Injection seat shell of implantable drug delivery device and manufacturing method of injection seat shell

By using epoxy resin AB glue and vacuum stirring degassing, segmented thermal curing and rapid cooling demoulding technology, the biocompatibility, sealing performance and demoulding problems of the injection seat shell of the implantable drug delivery device have been solved and achieved More efficient production and safer medical devices.

CN118743789AActive Publication Date: 2024-10-08WEICAN (NANJING) MEDICAL TECH DEV CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410734730.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

The shell material of the injection seat of the existing implantable drug delivery device does not meet the medical device standards and has biocompatibility issues. The injection molding process is time-consuming and uneven mixing leads to bubbles and voids, which affects the sealing performance and drug stability, and creates demoulding problems. And the use of release agents increases medical risks.

Method used

Epoxy resin AB glue is used as the material, and through vacuum stirring, deaeration and segmented thermal curing processes, the glue ratio and temperature are controlled to reduce the generation of bubbles, improve deaeration and curing efficiency, and adopt a rapid cooling demoulding method to ensure the uniformity of the shell sex and integrity.

Benefits of technology

It improves the biocompatibility, sealing performance and durability of the shell, reduces the risk of drug leakage, enhances the success rate of demoulding, reduces medical risks, and improves production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743789A_ABST
    Figure CN118743789A_ABST
Patent Text Reader

Abstract

The invention discloses a shell of an injection seat of an implantable drug delivery device and a manufacturing method thereof, the shell is made of epoxy resin AB glue, the epoxy resin AB glue comprises a component A and a component B. The method comprises the following steps: step S1, respectively weighing the component A and the component B according to a mass ratio of 100: (30-50), and mixing to obtain the epoxy resin AB glue; s2, the epoxy resin AB glue obtained after the step S1 is completed is subjected to vacuum stirring and defoaming through a vacuum stirring and defoaming machine; s3, a mold and the epoxy resin AB glue obtained after the step S2 are placed in constant-temperature equipment for heat preservation, and the epoxy resin AB glue is injected into the mold; s4, the mold in the step S3 is oscillated, and then the mold is put into a drying box to be subjected to thermocuring; and S5, the mold obtained after the step S4 is completed is put into a condensing device to be rapidly cooled and demolded. The device can improve the uniformity and transparency of the shell, improve the defoaming effect, increase the success rate of demolding, and reduce the medical risk.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical instruments, and in particular to an injection seat shell of an implantable drug delivery device and a manufacturing method thereof. Background Art

[0002] As a vascular access device that is completely implanted in the patient's body, the implantable drug delivery device can provide a safe and reliable venous access for patients who need long-term and repeated infusion therapy. Therefore, the selection and production of its shell material is crucial. First, materials that meet medical device standards and have good biocompatibility should be selected to ensure that the shell does not cause rejection reactions or other adverse effects in human tissues; secondly, small and lightweight devices are more suitable for implantation in patients, which can reduce the patient's discomfort and activity restrictions in daily life. Especially for patients who need long-term implantation, reducing the size and weight of the implantable drug delivery device can reduce discomfort and improve the quality of life; in addition, in the specific production process, the shell of the injection seat of the implantable drug delivery device is usually an injection molded part, and injection molding takes a long time and is mixed. Unevenness will eventually lead to bubbles in the shell, which may further cause holes or pores to form inside the shell, reducing the sealing performance of the shell, and may also cause drug leakage or external environmental substances to enter the device, affecting the stability and effect of the drug. It will also reduce the overall strength and durability of the shell, causing it to crack, deform or fail during use, affecting the function and safety of the device; at the same time, in current practice, complete demolding is a major problem. Even if demolding is performed after cooling to room temperature, the integrity is still not high. Demolding is generally achieved by applying a release agent, but this product is used for medical use, and the addition of a release agent will introduce new risks of use. Summary of the invention

[0003] In view of the above technical problems, the present invention provides an injection seat shell of an implantable drug delivery device and a manufacturing method thereof.

[0004] According to a first aspect of one or more embodiments of the present invention, there is provided a method for manufacturing a housing of an injection seat of an implantable drug delivery device, wherein the housing is made of epoxy resin AB glue, and the epoxy resin AB glue comprises component A and component B. The manufacturing method comprises the following steps:

[0005] Step S1, weighing component A and component B respectively in a mass ratio of 100:30-50 and mixing them to obtain epoxy resin AB glue;

[0006] Step S2, vacuum stirring and degassing the epoxy resin AB glue obtained in step S1 by a vacuum stirring and degassing machine;

[0007] Wherein, the vacuum stirring degassing in step S2 comprises:

[0008] In the first degassing stage, the mixture is degassed in a vacuum stirring degassing machine at a speed of 500 to 1200 r / min for 20 to 90 seconds;

[0009] In the second degassing stage, the mixture is degassed in a vacuum stirring degassing machine at a speed of 1300 to 2000 r / min for 20 to 90 seconds;

[0010] In the third degassing stage, the mixture is degassed in a vacuum stirring degassing machine at a speed of 2100 to 2300 r / min for 20 to 90 seconds;

[0011] The fourth degassing stage is to degas in a vacuum stirring degassing machine at a speed of 2400 to 3000 r / min for 20 to 90 seconds;

[0012] Step S3, placing the mold and the epoxy resin AB glue obtained in step S2 in a constant temperature device for heat preservation, and injecting the epoxy resin AB glue into the mold;

[0013] Step S4, shaking the mold after completing step S3, and then placing it in a drying oven for thermal curing;

[0014] Wherein, the step S4 comprises:

[0015] The first heat curing stage: curing at 60-90°C for 30-60 minutes;

[0016] The second heat curing stage: curing at 90-180°C for 30-60 minutes;

[0017] Step S5, placing the mold after completing step S4 into a cooling device for rapid cooling and demoulding. Preferably, the component A includes epoxy resin and an auxiliary agent, and the component B is a curing agent.

[0018] Preferably, the vacuum stirring and degassing machine performs vacuum stirring and degassing at -0.5 to 5 kPa.

[0019] Preferably, step S3 comprises:

[0020] The mold and the epoxy resin AB glue completed in step S2 are kept at a constant temperature of 30 to 80° C. for 20 to 60 minutes.

[0021] Preferably, step S3 comprises:

[0022] The thermostatically controlled epoxy resin AB glue is slowly injected into the mold along the edge.

[0023] Preferably, step S4 comprises:

[0024] The mold is shaken in an oscillator at 50-100 V for 30 seconds to 3 minutes, and then placed in a drying oven for thermal curing.

[0025] Preferably, the step S5 comprises: rapidly cooling the mold to 30-60° C. within 1-5 minutes using a condensation device.

[0026] According to a second aspect of one or more embodiments of the present invention, the present invention further provides an injection seat shell of an implantable drug delivery device, wherein the injection seat shell of the implantable drug delivery device is prepared by an optional method for manufacturing the injection seat shell of the implantable drug delivery device.

[0027] The present invention selects epoxy resin component A and component B, reduces the glue ratio to improve the uniformity and transparency of the shell, adopts vacuum stirring degassing after mixing to improve the degassing effect, and maintains the mold and epoxy resin AB glue at a constant temperature before inverting the mold to avoid the generation of new bubbles. The rapid cooling method can increase the success rate of demolding and the integrity of the product, thereby reducing medical risks. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention will be further described below in conjunction with the accompanying drawings.

[0029] Figure 1 It is a schematic diagram of the manufacturing method of the present invention;

[0030] Figure 2 This is a schematic diagram of the shape of the injection seat shell of the implantable drug delivery device of the present invention;

[0031] Figure 3 It is a bar graph of the residual bubble rate under different degassing means in the present invention. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "front", "rear", "left", "right", "up", "down", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0034] See also Figure 1 , the present invention provides a technical solution:

[0035] A method for manufacturing an injection seat shell of an implantable drug delivery device, wherein the shell is made of epoxy resin AB glue, and the epoxy resin AB glue includes component A and component B. The method includes the following steps:

[0036] Step S1, weighing component A and component B respectively in a mass ratio of 100:30-50 and mixing them to obtain epoxy resin AB glue;

[0037] Step S2, vacuum stirring and degassing the epoxy resin AB glue obtained in step S1 by a vacuum stirring and degassing machine;

[0038] Step S3, placing the mold and the epoxy resin AB glue obtained in step S2 in a constant temperature device for heat preservation, and injecting the epoxy resin AB glue into the mold;

[0039] Step S4, shaking the mold in step S3, and then placing it in a drying oven for thermal curing;

[0040] Step S5, placing the mold after completing step S4 into a condensation device for rapid cooling and demoulding.

[0041] The implantable drug delivery device injection seat made by the present invention is as follows Figure 2 As shown, it is provided with a medicine inlet and a medicine outlet, and a cavity is left inside to contain the medicine liquid. Figure 2 As a form of the injection seat of the implantable drug delivery device, it is only used to facilitate the understanding of those skilled in the art and does not constitute a limitation on the specific form of the shell in the present invention. Those skilled in the art can use the manufacturing method provided in the present invention to manufacture the same or similar or significantly different implantable drug delivery device injection seat shell, as long as it conforms to the general understanding of the technicians in this field on the injection seat shell of the implantable drug delivery device.

[0042] In step S1, the epoxy resin AB glue is selected to ensure biocompatibility, facilitate the implantation of the shell into the human body, and reduce possible rejection reactions. Epoxy resin AB glue is another name for a two-liquid mixed hardening glue, one liquid is the glue also called component A, and the other liquid is the hardener also called component B. The two liquids must be mixed to harden. The commonly used component A is acrylic modified epoxy or epoxy resin, or contains catalysts and other additives, and the component B is modified amine or other hardeners, or contains catalysts and other additives.

[0043] In a specific embodiment, the component A includes epoxy resin and an auxiliary agent, and the component B is a curing agent. After experiments, the formula reduces the cost and raw material requirements on the basis of ensuring product performance. If conditions permit, the present invention does not limit the specific composition of components A and B. In another specific embodiment, component A is mainly composed of bisphenol epoxy resin, and hydantoin epoxy resin is added to the component; component B is mainly composed of low molecular weight polyamide, and 4,4'-diaminodiphenyl sulfone is added to the component, which can improve the thermal stability and aging resistance of epoxy resin AB glue.

[0044] In step S1, mixing component A and component B in a certain proportion can change the shape, performance and curing time of the finished product. Too much component A and too little component B will cause difficulty in curing or even no curing. Too little component A and too much component B will cause too fast curing, or even curing without complete mixing, which is inconvenient for other steps and has poor uniformity and transparency. When component A and component B are mixed in a mass ratio range of 100:51 to 80, the finished product shell will have flocculent stripes, affecting the appearance of the product. The present invention mixes component A and component B in a mass ratio range of 100:30 to 50, and the finished product shell is uniform and transparent.

[0045] In step S2, the epoxy resin AB glue that completes step S1 is vacuum stirred and degassed by a vacuum stirring and degassing machine to minimize bubbles. The presence of bubbles in the injection seat shell of the implantable drug delivery device may cause holes or pores to form inside the shell, reducing the sealing performance of the shell, and may also cause drug leakage or external environmental substances to enter the device, affecting the stability and effect of the drug. It will also reduce the overall strength and durability of the shell, causing it to break, deform or fail during use, affecting the function and safety of the device. Therefore, it is necessary to minimize the generation of bubbles. Current degassing methods mainly include heating degassing and ultrasonic degassing. Heating degassing can cause the glue to solidify in advance, affecting subsequent operations such as reverse molding. Although ultrasonic degassing can reduce bubbles, the ultrasonic time is long and bubbles cannot be completely removed, especially dense and fine bubbles. The present invention adopts vacuum stirring and degassing, and a low pressure or negative pressure environment is generated by a vacuum stirring and degassing machine. The bubbles in the epoxy resin AB glue are removed by the effect of stirring force under high-speed rotation.

[0046] In order to test the vacuum stirring degassing effect, this application used six degassing methods to conduct experiments. The degassing effects are shown in Table 1, and the residual bubble rate can be referred to Figure 3 .

[0047] Table 1 Degassing effects of different degassing methods

[0048]

[0049] When using single-stage degassing, when the speed of the vacuum stirring degassing machine is lower than 1400r / min, the epoxy resin AB glue is prone to uneven mixing, flocs, and is in a translucent state, affecting the uniformity of the appearance of the finished product; when the speed of the vacuum stirring degassing machine exceeds 3000r / min, the epoxy resin AB glue is mixed evenly and large bubbles are basically removed, but it is difficult to remove dense small bubbles, and even cause the dense small bubbles to increase, which will affect the appearance and other performances of the finished product and increase medical risks.

[0050] Under the action of centrifugal force, the bubbles in the epoxy resin AB glue will be pushed to the periphery and separated from the colloid. The radius of small bubbles is smaller and the centrifugal force is also smaller. Therefore, the segmented vacuum stirring degassing method can increase the speed for small bubbles to optimize the degassing effect. When the degassing stage is divided into two stages, the number of large bubbles and dense small bubbles is significantly reduced, but small bubbles still exist for more than 50%. When the degassing stage is divided into three stages, dense small bubbles can be gradually removed by increasing the rotation speed step by step. Specifically, in the first degassing stage, the epoxy resin AB glue is mixed evenly by stirring and degassing at a rotation speed of 500-1200 r / min in the vacuum stirring degassing machine; in the second degassing stage, the epoxy resin AB glue is stirred and degassed at a rotation speed of 1300-2000 r / min for 20-90 s in the vacuum stirring degassing machine, and basically no large bubbles exist in the epoxy resin AB glue; in the third degassing stage, the epoxy resin AB glue is stirred and degassed at a rotation speed of 2100-2300 r / min for 20-90 s in the vacuum stirring degassing machine to further remove small bubbles in the epoxy resin AB glue, and the number of small bubbles is reduced by 67% compared with the two-stage degassing.

[0051] When the vacuum stirring degassing is divided into four stages, the dense small bubbles can also be gradually removed by increasing the speed step by step. Specifically, in the first degassing stage, the vacuum stirring degassing machine is stirred at a speed of 500-1200r / min for 20-90s, and it can be further preferably stirred at a speed of 800-1200r / min for degassing; in the second degassing stage, the vacuum stirring degassing machine is stirred at a speed of 1300-2000r / min for degassing for 20-90s, and basically no large bubbles exist in the epoxy resin AB glue; in the third degassing stage, the vacuum stirring degassing machine is stirred at a speed of 2100-2100r / min for degassing. ~2300r / min speed stirring for 20~90s. Practice shows that at this time, the small bubbles in the epoxy resin AB glue are reduced. It can be further preferred to stir and deaerate at a speed of 2100~2200r / min. At this time, the small bubbles in the epoxy resin AB glue can be reduced by 67%; the fourth deaeration stage, stirring at a speed of 2400~3000r / min in a vacuum stirring deaerator for 20~90s. Practice shows that at this time, the epoxy resin AB glue has basically no bubbles remaining, and no new bubbles are generated. It can also be further preferred to stir and deaerate at a speed of 2400~2600r / min. Generally speaking, if you want to improve the effect of stirring and deaeration, you need to extend the stirring time, but too long stirring time will cause the glue material to stratify, affecting the curing and final product performance. Therefore, segmented stirring can gradually remove the bubbles extending from the outer layer to the inner layer, ensuring that the bubbles at each level can be completely removed. At the same time, an extremely short high-speed rotation time is guaranteed to avoid stratification of the glue material. This method can not only achieve the effect of zero bubbles, but also greatly save time costs.

[0052] In one specific embodiment, the vacuum stirring deaerator performs vacuum stirring deaeration at 5 to 10 kPa. In another specific embodiment, the vacuum stirring deaerator performs vacuum stirring deaeration at -0.5 to 5 kPa. A low pressure or negative pressure environment can further improve the deaeration effect.

[0053] In step S3, the mold and the epoxy resin AB glue completed in step S2 are placed in a constant temperature device for heat preservation, and the epoxy resin AB glue is injected into the mold. Practice shows that when there is a temperature difference between the mold and the epoxy resin AB glue that has been mixed and degassed, new bubbles are likely to appear during the process of injecting the epoxy resin AB glue into the mold, and the glue may be unevenly distributed. Therefore, keeping the two at the same temperature before injection can improve the final shell molding effect.

[0054] In one specific embodiment, the mold and the epoxy resin AB glue completed in step S1 are kept at a constant temperature of 30 to 80° C. for 20 minutes. In another specific embodiment, the mold and the epoxy resin AB glue completed in step S1 are kept at a constant temperature of 30 to 80° C. for 20 to 60 minutes to ensure that there is no temperature difference between the two.

[0055] In a specific embodiment, the thermostatic epoxy resin AB glue is slowly injected into the mold along the edge to reduce the generation of bubbles and make the glue evenly distributed. The speed of injecting the glue into the mold is controlled to avoid being too fast or too slow to ensure that the glue fills every corner of the mold. A slow and even injection method can be used, or a vibration or tapping method can be used to help expel air and make the glue filling more even.

[0056] In step S4, the mold after step S3 is shaken and then placed in a drying oven for thermal curing. The shaking can reduce bubbles that appear after the glue is injected into the mold and improve the uniformity of the glue distribution.

[0057] In one specific embodiment, the mold can be placed in a drying oven for thermal curing after being shaken in an oscillator at 50 to 100 V for 3 to 5 minutes. In another specific embodiment, the mold can be placed in a drying oven for thermal curing after being shaken in an oscillator at 50 to 100 V for 30 seconds to 3 minutes to reduce the curing time.

[0058] In the current shell manufacturing process, room temperature curing or single-stage thermal curing is usually used. In order to test the curing effect, the present application uses seven curing methods to conduct experiments, and the curing effects are shown in Table 2.

[0059] Table 2 Degassing effects of different degassing methods

[0060]

[0061] When curing at room temperature, it usually takes a long time, and it varies according to the different ratios and total amount of AB glue, but generally speaking, it takes at least 48 hours to fully cure. The hand touch test of curing at room temperature for 24 hours shows that the outer layer is sticky, the middle layer is sticky, and the hardness of the outer layer is 32.3. Under normal conditions, the higher the temperature, the more time can be saved. However, according to experimental results, although single-stage heat curing can shorten the curing time, it is very easy to cause explosion when the temperature is raised at one time, which affects the normal cross-linking between the molecules of AB glue, greatly reducing the mechanical strength of the final product, and the internal and external curing are inconsistent. The hardness of the center layer is different from that of the outer layer, and the center layer is difficult to fully cure. As described in Table 2, when the drying oven was set to 70°C for curing for 60 minutes, the outer layer was cured while the center layer was not cured; when the drying oven was set to 70°C for curing for 150 minutes, the center layer was still sticky when touched, and the hardness increased slightly, but still did not exceed 50D / HA, which shows that the center layer is difficult to be completely cured when the temperature does not meet the standard; when the drying oven was set to 180°C for curing for 60 minutes, the outer layer was cured, the hardness exceeded 90D / HA, the center layer was still sticky to the touch, and the hardness difference between the center layer and the outer layer was still large; when the drying oven was set to 180°C for curing for 150 minutes, the center layer was slightly sticky when touched, and the hardness reached 72.6D / HA.

[0062] The present invention can solve the defects of traditional curing by using segmented thermal curing. In a specific embodiment, the thermal curing is divided into two stages: the first curing stage: curing at 40°C for 60 minutes; the second curing stage: curing at 70°C for 60 minutes. As a result, the outer layer is cured, while the central layer is not cured. Although the hardness of the outer layer exceeds 90D / HA, the hardness of the central layer is only 63.4D / HA.

[0063] In another specific embodiment, the thermal curing is divided into two stages: the first curing stage: curing at 70°C for 30 minutes; the second curing stage: curing at 150°C for 60 minutes. As a result, both the inner and outer layers are completely cured and the hardness exceeds 90D / HA. At the same time, the curing time is shortened to 90 minutes, which improves the curing efficiency. The segmented curing method realizes layer-by-layer curing, making the inner and outer layers more uniformly cured without affecting the mechanical strength of the product. Analysis shows that the first thermal curing stage: curing at 60-90°C for 30-60 minutes is mainly used to avoid excessive internal stress, and the second thermal curing stage: curing at 90-180°C for 30-60 minutes can achieve better cross-linking density.

[0064] In step S5, the mold that completes step S4 is placed in a condensing device for rapid cooling and demoulding. At present, it is a big problem to achieve complete demoulding after the glue solidifies. Even if demoulding is performed after cooling to room temperature, the integrity is still not high. Therefore, demoulding is generally achieved by applying a release agent. However, this product is used for medical purposes, and the increase of the release agent will introduce new risks of use. The present invention adopts a rapid cooling method, utilizes the performance difference of the mold and the epoxy resin AB glue surface at low temperature, separates the two, increases the success rate of demoulding, and the integrity of the product. For the medical industry, it can also reduce the risk of the product by not introducing new substances.

[0065] In one specific embodiment, the mold can also be rapidly cooled to 10-20° C. within 5-10 minutes using a condensation device. In another specific embodiment, the mold can be rapidly cooled to 30-60° C. within 1-5 minutes using a condensation device to further improve the condensation efficiency.

[0066] Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.

Claims

1. A method for manufacturing an injection seat shell of an implantable drug delivery device, wherein the shell is made of epoxy resin AB glue, and the epoxy resin AB glue comprises component A and component B, characterized in that: The method comprises the following steps: Step S1, weighing component A and component B respectively in a mass ratio of 100:30-50 and mixing them to obtain epoxy resin AB glue; Step S2, performing vacuum stirring and degassing on the epoxy resin AB glue obtained in step S1 by a vacuum stirring and degassing machine; Wherein, the vacuum stirring degassing in step S2 comprises: In the first degassing stage, the mixture is degassed in a vacuum stirring foaming machine at a speed of 500 to 1200 r / min for 20 to 90 seconds; In the second degassing stage, the mixture is degassed in a vacuum stirring degassing machine at a speed of 1300 to 2000 r / min for 20 to 90 seconds; In the third degassing stage, the mixture is degassed in a vacuum stirring degassing machine at a speed of 2100 to 2300 r / min for 20 to 90 seconds; The fourth degassing stage is to degas in a vacuum stirring degassing machine at a speed of 2400 to 3000 r / min for 20 to 90 seconds; Step S3, placing the mold and the epoxy resin AB glue obtained in step S2 in a constant temperature device for heat preservation, and injecting the epoxy resin AB glue into the mold after heat preservation; Step S4, shaking the mold injected with epoxy resin AB glue in step S3, and then putting it into a drying oven for thermal curing; Wherein, the step S4 comprises: The first heat curing stage: curing at 60-90°C for 30-60 minutes; The second heat curing stage: curing at 90-180°C for 30-60 minutes; Step S5, placing the mold after completing step S4 into a cooling device for rapid cooling and demoulding.

2. The method for manufacturing an injection seat shell of an implantable drug delivery device according to claim 1, characterized in that: The component A comprises epoxy resin and auxiliary agent, and the component B is a curing agent.

3. The method for manufacturing the injection seat shell of the implantable drug delivery device according to claim 2, characterized in that: The vacuum stirring and degassing machine performs vacuum stirring and degassing at -0.5 to 5 kPa.

4. The method for manufacturing an injection seat shell of an implantable drug delivery device according to claim 1, characterized in that: The step S3 comprises: The mold and the epoxy resin AB glue completed in step S2 are kept at a constant temperature of 30 to 80° C. for 20 to 60 minutes.

5. The method for manufacturing an injection seat shell of an implantable drug delivery device according to claim 1, characterized in that: The step S3 comprises: The thermostatically controlled epoxy resin AB glue is slowly injected into the mold along the edge.

6. The method for manufacturing an injection seat shell of an implantable drug delivery device according to claim 1, characterized in that: The step S4 comprises: The mold is shaken in an oscillator at 50-100 V for 30 seconds to 3 minutes, and then placed in a drying oven for thermal curing.

7. The method for manufacturing an injection seat shell of an implantable drug delivery device according to claim 1, characterized in that: The step S5 includes: rapidly cooling the mold to 30-60° C. within 1-5 minutes using a cooling device.

8. An injection seat housing of an implantable drug delivery device, characterized in that: The injection seat shell of the implantable drug delivery device is prepared by the manufacturing method of the injection seat shell of the implantable drug delivery device according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • High-temperature-resistant zinc-rich anti-corrosion coating and preparation method thereof

    CN105505127A

  • Organosilicon packaging adhesive and preparation method and application thereof

    CN108913090A

  • LED device and packaging method thereof

    CN111326644A

  • Polyurethane blade forming method

    CN113927799A

  • Epoxy resin and method for improving direct current breakdown strength of epoxy resin

    CN118082256A