Decellularized mushroom stem gel scaffold as well as preparation method and application thereof

By using an acellular mushroom stem gel scaffold attached with MOFs or MOFs@ICA using a hole array, the problem of low bacterial control and healing efficiency in traditional treatment of infected bone defects is solved, and effective removal of infected bone defects and new bone formation are achieved. , providing a cutting-edge treatment option.

CN118743783APending Publication Date: 2024-10-08THE SECOND AFFILIATED HOSPITAL TO NANCHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991962.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional treatments for infected bone defects cannot effectively control bacterial infection and accelerate healing, especially when antibiotic resistance and nonunion complications exist.

Method used

An acellular mushroom stem gel scaffold is used, which has a hole array and is attached with a mineralized gel of MOFs or MOFs@ICA to control bacterial infection, guide bone marrow mesenchymal stem cell migration and macrophage polarization, and promote new bone formation. .

Benefits of technology

It clears infectious bacteria in animals, induces extracellular matrix secretion and arrangement, promotes new bone formation, and significantly improves the healing efficiency of infected bone defects, providing an effective treatment strategy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743783A_ABST
    Figure CN118743783A_ABST
Patent Text Reader

Abstract

The invention provides a decellularized mushroom stem gel scaffold as well as a preparation method and application thereof. The decellularized mushroom stem gel scaffold is provided with a pore channel array, is calcified gel attached with MOFs (at) ICA, and can control bacterial infection, guide bone marrow mesenchymal stem cell migration and accelerate polarization and osteogenic differentiation of macrophages. In an animal body, the decellularized mushroom gel stem scaffold disclosed by the invention can be used for removing infected bacteria and inducing extracellular matrix secretion and arrangement within 3 days, and promoting new bone formation to cover defects within 8 weeks, so that a promising strategy is provided for treating infectious bone defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a decellularized mushroom stem gel scaffold and a preparation method and application thereof. Background Art

[0002] Bone infection, also known as osteomyelitis, can be caused by a variety of factors, such as open fractures or traumatic injuries, surgical procedures, and the spread of bacterial infection from nearby soft tissue to the bone, such as diabetic foot ulcers, pressure sores, and bedsores. Bacterial infection can significantly affect the healing process of bone infection, triggering an inflammatory response that disrupts the normal healing cascade, resulting in prolonged healing time and a higher risk of complications (such as osteomyelitis and nonunion). In severe cases, bacterial infection may require surgical intervention, such as debridement or antibiotics.

[0003] Infected bone defect is a common clinical disease, but traditional treatments often fail to achieve the desired results, especially leading to antibiotic resistance and nonunion complications. Summary of the invention

[0004] Based on this, it is necessary to provide a decellularized mushroom stem gel scaffold and its preparation method and application, which can coordinate bacterial removal and accelerate the repair of infected bone defects.

[0005] The present invention adopts the following technical solution:

[0006] The present invention provides a decellular mushroom stem gel scaffold having a pore array, and the pore array is attached with a mineralized gel containing MOFs or MOFs@ICA; the MOFs are mainly prepared by reacting zinc acetate and curcumin; the MOFs@ICA are mainly prepared by MOFs and icariin (ICA). Preferably, in the decellular mushroom stem gel scaffold, the diameter of the pore array is not greater than 2 mm.

[0007] The present invention also provides a preparation method of a decellular mushroom stem gel scaffold, comprising the following steps: preparing decellular mushroom stems; preparing MOFs or MOFs@ICA; preparing a hydrogel precursor solution containing sodium alginate and polyvinyl alcohol, mixing the hydrogel precursor solution with MOFs or MOFs@ICA, and then adding the decellular mushroom stems, and vacuum immersing to form a hydrogel load layer; placing the hydrogel load layer in a calcium chloride solution for cross-linking, freezing and thawing treatment, to obtain a calcium cross-linked gel scaffold; biomineralization reaction: adding the calcium cross-linked gel scaffold to a solution containing dipotassium hydrogen phosphate and calcium chloride for reaction, transferring to ammonia water to stabilize calcium phosphate precipitates after the reaction, and immersing and removing impurities with a phosphate buffer solution to obtain a decellular mushroom stem gel scaffold containing a mineralized gel.

[0008] In some of the embodiments, the method for preparing decellularized mushroom stems comprises the following steps: soaking the mushroom stems in an SDS solution, then soaking them in a mixed solution containing sodium hypochlorite and Triton X-100, washing them, and freeze-drying them.

[0009] In some of the embodiments, the method for preparing MOFs comprises the following steps: reacting zinc acetate, curcumin and 2-methoxy-4-methylphenol in a mixture solution of dimethylformamide and anhydrous ethanol under stirring at room temperature; heating the reaction solution to 100° C. for heat preservation to obtain a crude product; washing the crude product, centrifuging it and vacuum drying it.

[0010] In some of the embodiments, the method for preparing MOFs@ICA comprises the following steps: reacting zinc acetate, curcumin and 2-methoxy-4-methylphenol in a mixture solution of dimethylformamide and anhydrous ethanol under stirring at room temperature, heating the reaction solution to 100° C. for insulation reaction to obtain a crude product; washing the crude product, centrifuging it, and vacuum drying it to obtain MOFs; and then adding MOFs to an icariin aqueous solution for stirring reaction, centrifuging it, and drying it to obtain MOFs@ICA.

[0011] In some embodiments, the hydrogel precursor solution mainly contains 2.5 wt % sodium alginate and 5 wt % polyvinyl alcohol.

[0012] In some of the embodiments, the freezing and thawing treatment is freezing at -20°C for 12 hours and thawing at room temperature for more than 6 hours, and the cycle is repeated multiple times.

[0013] In some of the embodiments, in the biomineralization reaction, the concentration of potassium hydrogen phosphate is 300 mM, the concentration of calcium chloride is 500 mM, and the pH of ammonia water is 11.

[0014] The present invention provides application of the decellularized mushroom stem gel scaffold in preparing a medicine for preventing or treating infectious bone defects.

[0015] The present invention provides application of the decellularized mushroom stem gel scaffold in preparing a medicine for preventing or treating bacterial infection.

[0016] Compared with the prior art, the core advantages of the present invention are:

[0017] The present invention provides for the first time a decellularized mushroom stem gel scaffold, a preparation method thereof, and an application thereof in the repair of infected bone defects. The decellularized mushroom stem gel scaffold of the present invention has a pore structure in a specific size range and contains a mineralized gel of MOFs or MOFs@ICA, which can control bacterial infection, guide the migration of bone marrow mesenchymal stem cells (BMSCs), and accelerate the polarization of M2 macrophages and the osteogenic differentiation of BMSCs. In animals, the application of the decellularized mushroom stem gel scaffold of the present invention can clear infected bacteria, induce the secretion and arrangement of extracellular matrix, and promote new bone formation to cover defects, providing a promising strategy for the treatment of infected bone defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The physical and chemical properties of the decellularized mushroom stem gel scaffold and other products of its preparation process are characterized; wherein, in Figure A, (i) refers to the decellularization process (Decellularization) of mushroom stem to form decellularized mushroom stem (DM), (ii) refers to Zn2+ / curcumin to form MOFs, and then adsorb icariin (Icarin, ICA) to form MOFs@ICA, (iii) Alg / PVAHydrogel pre-solution to form reinforced hydrogel HM, HM-MOFs, HM-MOFs@ICA, and then biomineralization (Mineralization) to form MHM, and Zn2+ / curcumin to form MOFs@ICA, and then adsorb icariin (ICA) to form MOFs@ICA, and (iv) Alg / PVAHydrogel pre-solution to form reinforced hydrogel HM, HM-MOFs, HM-MOFs@ICA, and then biomineralization (Mineralization) to form MHM, and Zn2+ / curcumin to form MOFs@ICA, and then adsorb icariin (ICA) to form MOFs@ICA, and (v) Alg / PVAHydrogel pre-solution to form reinforced hydrogel HM, HM-MOFs, HM-MOFs@ICA, and then biomineralization (Mineralization) to form MHM, and Zn2+ / curcumin to form MOFs@ICA, and (vi) Alg / PVAHydrogel pre-solution to form reinforced hydrogel HM, HM-MOFs, HM-MOFs@ICA, and (vii ... 2+ / Curcumin MOFs (abbreviated as MHM-MOFs) are based on Icariin and Zn 2+ / co-loaded MHM (abbreviated as MHM-MOFs@ICA); Figure B is the SEM and elemental maps of MOFs and MOFs@ICA; Figure C is an overall view of DM, HM, MHM, MHM-MOFs, and MHM-MOFs@ICA, showing that MHM-MOFs@ICA has a through-hole array with a diameter of 1.2 mm; Figure D is the UV spectral absorption curves of DM, HM, MHM, MHM-MOFs, and MHM-MOFs@ICA; Figure E is the tensile strain-stress curves of DM, HM, MHM, MHM-MOFs, and MHM-MOFs@ICA; Figure F is Statistical graph of tensile strength of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA; Figure G is the SEM image of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA; Figure H is the pseudo-color image of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA, indicating the channel angle mapping; Figure I is the angle distribution of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA channels; *p<0.05, **p<0.01, ***p<0.001, ***p<0.0001.

[0019] Figure 2 Statistical graphs of the experimental results of biocompatibility and cell penetration behavior of decellularized mushroom gel stem scaffolds and other products in their preparation process; Figure A corresponds to the schematic diagram of bone marrow stromal stem cell inoculation, adhesion, and directional channel penetration of the scaffold; Figure B is a statistical graph showing the proliferation effect of BMSCs by CCK-8 assay; Figures C and D are live / dead cell staining images and quantitative statistical graphs; Figure E shows the confocal 3D reconstructed image of BMSC distribution after 1 and 3 days of culture; Figures F and G are the profiles and quantitative statistical graphs of cell migration distance; Figures H and I are statistical graphs of cell density at different penetration depths from 100 to 500 μm; *p<0.05, **p<0.01, ***p<0.001, ***p<0.0001.

[0020] Figure 3 Statistical graphs of experimental results of the effects of decellularized mushroom stem gel scaffolds and other products in its preparation process on macrophages; Figures A and B are ROS fluorescence images and semi-quantitative analysis of ROS inhibition (%); Figures C and D are CD206 and CD86 fluorescence images and expression heat maps; Figures E and F are Western blot analysis diagrams and the effects of different products on cell polarization; Figure G is a schematic diagram of the analysis of the effects on ROS expression of CD206 and CD86; *p<0.05, **p<0.01, ***p<0.001, ***p<0.0001.

[0021] Figure 4Statistical graphs of experimental results on the effects of decellularized mushroom gel stem scaffolds and other products in their preparation process on the osteogenic weathering of BMSCs; wherein, Figures AC are alkaline phosphatase (ALP) staining images and quantitative analysis statistical graphs of ALP activity; Figures DF are Alizarin red staining (AR) images and quantitative analysis statistical graphs of calcium nodules; Figures G and H are BMP2 and RUNX2 fluorescence staining images and their heat maps; Figure I is a schematic diagram of the analysis of how the products promote osteogenic differentiation and upregulate related biomarkers; *p<0.05, **p<0.01, ***p<0.001, ***p<0.0001.

[0022] Figure 5 Statistical graphs of experimental results on the effects of decellularized mushroom stem gel scaffolds and other products in their preparation process on the repair and regeneration of femoral bone defect models infected with Staphylococcus aureus in rats; Figures A and B are micro-CT 3D reconstructed images, sagittal and axial views of the control group and different products 4 and 8 weeks after surgery, respectively; Figures C and D are statistical graphs of regenerated bone volume (BV / TV, %) and trabecular thickness (Tb.Th, μm) of different products 4 and 8 weeks after surgery; Figures E and F are statistical graphs of colony images of infected bone defect areas and bacterial activity (%) of lavage fluids of different products 3 days after surgery; *p<0.05, **p<0.01, ***p<0.001, ***p<0.0001.

[0023] Figure 6 The figures are histological observation statistics of the decellularized mushroom stem gel scaffold and other products in its preparation process for the regeneration of infected bones 4 and 8 weeks after surgery; Figure A is the H&E staining of decalcified femurs with different products 4 and 8 weeks after surgery; Figure B is a semi-quantitative analysis of the regenerated extracellular matrix area based on the H&E staining images 4 and 8 weeks after surgery; Figure C is the trichrome staining of decalcified femurs 4 and 8 weeks after surgery; Figure D is a semi-quantitative analysis statistics of the collagen matrix area regenerated by different products 4 and 8 weeks after surgery based on the trichrome staining images; **p<0.01, ***p<0.001, ***p<0.0001.

[0024] Figure 7 The figures are statistical diagrams of the effects of the decellularized mushroom stem gel scaffold and other products of its preparation process on promoting the rapid growth of bone matrix along the directional arrangement; Figure A is a schematic diagram of the preparation of the modified decellularized mushroom scaffold and its implantation in the infected bone defect (3 mm in diameter) of the rat femur, and the red arrow indicates the direction of the channel; Figure B is a trichrome staining of the decalcified femur of the control group and the supplemented product 4 weeks after surgery, and the black arrow indicates the direction of the regenerated tissue; Figure C is a false color image from the trichrome staining indicating the direction of the regenerated tissue, and zero and 180 degrees are defined as parallel to the long axis of the femur; Figure D is the angular distribution of the regenerated collagen tissue 4 weeks after surgery.

[0025] Figure 8 Statistical graphs of experimental results on the effects of decellularized mushroom gel scaffolds and other products in their preparation process on promoting the healing of infected bone defects; Figures A to C are CD206 and CD86 immunofluorescence staining images and semi-quantitative analysis of decalcified femurs in the control group and the modified decellularized mushroom scaffold group 4 weeks after surgery; Figures D and E are BMP2, SMAD and RUNX2 immunofluorescence staining images and semi-quantitative analysis (heat map) of decalcified femurs in the control group and different products 4 weeks after surgery; Figures F and G are GDF15, CCL2 and RANKL immunofluorescence staining images and semi-quantitative analysis (heat map) of decalcified femurs in the control group and different products 4 weeks after surgery; Figure H is a schematic diagram of the principle analysis of hydroxyapatite, MOFs and ICA synergistically upregulating the BMP2 / Smad / RUNX2 signaling pathway to promote osteogenic differentiation; *p<0.05, **p<0.01, ***p<0.0001.

[0026] Fig. 9 Schematic diagram of the preparation of decellularized mushroom gel scaffold and analysis of its efficacy mechanism.

[0027] Fig.10 The figures are a general view of fresh Agaricus bisporus and a statistical graph of the protein and DNA content remaining after decellularization; Figure A is a general view and a longitudinal cross-sectional view of Agaricus bisporus and a longitudinal cross-sectional view of the mushroom stem; Figure B is a statistical graph of the residual DNA content of the decellularized mushroom stem; Figure C is a statistical graph of the residual protein content of the decellularized mushroom stem; ****p<0.0001.

[0028] Fig.11 Figure 1 is the physical and chemical characterization of Zn2+ / curcumin MOFs and ICA; Figure A is the X-ray photoelectron spectroscopy (XPS) spectra of MOFs, ICA, and MOFs@ICA; Figure B is the X-ray diffraction (XRD) spectra of MOFs and MOFs@ICA; Figure C is the UV absorption spectra of MOFs, ICA, and MOFs@ICA; Figure D is the Fourier transform infrared spectra (FTIR) of MOFs, ICA, and MOFs@ICA.

[0029] Fig.12 The activity statistics of rBMSCs under different concentrations of MOFs and MOFs@ICA; ns: not meaningful.

[0030] Fig.13 Characterization of mineralized hydroxyapatite on the decellularized mushroom stem gel scaffold; Figure A is a scanning electron microscope image; Figure B is an elemental energy spectrum analysis.

[0031] Fig.14Figure 3 is the mechanical properties characterization of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA; Figures A and B are the compression moduli of decellularized mushroom stem (DM), sodium alginate hydrogel-reinforced DM (Alg-DM), polyvinyl alcohol hydrogel-reinforced DM (PVA-DM) and sodium alginate and polyvinyl alcohol hydrogel-reinforced DM (HM), and all samples (8 mm in diameter, 5 mm in height) are dry; Figure C is the stress-strain curves of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA in the tensile test; Figure D is the tensile modulus of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA; *p<0.05, **p<0.01, ***p<0.001, ****p<0.0001.

[0032] Fig.15 Characterization of the channel characteristics of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA; Figure A is the porosity test diagram; Figure B is the pore size test diagram; Figure C is the aspect ratio of the array channel; ****p<0.0001.

[0033] Fig.16 Zn 2+ , curcumin (Cur) and icariin (ICA) release-time curve statistics; Figure A is Zn 2+ A is the release-time curve of Cur from MHM-MOFs and MHM-MOFs@ICA; Figure B is the release-time curve of Cur from MHM-MOFs and MHM-MOFs@ICA; Figure C is the release-time curve of ICA from MHM-MOFs@ICA.

[0034] Fig.17 Evaluation of the in vitro pro-angiogenic effects of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA; Figure A is a representative image of the scratch assay of HUVECs after co-culture with different product extracts; Figure B is a quantitative analysis of the scratch closure rate (residual wound area, %) after co-culture with different product extracts; Figure C is a representative image of HUVECs in the transwell migration assay after co-culture with different product extracts; Figure D is a representative image of the migrating cells (mm 2 ) quantitative analysis; Figure E is a representative image of HUVECs tube formation assay after co-culture with different product extracts; Figure F is a quantitative analysis of branch points (mm2) after co-culture with different product extracts; *p<0.05, **p<0.01, ***p<0.001, ****p<0.0001.

[0035] Fig.18The in vitro antibacterial activity test graphs of DM, HM, MHM, MHM-MOFs and MHM-MOFs@ICA; Figure A is the plate clone image of Staphylococcus aureus and Escherichia coli after co-culture with different products; Figures B and C are the bacterial viability of Staphylococcus aureus and Escherichia coli after co-culture with different products; Figure D is the SEM image of Staphylococcus aureus and Escherichia coli after co-culture with different products; ****p<0.0001.

[0036] Fig.19 Immunofluorescence staining images of CD31 in the decalcified femurs of the control group and the modified decellularized mushroom stem gel scaffold group 4 weeks after surgery (A) and semi-quantitative analysis of relative fluorescence intensity (B); ***p<0.001, ****p<0.0001. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can understand the present invention more clearly. The following embodiments are only used to illustrate the present invention, but are not only used to limit the scope of the present invention. Based on the specific embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work belong to the protection scope of the present invention. In the embodiments of the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art; in the embodiments of the present invention, if not specifically specified, the technical means used are conventional means well known to those skilled in the art.

[0038] Sources of key test materials:

[0039] Fresh white Agaricus bisporus: purchased from the local Yonghui Supermarket, and the mushroom stalk (stem) was separated.

[0040] The decellularized mushroom stem (also referred to as "decellularized mold matrix", abbreviated as "DM"), the decellularized preparation method is: cut the mushroom stem, immerse it in an aqueous solution containing 10wt% SDS for 5 days, and then immerse it in a mixture containing 10wt% sodium hypochlorite and 0.1% (v / v) Triton X-100 for 48 hours for decellularization (Decellularization), and obtain a crude decellularized mushroom stem product. The crude decellularized mushroom stem product is washed with 75% alcohol for 3 times, and then immersed in deionized water for about 72 hours to remove residual chemicals. After that, the decellularized mushroom stem impurity-free sample is frozen at -20°C for 12 hours, and then freeze-dried for 24 hours to obtain a decellularized mushroom matrix (DM).

[0041] The preparation method of MOFs is as follows: zinc acetate (160 mg), curcumin (480 mg) and 2-methoxy-4-methylphenol (400 mg) are stirred in a mixture solution of dimethylformamide (DMF) (32 mL) and anhydrous ethanol (8 mL) at room temperature for 2 hours. The reaction solution is then heated to 100°C and kept in a constant temperature oil bath at 100°C for 12 hours, centrifuged, washed with DMF 5 times, and then dried overnight at 50°C under vacuum to obtain MOFs.

[0042] Preparation method of MOFs@ICA: dissolve icariin (ICA) (20 mg) in deionized water (20 mL) to form an ICA solution; add MOFs (40 mg) to the above ICA solution and continue stirring for 24 hours, centrifuge and freeze-dry the solution after the reaction to obtain MOFs@ICA.

[0043] Preparation of hydrogel-reinforced decellular mushroom matrix (HM): The decellularized mushroom stem (DM) was placed in a hydrogel precursor solution (an aqueous solution containing 2.5 wt% sodium alginate and 5 wt% polyvinyl alcohol (PVA)) and immersed in a vacuum chamber for 2 h. It was then immersed in a 500 mM calcium chloride aqueous solution for cross-linking. The HM was then frozen at -20 °C for 12 h and thawed at room temperature for more than 6 h. The freeze-thaw cycle was repeated 3 times.

[0044] Preparation of biomineralized decellular mushroom matrix (MHM): HM was immersed in 300 mM potassium hydrogen phosphate solution and 500 mM calcium chloride solution for reaction, then transferred to ammonia water with a pH of 11 to stabilize the calcium phosphate precipitate, and then transferred to a phosphate buffered saline solution with a pH of 7.4 for 5 days to remove unreacted substances to obtain the mineralized decellular mushroom matrix.

[0045] Example 1-1

[0046] This embodiment provides a method for preparing a decellularized mushroom stem gel scaffold MHM-MOFs, comprising the following steps:

[0047] S1, placing MOFs in a hydrogel precursor solution and mixing to form a hydrogel precursor solution containing MOFs.

[0048] S2, the decellularized mushroom stem (DM) was placed in a hydrogel precursor solution containing MOFs and immersed in vacuum for 2 h, then immersed in a 500 mM calcium chloride aqueous solution for cross-linking, and then frozen at -20 °C for 12 h and thawed at room temperature for more than 6 h. The freeze-thaw cycle was repeated 3 times to obtain a hydrogel-reinforced decellularized mushroom stem scaffold containing MOFs (HM-MOFs).

[0049] S3, Biomineralization:

[0050] HM-MOFs were immersed in 300 mM potassium dihydrogen phosphate solution and 500 mM calcium chloride solution for reaction, then transferred to ammonia water with a pH of 11 to stabilize the calcium phosphate precipitate, and then transferred to a phosphate buffered saline solution with a pH of 7.4 for 5 days to remove the unreacted substances to obtain the mineralized decellularized mushroom stem gel scaffold (MHM-MOFs).

[0051] Example 1-2

[0052] This embodiment provides a method for preparing a decellularized mushroom stem gel scaffold MHM-MOFs@ICA, comprising the following steps:

[0053] S1, placing MOFs@ICA in a hydrogel precursor solution and mixing to form a hydrogel precursor solution containing MOFs@ICA.

[0054] S2, the decellularized mushroom stem (DM) was placed in a hydrogel precursor solution containing MOFs@ICA and immersed in vacuum for 2 h, then immersed in a 500 mM calcium chloride aqueous solution for cross-linking, and then frozen at -20 °C for 12 h and thawed at room temperature for more than 6 h. The freeze-thaw cycle was repeated 3 times to obtain a hydrogel-reinforced decellularized mushroom stem scaffold containing MOFs@ICA (HM-MOFs@ICA).

[0055] S3, Biomineralization:

[0056] HM-MOFs@ICA was immersed in 300 mM potassium dihydrogen phosphate solution and 500 mM calcium chloride solution for reaction, then transferred to ammonia water with a pH of 11 to stabilize the calcium phosphate precipitate, and then transferred to a phosphate buffered saline solution with a pH of 7.4 for 5 days to remove the unreacted substances to obtain the mineralized decellularized mushroom stem gel scaffold (MHM-MOFs@ICA).

[0057] The preparation process and the final product were characterized. Figure 1 as well as Figures 10 to 19 .

[0058] like Figure 1 As shown in Figure 2, scanning electron microscopy (SEM) images show that MOFs@ICA is a cubic particle with an average particle size of about 1.2 μm. The surface of MOFs@ICA appears to be rougher than that of MOFs. Elemental mapping images and X-ray photoelectron spectroscopy (XPS) spectra show that MOFs@ICAMOFs contains zinc (proven by the characteristic peak of Zn at 1022 eV in XPS), which is evenly distributed ( Figure 1 B and Fig.11Fourier transform infrared spectroscopy (FTIR) spectroscopy further confirmed MOFs@ICA, showing characteristic peaks of icariin (ICA) at 1600 cm-1 and 2930 cm-1, and characteristic peaks of MOFs MOFs@ICA ( Fig.11 Figure B). X-ray diffraction (XRD) spectra showed that MOFs@ICA showed similar XRD patterns, indicating that the addition of ICA did not change the crystal structure of MOFs ( Fig.11 The UV absorption spectrum shows that MOFs@ICA exhibits characteristic peaks consistent with curcumin (270 nm) and ICA (320 nm). Fig.11 Figure D in the figure).

[0059] like Fig.13 As shown, SEM images and elemental energy spectrum analysis showed the presence of hydroxyapatite in the decellularized mushroom stems after mineralization.

[0060] As can be seen from Figures A and B in 14, the compressive modulus and elastic modulus of DM treated with alginate and PVA hydrogel (2.5 wt% alginate or 5 wt% PVA) were significantly increased compared with DM treated with alginate or PVA alone.

[0061] Through further testing, see Figure 1 Figure E, Figure 1F, and Fig.14 Figures C and D in Figure 2 indicate that the mechanical properties of HM can be further enhanced after mineralization. SEM images show that hydroxyapatite (HA) is attached to the pore walls of the mineralized decellularized mushroom stem gel scaffolds compared with DM and HM ( Figure 1 (Fig. G).

[0062] Pseudo-color images and orientation analysis showed that both DM and modified decellularized mushroom stem gel scaffolds had vertically aligned channel structures ( Figure 1 (Fig. 1H and 1I).

[0063] Depend on Fig.15 As can be seen in Figure A, although the porosity of the decellularized mushroom stem scaffolds was reduced compared to DM, it was still more than 60%. Hydrogel and mineralization did not change the longitudinal channel structure of the decellularized mushroom scaffolds (aspect ratio greater than 3), which is characterized by a short diameter of approximately 100 μm and a long diameter of approximately 300 μm, see Fig.15 Figures B and C in .

[0064] Release experiments showed that HMM-MOFs and MHM-MOFs@ICA released within 2 weeks and continued to release slowly for more than 4 weeks, see Fig.16 Figures A and C in the figure.

[0065] It is worth noting that compared with DM, HM and MHM, which are all white, MHM-MOFs are orange and MHM-MOFs@ICA is yellow. Compared with fresh mushrooms, the residual DNA and protein contents of decellularized mushroom stems (DM) were significantly reduced.

[0066] Example 2 In vitro biocompatibility and antibacterial ability of decellularized mushroom stem gel scaffolds

[0067] Detailed test method steps for in vitro biocompatibility:

[0068] 1 g of biomaterials (HM, MHM, MHM-MOFs, MHM-MOFs@ICA) were immersed in 10 mL of DMEM culture medium scaffold for 24 h to prepare the extracts. After the extracts were filtered and sterilized, 10% FBS and 1% P / S were added for cell experiments.

[0069] CCK-8 and cell live-death staining experiments were used to evaluate the in vitro biocompatibility of biomaterials. BMSCs were seeded into 96-well plates with 2000 cells per well and cultured in DMEM medium containing 10% fetal bovine serum (FBS) and 1% streptomycin / gentamicin (P / S) and biomaterial extracts. The culture medium was changed every 2 days. At the predetermined time points, cell staining and evaluation were performed according to the instructions of CCK8 and acridine orange / ethidium bromide staining kits (Mairuida Technology (CAT No.: M247364, Shenzhen, China)).

[0070] Depend on Figure 2 As can be seen from Figures A and B, compared with the control, HM, MHM, MHM-MOFs, and MHM-MOFs@ICA all affect cell viability. Moreover, MHM-MOFs and MHM-MOFs@ICA affect cell viability and migration behavior.

[0071] Depend on Figure 2 As can be seen from Figure C: In the CCK-8 assay, HM, MHM, MHM-MOFs, and MHM-MOFs@ICA did not affect long-term cell proliferation compared with the control.

[0072] In addition, in the scratch test of HUVECs co-cultured with the above products, HMM-MOFs and MHM-MOFs@ICA showed smaller scratch areas after 24 and 48 hours compared with the control group, HM group, and MHM group (see Fig.18 Quantitative analysis of scratch closure rates confirmed these findings (see Fig.18 Figure B in the figure).

[0073] In addition, in the Transwell assay of HUVECs after co-culture, the HMM-MOFs and MHM-MOFs@ICA groups showed significantly more significant numbers of migrating cells and denser cell densities compared with the control group, HM group, and MHM group, see Fig.18 C. Quantitative analysis of the number of migrated cells confirmed these results, see Fig.18 Figure D in .

[0074] Furthermore, in the HUVECs tube formation assay, the HMM-MOFs and MHM-MOFs@ICA groups showed more dense branch points compared with the control, HM, and MHM groups, see Fig.18 Figures E and F in the figure.

[0075] Detailed test method steps for antibacterial ability:

[0076] The biomaterials (HM, MHM, MHM-MOFs, MHM-MOFs@ICA) (5 mm × 5 mm cylinder) were placed in 5 mL centrifuge tubes, and then inoculated with 100 μL of Staphylococcus aureus or Escherichia coli (106 CFU / mL) and cultured for 6 h. The co-cultured bacterial culture medium was taken out and diluted to 1×10 -5 times. The antibacterial properties of each biomaterial against Staphylococcus aureus and Escherichia coli were tested using the agar plate method. After incubation on the agar plate for 18 hours, the agar plate was photographed and the colonies were counted. After that, each group of biomaterials was gradient dehydrated and freeze-dried, and the bacterial morphology treated with HM, MHM, MHM-MOFs and MHM-MOFs@ICA was observed using SEM. The results show that:

[0077] The plate clone images of Staphylococcus aureus and Escherichia coli after co-culture with the same products showed that MHM-MOFs and MHM-MOFs@ICA exhibited significant antibacterial properties and lower bacterial viability compared with the control group, HM group, and MHM group, see Fig.17 Middle AC picture.

[0078] In addition, SEM images showed that the bacteria on the surface of MHM-MOFs and MHM-MOFs@ICA showed obvious abnormal morphology, such as depression, shrinkage (yellow arrows), and bacterial fragments (red arrows) compared with the control group, HM group, and MHM group, which indicated that MHM-MOFs and MHM-MOFs@ICA had significant antibacterial properties, see Fig.17 Figure D in .

[0079] Example 3 Cell penetration test

[0080] In the cell scratch test, human umbilical vein endothelial cells (HUVECs) were seeded in a six-well plate. When the cell density reached about 90%, a 1 mL pipette tip was used to draw a straight line in the center of each well, and the detached cells were rinsed and discarded with PBS buffer. Each group was added with the extract prepared by biomaterials (HM, MHM, MHM-MOFs, MHM-MOFs@ICA) and cultured for 24 hours and 48 hours. Cell crawling and proliferation were observed by taking photos at 0, 24 and 48 hours of culture, and the gap closure rate was measured using ImageJ software.

[0081] In the Transwell assay, 100 μL (containing 1×10 4 A suspension of human umbilical vein endothelial cells (HUVECs) (DMEM medium containing 1% FBS) was added to the Transwell chamber (Corning, USA). All chambers were then transferred to 24-well plates containing 500 μL of HM, MHM, MHM-MOFs and MHM-MOFs@ICA extracts, respectively, with standard cell culture medium as a control. After incubation for 24 hours at 5% CO 2 and 37°C, the cells were stained with crystal violet staining solution (Beyotime, China) and photographed under a microscope to calculate the number of migrated cells per unit area.

[0082] The test results are as follows Figure 2 As shown, Figure 2 Figure D shows that HM, MHM, MHM-MOFs, and MHM-MOFs@ICA contain many directional channels that can promote cell penetration. Figure 2 Figures E and F in the figure show the vertical migration pattern of rBMSCs in the above product over time through confocal 3D reconstruction images and migration profiles, respectively. Figure 2 Panel G shows that initially, one day after seeding, cells were mainly located in the range of 100 to 200 μm, and then migrated downward to the range of 300 to 500 μm on the third day. Figure 2 Figures H and I in the figure show that the quantitative analysis of cell density at different depths showed a similar trend. The cells were mainly concentrated in the upper layer on the first day, and gradually increased and migrated to the lower layer on the third day. Figure 2 Figures E and I in Figure 2 show that the migration depth of rBMSCs in MHM-MOFs and MHM-MOFs@ICA is greater than that in DM, HM, and MHM. The migration depth of rBMSCs in MHM-MOFs@ICA is the greatest, and the density of rBMSCs migrating at the bottom exceeds that of the MHM-MOFs group, indicating that MHM-MOFs@ICA can further enhance the proliferation and migration behavior of rBMSCs.

[0083] Example 4: Polarization and free radical scavenging ability test of Raw264.7 macrophages

[0084] To evaluate the antioxidant capacity of HM, MHM, MHM-MOFs and MHM-MOFs@ICA extracts, 2,2-diphenyl-1-trinitrohydrazine (DPPH) was used to determine their free radical scavenging activity. The reaction mixture (200 μL) (including DPPH and biomaterial extract) was reacted for 30 minutes under light-proof conditions, and then the absorbance at 517 nm was measured by UV spectrometer (UV-3100 instrument, Shanghai Miput Instrument Co., Ltd.). For grouping, the group without any biomaterial extract but only DPPH was the control group. The following formula was used to determine free radical inhibition:

[0085] Inhibition rate (%) = (1-OD value of sample group / OD value of control group) × 100%

[0086] In addition, 2′,7′-dichlorodihydrofluorescein diacetate (DCFH-DA) was used to detect the ROS scavenging ability of biomaterials (HM, MHM, MHM-MOFs and MHM-MOFs@ICA). Raw264.7 cells were seeded in 6-well plates at 20,000 cells per well, and then incubated with the extract of biomaterials for 24 hours, and then incubated with 0.3 mM hydrogen peroxide for 30 minutes. The supernatant was removed, and 1 mL of DCFH-DA (concentration of 10×10 -6 M DMEM medium) for continuous incubation for 30 minutes. For grouping, the group stained with DCFH-DA alone was the control group (negative control group), and the group not adding any biological material extract but only incubating with 0.3mM hydrogen peroxide, and then the group stained with DCFH-DA was the H2O2 group (positive control group). The fluorescence of the cells was imaged using an inverted fluorescence microscope. The test results are shown in Figure 3 As shown in Figures A and B.

[0087] Depend on Figure 3 As can be seen in Figure A, MHM-MOFs and MHM-MOFs@ICA have the effect of inhibiting ROS compared with HM and MHM treatments.

[0088] Depend on Figure 3 As can be seen from Figure B, compared with HM and MHM treatments, the effects of free radicals in Raw264.7 cells treated with MHM-MOFs and MHM-MOFs@ICA were more significant, and MHM-MOFs@ICA treatment had better antioxidant capacity than MHM-MOFs.

[0089] The method steps of the macrophage polarization test are:

[0090] Raw264.7 cells were cultured in high-glucose DMEM medium containing 100 ng / ml lipopolysaccharide (LPS) for 24 hours to produce an inflammatory microenvironment. Then, the medium was replaced with conditioned medium containing extracts of biomaterials (HM, MHM, MHM-MOFs and MHM-MOFs@ICA) and cultured for another 48 hours. The treated Raw264.7 cells were fixed with 4% paraformaldehyde solution for 10 minutes, permeabilized with 0.5% Triton and blocked with 10% BSA. Rabbit polyclonal anti-CD206 was co-incubated overnight, and then goat anti-rabbit IgG secondary antibody was incubated together for 1 hour. Then, the cell nuclei were stained with DAPI (Biyuntian Biotechnology, Cat. No. C1005) and observed and photographed by confocal microscopy (Nikon A1, Japan). Similarly, rabbit polyclonal CD86 antibody was used for immunofluorescence staining. In addition, the expression of CD86 and CD206 in Raw264.7 was analyzed by Western blotting (WB) experiments. Test results see Figure 3 As shown in Figures C to F.

[0091] Depend on Figure 3 As can be seen from Figures C and D, the fluorescence staining images of CD206 (M2 macrophage marker) and CD86 (M1 macrophage marker) and the corresponding expression heat maps indicate that MHM-MOFs and MHM-MOFs@ICA can promote the polarization of macrophages from a pro-inflammatory state to a pro-regenerative phenotype.

[0092] Depend on Figure 3 As can be seen from Figures E and F, Western blot analysis revealed that CD86 expression was reduced and CD206 expression was enhanced during MHM-MOFs and MHM-MOFs@ICA treatment.

[0093] Further analysis such as Figure 3 As shown in Figure G: The above results indicate that MOFs and icariin can promote the polarization of M2 macrophages by inhibiting the production of ROS.

[0094] Example 5 In vitro BMSCs osteogenic differentiation assay

[0095] Alkaline phosphatase staining and activity assay: Osteogenic precursor cells (MC3T3) (4000 cells / well) were planted in 24-well plates. When the cell density reached about 60%, the culture medium was replaced with the extract of biomaterials (HM, MHM, MHM-MOFs and MHM-MOFs@ICA) prepared with osteoinduction medium, and the culture medium was replaced every 3 days. After 7 or 14 days of culture, MC3T3 was washed with PBS and fixed with 4% paraformaldehyde at room temperature for 10 minutes. After that, the induced differentiated cells were stained according to the instructions of the BCIP / NBT alkaline phosphatase colorimetric kit (Shanghai Biyuntian Biotechnology Co., Ltd.). Photographs were taken using a microscope. The alkaline phosphatase activity of each group of cells was determined according to the alkaline phosphatase detection kit (Shanghai Biyuntian Biotechnology Co., Ltd.).

[0096] Alizarin red staining and quantitative analysis of calcium nodules: Alizarin red staining kit (Biyuntian Biotech, Cat. No. C0148S) was used to stain the differentiated cells fixed with paraformaldehyde according to the instructions. Then, 1 mL of 10% cetylpyridinium chloride was added to each well to dissolve the stained calcium nodules in order to determine the amount of calcium deposition. After 1 hour, the absorbance of each group at 490 nm was measured by a multifunctional microplate reader.

[0097] Immunofluorescence staining of osteogenic differentiation markers: MC3T3 cells after 7 days of co-culture were subjected to immunofluorescence staining in the same manner as above. Finally, cells were observed and photographed using an inverted fluorescence microscope (Carl Zeiss, Oberkochen, Germany), and the fluorescence intensity was semi-quantitatively analyzed using Image J software.

[0098] qPCR determination of osteogenic differentiation-related gene expression: After 7 days of co-culture, RNA was extracted from each group of MC3T3 cells using HiPure Total RNATrace Kit (Magen, China), and the gene expression of BMP2 and RUNX2 was analyzed by RT-qPCR. The results were normalized to the expression of the gene GAPDH.

[0099] The primer sequences used in this experiment are as follows:

[0100] RUNX2 fragment length 121 bp: TGACACTGCCACCTCTGACTTCTA and

[0101] AGGGATGAAATGCTTGGGAACT;

[0102] Bmp2 fragment length 175 bp: GCTGACCACCTGAACTCCACT and CCTCCACAACCATGTCCTGATAA;

[0103] GAPDH fragment length 133 bp: CCTCGTCCCGTAGACAAAATG and

[0104] TGAGGTCAATGAAGGGGTCGT.

[0105] Test results such as Figure 4 shown.

[0106] Figure 4 Figures AC in the figure are alkaline phosphatase (ALP) staining to verify the osteogenic properties of HM, MHM, MHM-MOFs, and MHM-MOFs@ICA after 7 and 14 days of in vitro co-culture. The results show that the blue color of MHM, MHM-MOFs, and MHM-MOFs@ICA groups is darker, indicating that the osteogenic effect is more significant and can promote the osteogenic differentiation of BMSCs in vitro, and MHM-MOFs@ICA has a better effect.

[0107] Figure 4 Figure DE in the figure uses Alizarin red staining (AR) to verify the osteogenic properties of HM, MHM, MHM-MOFs, and MHM-MOFs@ICA after 14 and 21 days of in vitro co-culture. The results show that MHM-MOFs@ICA has more red nodules. Compared with HM treatment, MHM, MHM-MOFs, and MHM-MOFs@ICA can promote the osteogenic differentiation of BMSCs in vitro, and MHM-MOFs@ICA has a better effect.

[0108] Figure 4 Figures G and H in the figure are fluorescence staining images of BMP2 and RUNX2 and semi-quantitative analysis of fluorescence intensity (heat map). The results show that compared with HM treatment, MHM, HMM-MOFs and MHM-MOFs@ICA showed higher BMP2 and RUNX2 expression levels after 7 days of co-culture, and MHM-MOFs@ICA had a better effect.

[0109] Figure 4 Figure I in Figure 2 suggests that hydroxyapatite, MOFs, and ICA in MHM-MOFs@ICA can synergistically enhance the differentiation of BMSCs into osteoblasts and stimulate the expression of osteogenic biomarkers. This demonstrates that MHM-MOFs@ICA can effectively promote the polarization of M2 macrophages and the osteogenic differentiation of BMSCs.

[0110] Example 6 Rat femoral infection defect test

[0111] Rat Staphylococcus aureus infected femoral bone defect model The SD rats (male, 12 weeks) used in this experiment were purchased from Changsha Tianqin Biotechnology Co., Ltd. The experimental groups included a control group (no material intervention), an HM group, an MHM group, an MHM-MOFs group, and an MHM-MOFs@ICA group, with 6 rats in each group. The rats were anesthetized by intraperitoneal injection of 3% sodium pentobarbital solution, the legs were skinned and hair removed, and the legs were disinfected twice with iodine tincture. A longitudinal incision was made on the outside of the lower thigh of the rat to expose the femoral shaft, and a 3mm diameter and 2mm deep femoral defect was made in the lower femur using a 3mm diameter drill. Subsequently, 10μL of Staphylococcus aureus (1×10 7 CFU / mL) were injected into the bone defect site. In the HM, MHM, MHM-MOFs, and MHM-MOFs@ICA groups, biomaterials with a diameter of 3 mm and a height of 2 mm were implanted simultaneously (HM, MHM, MHM-MOFs, and MHM-MOFs@ICA). The control group was injected with Staphylococcus aureus only without any material treatment. The muscles and skin were sutured layer by layer, and the skin was disinfected again with iodine tincture.

[0112] Test results see Figure 5 , Figure 6 and Figure 7 .

[0113] Figure 5 Figures A and B in the figure are micro-CT 3D reconstruction images and sagittal and axial views at 4 and 8 weeks after surgery. The results showed that compared with the control and HM treatment groups, the amount of regenerated bone increased significantly after MHM, MHM-MOFs, and MHM-MOFs@ICA treatment, indicating that it can effectively

[0114] Figure 5 Figures C and D are the statistical graphs of regenerated bone volume (BV / TV, %) and trabecular thickness (Tb.Th, μm) at 4 and 8 weeks after surgery, respectively. The results show that compared with the control and HM treatment groups, the trabecular bone of the regenerated bone after MHM, MHM-MOFs, and MHM-MOFs@ICA treatment is denser and closer to the structure of normal bone tissue.

[0115] Figure 5 Figures E and F in the figure are the statistical graphs of the bacterial colonies and the bacterial activity (%) of the lavage fluid in the infected bone defect area 3 days after surgery. The results showed that compared with the control, HM, and MHM treatment groups, the bacteria in the MHM-MOFs and MHM-MOFs@ICA treatment groups were significantly reduced.

[0116] Figure 6Figure A shows the HE staining of decalcified femurs 4 and 8 weeks after surgery. The results show that compared with the control and HM treatment groups, more regenerated bone was found after MHM, MHM-MOFs, and MHM-MOFs@ICA treatment.

[0117] Figure 6 Figure B shows the semi-quantitative analysis of the regenerated organic bone matrix of the decalcified femur at 4 and 8 weeks after surgery. The results showed that when the remaining defect area of ​​the bone defect was normalized to the original defect area, the bone healing area of ​​MHM-MOFs@ICA (58.6±0.6%) was significantly increased compared with the blank group (21.5±0.9%), MH (21.7±0.7%), MHM (42.3±0.3%) and MHM-MOFs (53.1±0.9%).

[0118] Figure 6 Figures C and D in the figure are three-color analysis of the regenerated collagen matrix of the decalcified femur at 4 and 8 weeks after surgery. The results showed that compared with the blank group (17.5±0.7%), MH (22.4±0.7%), MHM (29.1±0.6%) and MHM-MOFs (40.4±0.6%), the bone formation of MHM-MOFs@ICA (48.6±0.9%) was significantly increased. Compared with the control and HM treatment groups, MHM, MHM-MOFs, and MHM-MOFs@ICA treatments were able to produce more regenerated collagen matrix.

[0119] In addition, by Fig.19 As can be seen from Figures A and B, the CD31 expression levels of the HMM MOF and MHM-MOFs@ICA groups were higher than that of the MHM group.

[0120] Figure 7 Figures A to D in Figure 4 show that trichrome staining and false color images of regenerated collagen tissue in infected bone defects 4 weeks after surgery showed that the collagen matrix of the control group was disordered. The HM, MHM, HMM-MOFs, and MHM-MOFs@ICA treatment groups showed parallel arrangement and high consistency, consistent with the long axis of the femur. Compared with the control, the vertically arranged channel arrays of HM, MHM, MHM-MOFs, and MHM-MOFs@ICA can be aligned with the anatomical axis and force line of the femur, promoting the directional growth of the regenerated tissue. This orientation is attributed to the longitudinal channel structure of the acellular mushroom scaffold.

[0121] The potential mechanism of MHM-MOFs@ICA in regulating the repair of infected bone defects in rats was further explored and analyzed. Figure 8 As shown:

[0122] Depend on Figure 8As can be seen from Figures A to D in the figure: the control group, HM treatment group and MHM treatment group showed M1 / M2 ratio greater than 1, indicating that there is mainly pro-inflammatory response in the bone defect; the HMM-MOFs treatment group showed M1 / M2 ratio equal to 1, which indicates that there is a balance between pro-inflammatory response and pro-regenerative response. Interestingly, the MHM-MOFs@ICA treatment group showed less than 1, indicating that there is a main pro-regenerative immune response in the defect area.

[0123] Depend on Figure 8 As shown in Figure E, HMM-MOFs and MHM-MOFs@ICA showed higher expression levels of three markers (BMP2, SMAD, and RUNX2) compared with the control and HM treatment groups, indicating that MHM-MOFs@ICA can potentially enhance osteogenic differentiation and bone regeneration by upregulating the BMP2 / SMAD / RUNX2 signaling pathway.

[0124] Depend on Figure 8 As shown in Figure F, HMM-MOFs and MHM-MOFs@ICA showed higher expression levels of three markers (GDF15, CCL2, and RANK) compared with the control and HM treatment groups. This indicates that MHM-MOFs@ICA can promote the recruitment and functional differentiation of endogenous cells in the early stage of infected bone defects by upregulating the GDF15, CCL2, and RANK signaling pathways.

[0125] Depend on Figure 8 Figure H shows that hydroxyapatite, MOFs and ICA in MHM-MOFs@ICA synergistically upregulate the BMP2 / Smad / RUNX2 signaling pathway to promote osteogenic differentiation. In infected bone repair, MOF plays an important role in anti-infection, promoting angiogenesis and regulating the balance of M1-M2. The modified material also promotes endogenous cell recruitment and regulates the balance of osteoblasts and osteoclasts through the GDF15 / CCL2 / RANKL pathway. MHM-MOFs@ICA immunomodulation, cell recruitment and osteogenic differentiation are important steps in the process of infected bone repair.

[0126] It is worth emphasizing that the preparation technology route and application mechanism of the decellularized mushroom stem gel scaffold of the present invention refer to Fig. 9 . Specifically reflected in:

[0127] (1) The present invention preferably comprises a decellular mushroom stem gel scaffold having a pore array, and the pore array is attached with a biomineralized calcium gel of MOFs or MOFs@ICA. Preferably, in the decellular mushroom stem gel scaffold, the diameter of the pore array is no greater than 2 mm.

[0128] (2) The preferred decellularized mushroom stem gel scaffold of the present invention controls bacterial infection through Zn2+ / curcumin MOFs to promote the healing of infected bone defects, induces qualitative cell recruitment and growth, and cooperates with icariin to achieve the technical effects of immunomodulation and osteogenic differentiation.

[0129] It is necessary to point out that the above embodiments are limited to further elaboration and explanation of the technical solution of the present invention, and are not further limitations of the technical solution of the present invention. The method of the present invention is only a preferred implementation scheme, and is not used to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A decellularized mushroom stem gel scaffold, characterized in that: The device has a pore array, and the pore array is attached with a mineralized gel containing MOFs or MOFs@ICA; Wherein, the MOFs are mainly prepared by reacting zinc acetate and curcumin; The MOFs@ICA is mainly prepared from MOFs and icariin (ICA).

2. The decellularized mushroom stem gel scaffold according to claim 1, characterized in that: In the decellularized mushroom stem gel scaffold, the diameter of the pore array is no greater than 2 mm.

3. The method for preparing the decellularized mushroom stem gel scaffold according to claim 1 or 2, characterized in that: The steps include: preparing decellularized mushroom stems; Preparation of MOFs or MOFs@ICA; preparing a hydrogel precursor solution containing sodium alginate and polyvinyl alcohol, mixing the hydrogel precursor solution with MOFs or MOFs@ICA, adding decellularized mushroom stems, and vacuum immersing to form a hydrogel loading layer; placing the hydrogel loading layer in a calcium chloride solution for cross-linking, and freezing and thawing the solution to obtain a calcium cross-linked gel scaffold; Biomineralization reaction: the calcium cross-linked gel scaffold is added to a solution containing potassium dihydrogen phosphate and calcium chloride for reaction, after the reaction, it is transferred into ammonia water to stabilize the calcium phosphate precipitate, and impurities are removed by soaking in phosphate buffer to obtain a decellularized mushroom stem gel scaffold containing mineralized gel.

4. The method for preparing the decellularized mushroom stem gel scaffold according to claim 3, characterized in that: The method for preparing the decellularized mushroom stem comprises the following steps: soaking the Agaricus bisporus stem in an SDS solution, then soaking the stem in a mixed solution containing sodium hypochlorite and TritonX-100, washing, and freeze-drying.

5. The method for preparing the decellularized mushroom stem gel scaffold according to claim 3 or 4, characterized in that: The method for preparing MOFs comprises the following steps: reacting zinc acetate, curcumin and 2-methoxy-4-methylphenol in a mixture solution of dimethylformamide and anhydrous ethanol under stirring at room temperature; heating the reaction solution to 100° C. for heat preservation to obtain a crude product; washing the crude product, centrifuging it and vacuum drying it to obtain the product; The method for preparing MOFs@ICA comprises the following steps: reacting zinc acetate, curcumin and 2-methoxy-4-methylphenol in a mixture solution of dimethylformamide and anhydrous ethanol under stirring at room temperature, heating the reaction solution to 100° C. for heat preservation to obtain a crude product; washing the crude product, centrifuging it, and vacuum drying it to obtain MOFs; and then adding the MOFs to an icariin aqueous solution for stirring reaction, centrifuging it, and drying it to obtain MOFs@ICA.

6. The method for preparing the decellularized mushroom stem gel scaffold according to claim 3 or 4, characterized in that: The hydrogel precursor solution mainly contains 2.5 wt % sodium alginate and 5 wt % polyvinyl alcohol.

7. The method for preparing the decellularized mushroom stem gel scaffold according to claim 3 or 4, characterized in that: The freezing and thawing treatment is freezing at -20°C for 12 hours and thawing at room temperature for more than 6 hours, and the cycle is repeated multiple times.

8. The method for preparing the decellularized mushroom stem gel scaffold according to claim 3 or 4, characterized in that: In the biomineralization reaction, the concentration of dipotassium hydrogen phosphate is 300 mM, the concentration of calcium chloride is 500 mM, and the pH of ammonia water is 11.

9. Use of the decellularized mushroom stem gel scaffold according to claim 1 or 2 in the preparation of a drug for preventing or treating infectious bone defects.

10. Use of the decellularized mushroom stem gel scaffold according to claim 1 or 2 in preparing a drug for preventing or treating bacterial infection.