side with a coating composition comprising 92.6% triallyl isocyanurate and 7.4% lauroyl peroxide. The total coating weight (both sides) was 0.1 kg / kg. The weight of polyene applied was 0.0926 kg / kg and the weight of lauroyl peroxide applied was 0.0074 kg / kg. 500 cSt of vinyl terminated polysiloxane was then applied over the polyene / free radical initiator on each side, also with a total coating weight of 0.1 kg / kg. The coated fabric was then cured at 135°C for 30 minutes under a nitrogen pressure of 400 psig (2.07 MPa) and an oxygen level of less than 100 ppm. No melting was observed in the flame test. The treated fabric had a spray rating of 70 and an air permeability of 28.4 cubic feet / minute (13.4 L / s).
[0110] Similar results were seen when the coating weight of polysiloxane was increased to 0.15 kg / kg.
Claims
1. A solid state method for treating a synthetic thermoplastic article comprising a synthetic thermoplastic component, wherein the thermoplastic component comprises at least one synthetic thermoplastic resin having a crystalline melting temperature of at least 100° C., the method comprising: a) applying a coating composition to at least one surface of the article and in contact with at least one synthetic thermoplastic component of the article at a temperature below the crystalline melting temperature of the synthetic thermoplastic resin, wherein the coating composition comprises i) from 30 to 99.9 weight percent, based on the weight of the coating composition, of at least one polyene compound having from 2 to 6 vinyl groups and an equivalent weight per vinyl group of up to 125 grams per equivalent, and (ii) at least one free radical initiator, wherein a sufficient amount of the coating composition is applied to the article to provide at least 0.04 kilograms of polyene compound and at least 0.005 kilograms of peroxy or azo free radical initiator per kilogram of polyamide and / or polyester component in the article; as well as b) heating the coated article to a temperature of at least 70°C but below the crystalline melting temperature of the synthetic thermoplastic resin to decompose the peroxy or azo free radical initiator to form free radicals and produce crosslinks in the synthetic thermoplastic resin.
2. The solid-state process of claim 1, wherein the synthetic thermoplastic component comprises one or more of an aliphatic polyamide, a polyester, and a polyacrylonitrile.
3. The solid state process of claim 2, wherein the synthetic thermoplastic component comprises at least one thermoplastic aliphatic polyamide resin selected from the group consisting of nylon 4, nylon 6, nylon 8, nylon 9, nylon 10, nylon 12, nylon 4 / 6, nylon 5 / 6, nylon 6 / 6, nylon 6 / 9, nylon 10 / 10, and nylon 10 / 12.
4. The solid-state process of claim 2, wherein the synthetic thermoplastic component comprises at least one thermoplastic polyester resin selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene adipate / terephthalate, polybutylene adipate / terephthalate, polyethylene succinate, poly1,4-cyclohexanedimethanol terephthalate, and polybutylene succinate.
5. The solid state process of claim 2, wherein the synthetic thermoplastic component comprises at least one thermoplastic polyacrylonitrile.
6. The solid-state process of claim 1 wherein the synthetic thermoplastic article is a fabric comprising fibers of a synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C alone or in admixture with fibers of a polymer that is not a synthetic thermoplastic resin and has a crystalline melting temperature of at least 100°C, the fibers having a melting temperature of at least 100°C as measured according to ASTM D7138-16.
7. A solid state method for reducing melting and / or dripping of a fabric comprising fibers of a synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C alone or in admixture with fibers of a polymer other than a synthetic thermoplastic resin having a crystalline melting temperature of at least 100°C, the melting temperature of the fibers being at least 100°C as measured according to ASTM D7138-16, the method comprising: a) applying a coating composition to at least one surface of a fabric at a temperature below the melting temperature of the fiber, wherein the coating composition comprises i) from 30 to 99.9 weight percent, based on the weight of the coating composition, of at least one polyene compound, the polyene compound having from 2 to 6 vinyl groups and an equivalent weight per vinyl group of up to 125 grams per equivalent, and (ii) at least one free radical initiator, wherein a sufficient amount of the coating composition is applied to the article to provide at least 0.04 kilograms of the polyene compound and at least 0.005 kilograms of the peroxy or azo free radical initiator per kilogram of fabric; as well as b) heating the coated fabric to a temperature of at least 70°C but below said melting temperature of said fibers for a period of from 1 minute to 2 hours.
8. The solid state process of claim 6, wherein the synthetic thermoplastic resin is one or more of an aliphatic polyamide, a polyester, and a polyacrylonitrile.
9. The solid state method of claim 7, wherein the aliphatic polyamide is selected from the group consisting of nylon 4, nylon 6, nylon 8, nylon 9, nylon 10, nylon 12, nylon 4 / 6, nylon 5 / 6, nylon 6 / 6, nylon 6 / 9, nylon 10 / 10, and nylon 10 / 12.
10. The solid-state method according to claim 7, wherein the synthetic thermoplastic resin is at least one thermoplastic polyester resin selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene adipate / terephthalate, polybutylene adipate / terephthalate, polyethylene succinate, poly1,4-cyclohexanedimethanol terephthalate, and polybutylene succinate.
11. The solid state process of claim 7 wherein the synthetic thermoplastic resin is polyacrylonitrile.
12. The solid-state method according to any one of the preceding claims, wherein the polyene compound is 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, cyclohexanedimethanol diacrylate, alkoxylated hexanediol diacrylate, neopentyl glycol diacrylate, propoxylated neopentyl glycol diacrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane diacrylate, Propane triacrylate, propoxylated trimethylolpropane triacrylate, glycerol triacrylate, ethoxylated and / or propoxylated glycerol triacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate or pentaerythritol tetraacrylate, erythritol diacrylate, erythritol triacrylate or erythritol tetraacrylate, acrylated polyester oligomer, bisphenol A diacrylate, acrylated bisphenol A diglycidyl ether, ethoxylated bisphenol A diacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate oligomer, acrylated urethane oligomer, 1,4-butanediol diallyl ether, 1,5- Pentyl glycol diallyl ether, 1,6-hexanediol diallyl ether, neopentyl glycol diallyl ether, diethylene glycol diallyl ether, triethylene glycol diallyl ether, tetraethylene glycol diallyl ether, polyethylene glycol diallyl ether, dipropylene glycol diallyl ether, tripropylene glycol diallyl ether, cyclohexanedimethanol diallyl ether, alkoxylated hexanediol diallyl ether, neopentyl glycol diallyl ether, propoxylated neopentyl glycol diallyl ether, trimethylolpropane diallyl ether or triallyl ether, ethoxylated trimethylolpropane diallyl ether or triallyl ether, propoxylated trimethylolpropane diallyl ether or triallyl ether, glycerol diallyl ether or One or more of triallyl ether, ethoxylated and / or propoxylated glycerol di- or triallyl ether, pentaerythritol diallyl ether, triallyl ether or tetraallyl ether, erythritol diallyl ether, erythritol triallyl ether or erythritol tetraallyl ether, acrylated polyester oligomer, bisphenol A diacrylate, acrylated bisphenol A diglycidyl ether, ethoxylated bisphenol A diallyl ether, maleic acid diallyl ester, fumaric acid diallyl ester, phthalic acid diallyl ester, terephthalic acid diallyl ester, succinic acid diallyl ester or triallyl ester, cyanuric acid triallyl ester and isocyanuric acid triallyl ester.
13. The solid state process according to any one of the preceding claims, wherein the free radical initiator comprises 2% to 8% by total weight of the coating composition.
14. The solid state process of any one of the preceding claims, wherein the coating composition further comprises a vinyl terminated polysiloxane having from 0.1 to 2 mmol vinyl groups per gram.
15. The solid state process of claim 13 wherein the coating composition comprises 5 to 50 weight percent of a vinyl terminated polysiloxane having 0.1 to 2 mmol of vinyl groups per gram.
16. The solid state method according to claim 13 or 14, wherein the polyene compound, free radical initiator and vinyl terminated polysiloxane having 0.1 to 2 mmol of vinyl groups per gram together account for 50% to 100% of the total weight of the coating composition.