Cheap preparation method of carbon nitride loaded monatomic cobalt catalyst for PMS advanced oxidation reaction

Through the cheap preparation method of cobalt hydroxide and urea, the modified carbon nitride-supported single-atom cobalt catalyst solves the problems of high cost, complex steps and low treatment efficiency in the existing technology, and achieves rapid degradation of high-concentration pollutants. , significantly improving the processing capacity of the catalyst.

CN118744009APending Publication Date: 2024-10-08GUANGXI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410847332.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing preparation methods of single-atom cobalt catalysts have high costs, complex steps, and low efficiency in treating high-concentration pollutants, and cannot effectively degrade high-concentration dyes and antibiotic pollutants.

Method used

Cobalt hydroxide and urea are ground and calcined, and then modified in a water bath to prepare a carbon nitride-supported single-atom cobalt catalyst. This cheap method improves the activity and processing capacity of the catalyst.

Benefits of technology

The rapid degradation of high-concentration pollutants is achieved. The single-atom cobalt loading of the catalyst is increased, and the treatment efficiency is increased by 5-10 times. It can completely degrade 100 mg/L pollutants in 10 minutes, significantly improving the performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744009A_ABST
    Figure CN118744009A_ABST
Patent Text Reader

Abstract

The invention discloses a low-cost preparation method of a carbon nitride loaded monatomic cobalt catalyst for PMS advanced oxidation reaction, which comprises the following steps: (1) grinding cobalt hydroxide and urea, mixing, transferring into a crucible, sealing, and calcining to obtain an x% Co-CN catalyst; and (2) adding the x% Co-CN catalyst prepared in the step (1) into water, stirring at a certain temperature, and then carrying out suction filtration, washing and drying to obtain the modified Hx% Co-CN catalyst. The catalyst is used for treating high-concentration pollutants, is high in activity, can treat 100 mgL <-1 > high-concentration pollutants by taking dye methylene blue and antibiotic sulfamethoxazole as examples, is high in degradation rate, and can degrade 97% or above within 10 min. The performance of the catalyst prepared by Kg-level amplification is only reduced by 1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material preparation and environmental catalysis, and in particular to a low-cost preparation method of a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction. Background Art

[0002] Peroxymonosulfate (PMS) activation is an advanced oxidation process (AOPs) that has attracted wide attention in the field of water environment remediation in recent years. The peroxy bond cleavage in the PMS molecule triggers a chain reaction, producing sulfate radicals (·SO) with stronger oxidizing ability than hydroxyl radicals (·OH). 4 - ), degrading the target pollutants with highly active species. The sulfate radicals (·SO 4 - ) has extremely strong oxidizing ability and can quickly and efficiently degrade organic pollutants and quickly kill microorganisms in water. At present, the research on PMS is mainly concentrated in two aspects. One is to activate PMS as a new advanced oxidation technology to degrade various organic pollutants in water; the other is to use PMS as a disinfectant to study its disinfection process and the generation of toxic by-products in the disinfection process.

[0003] Cobalt-based materials catalyzing permonosulfate (PMS) is an important research direction of advanced oxidation water treatment technology. The existing single-atom cobalt catalyst synthesis is mainly divided into one-step method and multi-step method. The multi-step method has two or more preparation procedures, while the cobalt precursor used in other one-step methods to prepare single-atom cobalt catalysts is relatively expensive, and some one-step methods require a long time or more steps of pre-treatment. The existing methods for preparing single-atom cobalt catalysts use cobalt (II) acetylacetonate or CoNO 3 6H 2 O is used as a raw material for preparation, and the raw materials used in the preparation method are expensive, or the preparation process steps are relatively complicated.

[0004] For example, in patent applications CN116586090A and CN114534759A, a single-atom cobalt catalyst was prepared by the method of "supramolecular self-assembly-coordination / electrostatic adsorption-calcination", and the catalyst pretreatment steps prepared by this method are complicated. In patent application CN116212929B, a cobalt source solution (sulfonic acid phthalocyanine cobalt or sulfonic acid phthalocyanine dicobalt) and a salt solution are mixed evenly, dried, and pyrolyzed under the protection of an inert gas to obtain the cobalt single-atom catalyst. The method for preparing the catalyst uses expensive cobalt source raw materials. Moreover, the catalyst prepared by the prior art can only treat pollutants at lower concentrations.

[0005] For another example, Zhang et al. (Zhang W, Tay HL, Lim SS, et al. Supported cobalt oxide on MgO: Highly efficient catalysts for degradation of organic dyes in dilute solutions [J]. Applied Catalysis B: Environmental, 2010, 95 (1): 93-9.) synthesized nitrogen-doped carbon-coated cobalt nanoparticle catalyst Co@NC-750 with a clear core-shell structure by a two-step pyrolysis method. The catalyst dosage was 0.02 g / L; the oxidant (PMS) dosage was 0.1 g / L; the methylene blue concentration was 10 mg / L; the reaction time was 10 min; and the removal rate was 100%.

[0006] Tan et al. (Tan J, Xu C, Zhang X, et al. MOFs-derived defect carbonencapsulated magnetic metallic Co nanoparticles capable of efficiently activating PMS to rapidly degrade dyes [J]. Separation and Purification Technology, 2022, 289: 120812.) prepared MOF-derived carbon-coated magnetic metal Co-NPs, with a single metal cobalt species embedded in porous carbon defects. Catalyst dosage 0.02 g / L; oxidant (PMS) dosage 0.1 g / L; methylene blue concentration 10 mg / L; reaction time 10 min; removal rate is about 95%. The above catalyst is used for dye pollutant treatment, with a long treatment time, and can only treat low-concentration pollutants.

[0007] Wu et al. (Wu L, Guo P, Wang X, et al. Mechanism study of CoS 2 / Fe(III) / peroxymonosulfate catalysis system:The vital role of sulfur vacancies[J].Chemosphere,2022,288:132646.) studied the commercial CoS 2 / PMS system for the removal of methylene blue. Catalyst dosage 0.1g / L; oxidant (PMS) dosage 0.6g / L; methylene blue concentration 10mg / L; reaction time 15min; removal rate is about 65%.

[0008] Chen et al. (Chen H, Yang Y, Wei J, et al. Cobalt ferrites / activated carbon: Synthesis, magnetic separation and catalysis for potassium hydrogen persulfate [J]. Materials Science and Engineering: B, 2019, 249: 114420.) prepared magnetic cobalt ferrite (CoFe) by hydrothermal method. 2 O 4 ) / activated carbon (AC) nanocomposite materials were prepared and their catalytic effect on the degradation of methylene blue (MB) by potassium persulfate (PMS) was studied. The catalyst dosage was 0.4 g / L; the oxidant (PMS) dosage was 0.9 g / L; the methylene blue concentration was 50-200 mg / L; the reaction time was 60 min; the removal rates were approximately 100% (50 mg / L), 100% (100 mg / L), 70% (150 mg / L), and 60% (200 mg / L), respectively.

[0009] Wei et al. (Wei R, Wang H, Jiang L, et al. Molecular self-assembled synthesis of highly dispersed Co single-atom coordinated 2-methylimidazole modified carbon nitride for peroxymonosulfate activation [J]. Chemical Engineering Journal, 2023, 471: 144494.) prepared the gC nanostructured carbon ... 3 N 4 Single-atom cobalt material (2Co-MCA2MeIm) with Co-N sites. Catalyst dosage 0.1 g / L; oxidant (PMS) dosage 1.0 mM (0.614 g / L); sulfamethoxazole concentration 10 mg / L; reaction time 40 min; removal rate 99.1%. The catalyst is used to treat antibiotic pollutants, but the treatment time is long, and the pollutants that can be treated are also low concentrations, and the treatment efficiency is low.

[0010] Li et al. (Li X, Wen X, Lang J, et al. CoN 1 O 2Single-Atom Catalyst for Efficient Peroxymonosulfate Activation and Selective Cobalt(IV)=O Generation[J].Angewandte Chemie International Edition, 2023, 62(27):e202303267.) proposed a novel catalyst with unique N on the surface of Mn3O4. 1 O 2 The strategy of isolated cobalt sites with coordinated ligands was used to prepare CoN with an asymmetric coordination environment. 1 O 2 / Mn 3 O 4 The catalyst was prepared and its performance in PMS activation and sulfamethoxazole (SMX) degradation was studied. Catalyst dosage 0.2 g / L; oxidant (PMS) dosage 0.2 mM (0.12 g / L); sulfamethoxazole concentration 2 mg / L; reaction time 30 min; removal rate 100%. The catalyst is used to treat antibiotic pollutants, but the treatment time is long, and the pollutants that can be treated are also low concentrations, and the treatment efficiency is low.

[0011] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0012] The purpose of the present invention is to provide a cheap preparation method for a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction, thereby overcoming the disadvantages of high production cost, complicated production steps and poor pollutant treatment effect.

[0013] To achieve the above object, the present invention provides a low-cost preparation method of a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction, comprising the following steps:

[0014] (1) grinding cobalt hydroxide and urea, mixing them, transferring them into a crucible, sealing them, and calcining them to obtain an x% Co-CN catalyst;

[0015] (2) The x% Co-CN catalyst prepared in step (1) is added into water, stirred at a certain temperature, and then filtered, washed and dried to obtain a modified Hx% Co-CN catalyst.

[0016] Preferably, in the above technical solution, the mass ratio of the cobalt hydroxide and urea mixed in step (1) is 2-100:10000.

[0017] Preferably, in the above technical solution, the calcination temperature in step (1) is 500-600°C, the calcination time is 1-10h, and the heating rate is 2-10°C / min.

[0018] Preferably, in the above technical solution, the mass ratio of the Co-CN catalyst in step (2) to the volume ratio of water is 1:1000-10000 g / ml.

[0019] Preferably, in the above technical solution, step (2) is stirred at 50-95° C. for 1-24 h.

[0020] Preferably, in the above technical solution, step (2) is stirred at 90° C. for 1-24 h.

[0021] Preferably, in the above technical solution, the mass fraction of the monoatomic cobalt loading of the prepared modified Co-CN catalyst is 0.8-8wt%.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The present invention is a cheap preparation method for a carbon nitride-supported single-atom cobalt catalyst for a PMS advanced oxidation reaction, which uses cheap cobalt hydroxide as a cobalt source to prepare a carbon nitride-supported single-atom cobalt catalyst, while increasing the content of single-atom cobalt in the catalyst. Using safer cobalt hydroxide as a cobalt source, it can be prepared by simply mixing and grinding with urea. Then, it is modified in a water bath, and the modified catalyst can expose more active sites, and the coordination environment is changed, thereby improving the activity of the catalyst.

[0024] (2) The catalyst prepared by the method of the present invention is used to treat high-concentration pollutants. Taking the dye methylene blue (MB) and sulfamethoxazole (SMX) as examples, other catalysts can treat 5-20 mg / L under the same conditions, while the present invention can treat a high concentration of 100 mg / L, and the degradation rate is faster, and it can be completely degraded within 10 minutes. The performance of the modified catalyst is improved by more than 5-10 times compared with other catalysts. 100 ml of sulfamethoxazole solution (100 mg / L) can be degraded within 10 minutes, and the removal rate reaches 97%. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is the X-ray diffraction pattern of catalysts with different Co contents (x% Co-CN) before water bath modification;

[0026] Figure 2 is the X-ray diffraction pattern of catalysts with different Co contents (Hx%Co-CN) after water bath modification;

[0027] Figure 3 It is the Fourier infrared spectrum of 3.6%Co-CN and H3.6%Co-CN;

[0028] Figure 4 This is a field emission scanning electron microscope image of 3.6% Co-CN;

[0029] Figure 5 is a field emission scanning electron microscope image of H3.6%Co-CN;

[0030] Figure 6 This is the transmission electron microscopy image of 3.6% Co-CN;

[0031] Figure 7 It is the transmission electron microscopy image of H3.6%Co-CN;

[0032] Figure 8 This is a high-angle spherical aberration corrected scanning transmission electron micrograph of 3.6% Co-CN;

[0033] Fig. 9 This is a high-angle spherical aberration-corrected scanning transmission electron micrograph of H3.6%Co-CN;

[0034] Fig.10 This is an atomic force electron microscopy image of H3.6%Co-CN;

[0035] Fig.11 is the X-ray photoelectron spectra of catalysts with different Co contents (x% Co-CN) before water bath modification;

[0036] Fig.12 is the X-ray photoelectron spectra of catalysts with different Co contents (Hx%Co-CN) after water bath modification;

[0037] Fig.13 It is the near-edge structure diagram of Co K-edge X-ray absorption of standard samples (Co foil, CoO, Co3O4, CoPc) and catalysts (3.6% Co-CN, H3.6% Co-CN);

[0038] Fig.14 It is the wavelet transform diagram of the extended edge absorption spectra of the standard samples (Co foil, CoO, Co3O4, CoPc) and catalysts (3.6% Co-CN, H3.6% Co-CN);

[0039] Fig.15 This is the experimental effect diagram of the degradation of methylene blue by catalysts with different Co contents (Hx%Co-CN) after water bath modification;

[0040] Fig.16 This is the experimental effect diagram of H3.6% Co-CN degrading methylene blue at different pH;

[0041] Fig.17This is the experimental effect diagram of H3.6% Co-CN degrading methylene blue under different PMS concentrations.

[0042] Fig.18 This is the experimental effect diagram of the degradation of sulfamethoxazole by catalysts with different Co contents (Hx%Co-CN) after water bath modification;

[0043] Fig.19 This is the experimental effect diagram of H3.6% Co-CN degrading sulfamethoxazole at different pH values.

[0044] Fig. 20 This is the weight chart of the synthetic peeled kg-3.6% Co-CN. DETAILED DESCRIPTION

[0045] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0046] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0047] Example 1

[0048] A low-cost preparation method for a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction comprises the following steps:

[0049] (1) Preparation of 0.8% Co-CN catalyst: Weigh a certain amount of cobalt hydroxide (0.0079 g) and urea (10 g), grind them in an agate mortar until they are completely mixed, transfer them into a 30 ml ceramic crucible, seal it with tin foil, and calcine at 550 °C for 4 h at a heating rate of 4.3 °C / min.

[0050] (2) Modification: Weigh 1 g of the 0.8% Co-CN obtained by calcination in step (1), add 200 ml of deionized water, stir at 90°C for 12 h, filter, wash and dry to obtain modified catalyst H0.8% Co-CN. The H in the catalyst indicates that it has been modified after water bath.

[0051] Example 2

[0052] A low-cost preparation method for a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction comprises the following steps:

[0053] (1) Preparation of 1.8% Co-CN catalyst: Weigh a certain amount of cobalt hydroxide (0.0197 g) and urea (10 g), grind them in an agate mortar until they are completely mixed, transfer them into a 30 ml ceramic crucible, seal them with aluminum foil, and calcine them at 550 °C for 4 h at a heating rate of 4.3 °C / min.

[0054] (2) Modification: Weigh 1 g of the 1.8% Co-CN obtained by calcination in step (1), add 200 ml of deionized water, stir at a constant temperature of 90° C. for 12 h, and obtain the modified catalyst H1.8% Co-CN after suction filtration, washing and drying.

[0055] Example 3

[0056] A low-cost preparation method for a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction comprises the following steps:

[0057] (1) Preparation of 3.6% Co-CN catalyst: Weigh a certain amount of cobalt hydroxide (0.0395 g) and urea (10 g), grind them in an agate mortar until they are completely mixed, transfer them into a 30 ml ceramic crucible, seal it with tin foil, and calcine at 550 °C for 4 h at a heating rate of 4.3 °C / min.

[0058] (2) Modification: Weigh 1 g of the 3.6% Co-CN obtained by calcination in step (1), add 200 ml of deionized water, stir at a constant temperature of 90° C. for 12 h, and obtain the modified catalyst H3.6% Co-CN after suction filtration, washing and drying.

[0059] Example 4

[0060] A low-cost preparation method for a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction comprises the following steps:

[0061] (1) Preparation of 8.0% Co-CN catalyst: Weigh a certain amount of cobalt hydroxide (0.0788 g) and urea (10 g), grind them in an agate mortar until they are completely mixed, transfer them into a 30 ml ceramic crucible, seal it with tin foil, and calcine at 550 °C for 4 h at a heating rate of 4.3 °C / min.

[0062] (2) Modification: Weigh 1 g of the 8.0% Co-CN obtained by calcination in step (1), add 200 ml of deionized water, stir at a constant temperature of 90° C. for 12 h, and obtain the modified catalyst H8.0% Co-CN after suction filtration, washing and drying.

[0063] Example 5

[0064] A low-cost preparation method for a carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction comprises the following steps:

[0065] (1) Preparation of kg-3.6% Co-CN catalyst: Weigh a certain amount of cobalt hydroxide 1.315g and 333g urea, grind them with a grinder until they are completely mixed, transfer them into a 1000ml ceramic crucible, seal them with tin foil, and calcine them at 550℃ for 4h with a heating rate of 4.3℃ / min. Repeat the above operation and take 45 samples and put them into an electric furnace for firing.

[0066] (2) Modification: Weigh 1 g of kg-3.6% Co-CN obtained by calcination in step (1), add 200 ml of deionized water, stir at 90°C for 12 h, filter, wash and dry to obtain a modified catalyst Hkg-3.6% Co-CN. kg represents a kg-grade catalyst prepared by increasing the dosage of the raw materials used.

[0067] Comparative Example 1

[0068] A low-cost preparation method for a carbon nitride-supported single-atom cobalt catalyst for a PMS advanced oxidation reaction comprises the following steps: weighing a certain amount of cobalt hydroxide (0.0395 g) and urea (10 g), grinding them with an agate mortar until they are completely mixed, transferring them into a 30 ml ceramic crucible, sealing them with tin foil, and calcining them at 550° C. for 4 h at a heating rate of 4.3° C. / min; after calcination, a catalyst with 3.6% Co-CN is obtained.

[0069] Experimental Example 1

[0070] Catalytic degradation experiments were carried out using the catalysts prepared by the methods of Examples 1-5 and Comparative Example 1, and the method was as follows:

[0071] Catalyst degradation test under different conditions

[0072] The reaction conditions are as follows:

[0073] Methylene blue solution concentration - 100mg / L

[0074] PMS concentration - 0.5mM (about 0.307g / L)

[0075] Catalyst concentration - 0.1g / L

[0076] The above reaction was carried out in a 250 ml glass beaker, with an initial pH of 7 (±0.1), a 10 mM phosphate buffer solution to maintain a stable pH, a reaction temperature of 25 (±1)° C., and a reaction speed of 500 rpm.

[0077] 10 mg of the catalyst was added to 100 ml of methylene blue solution (100 mg / L methylene blue, 10 mM phosphate buffer solution), ultrasonically dispersed, PMS (0.5 mM) was added, samples were taken at certain intervals, quenched with an equal volume of methanol, and filtered through a 0.22 μm mixed cellulose MCE filter to obtain a sample solution. The concentration of the methylene blue solution was calculated by UV spectrophotometer. The effects of different catalysts tested are shown in Table 1.

[0078] Table 1: Catalysts for the degradation of methylene blue

[0079]

[0080] As shown in Table 1, the modified catalyst (H3.6% Co-CN) of Example 3 of the present invention can completely degrade 100 ml of methylene blue solution (100 mg / L) within 10 minutes, and the removal rate reaches 100%. Comparative Example 1 is an unmodified catalyst, and its removal rate is 85%, which is significantly lower than that of Example 3. The catalyst after water bath can be used to degrade ultra-high concentration dye organic pollutants. Common pollutants are 2-20 mg / L, and this catalyst can reach 100 mg / L, and the degradation efficiency is about 100% in 10 minutes.

[0081] 1. Catalyst degradation test at different pH values

[0082] The catalyst prepared in Example 3 (H3.6% Co-CN) was used for the degradation experiment, and the pH values ​​were adjusted to 3, 5, 7, 9, and 11, respectively. The degradation results are shown in Fig.16 shown. Fig.16 Experiments were conducted under different initial pH conditions, and high removal rates were achieved at 3-11, which has good stability and practical application significance.

[0083] 2. Degradation test of catalyst at different PMS concentrations

[0084] The catalyst prepared in Example 3 (H3.6% Co-CN) was used for the degradation experiment. The degradation results are shown in Fig.17 As shown, the lowest PMS concentration for removing 100 mg / L methylene blue solution is 0.5 mM.

[0085] 3. Degradation test of catalysts with different cobalt contents Degradation experiments were carried out using catalysts with different cobalt contents, as shown in Table 1 and Fig.15 As shown. H3.6%Co-CN has the best performance.

[0086] Experimental Example 2

[0087] Catalyst degradation test under different conditions

[0088] The reaction conditions are as follows:

[0089] Sulfamethoxazole solution concentration - 100mg / L

[0090] PMS concentration - 0.5mM (about 0.307g / L)

[0091] Catalyst concentration - 0.1g / L

[0092] The above reaction was carried out in a 250 ml glass beaker, with an initial pH of 7 (±0.1), a 10 mM phosphate buffer solution to maintain a stable pH, a reaction temperature of 25 (±1)°C, and a reaction speed of 500 rpm. The results of the experiments with different catalysts are shown in Table 2.

[0093] 10 mg of catalyst was added to 100 ml of sulfamethoxazole solution (100 mg / L sulfamethoxazole, 10 mM phosphate buffer solution), ultrasonically dispersed, PMS (0.5 mM) was added, samples were taken at certain intervals, quenched with an equal volume of methanol, and filtered through a 0.22 μm polyethersulfone (PES) filter to obtain a sample solution. The concentration of sulfamethoxazole solution was calculated by high performance liquid chromatography. The effects of different catalysts tested are shown in Table 2.

[0094] Table 2: Catalysts for the degradation of sulfamethoxazole

[0095]

[0096] As shown in Table 2, the modified catalyst (H3.6% Co-CN) of Example 3 of the present invention can degrade 100 ml of sulfamethoxazole solution (100 mg / L) within 10 minutes, and the removal rate reaches 97%. Comparative Example 1 is an unmodified catalyst, and its removal rate is 88%, which is significantly lower than that of Example 3. The catalyst after water bath can be used to degrade ultra-high concentration organic pollutants. Common pollutants are 2-20 mg / L, and this catalyst can reach 100 mg / L, and the degradation efficiency in 10 minutes reaches 97%.

[0097] 1. Degradation test of catalysts with different cobalt contents

[0098] The degradation experiments of sulfamethoxazole were carried out using catalysts with different cobalt contents, as shown in Table 2 and Fig.18 As shown. H3.6%Co-CN has the best performance.

[0099] 2. Catalyst degradation test at different pH values

[0100] The catalyst (H3.6% Co-CN) prepared in Example 3 was used to perform a sulfamethoxazole degradation experiment, and the pH values ​​were adjusted to 3, 5, 7, 9, and 11, respectively. The degradation results are shown in FIG. Fig.19 shown. Fig.19Experiments were conducted under different initial pH conditions. The catalyst performance was best in a neutral environment and could still maintain a good removal rate in a weakly alkaline environment. The effect was poor in extremely acidic and alkaline conditions.

[0101] 3. Preparation of kg-scale catalysts

[0102] The catalyst (kg-3.6% Co-CN) prepared in Example 5 was weighed (the beaker was peeled), as shown in Fig. 20 As shown, the results indicate that the one-step pyrolysis method of the present invention can be used to prepare kg-scale single-atom catalysts.

[0103] Experimental Example 3

[0104] The performance of the catalysts in Examples 1-5 and Comparative Example 1 was tested and characterized.

[0105] X-ray diffraction (XRD) patterns were collected using an X-ray diffractometer to characterize the crystal structure of the catalyst;

[0106] Fourier transform infrared spectrometer was used to collect Fourier transform infrared spectra (FT-IR) and characterize the functional groups of the catalyst;

[0107] Scanning electron microscope (SEM) images were collected using a field emission scanning electron microscope to characterize the microscopic morphology of the catalyst;

[0108] Field emission transmission electron microscopy (TEM) images were collected to further characterize the catalyst microstructure;

[0109] High-angle annular dark-field spherical aberration-corrected scanning transmission electron microscopy (HADDF-STEM) images were collected to characterize the single atoms in the catalyst;

[0110] Atomic force electron microscopy (AFM) images were collected using an atomic force electron microscope to measure the thickness of the nanosheets;

[0111] X-ray photoelectron spectrometer (XPS) was used to collect the Co element on the catalyst surface;

[0112] The near-edge and extended-edge X-ray absorption of Co K-edge were collected using a synchrotron radiation source to determine the catalyst valence state and atomic distance.

[0113] The absorbance of methylene blue was tested by ultraviolet spectrophotometer, and the degradation data of methylene blue was obtained.

[0114] The concentration of sulfamethoxazole was tested by high performance liquid chromatography, and the degradation data of sulfamethoxazole was obtained.

[0115] Figure 1 It shows that the incorporation of Co element does not change the crystal structure of graphitic carbon nitride, where the 100 and 002 crystal planes represent the tri-s-triazine ring structure within the graphitic carbon nitride layer and the interlayer stacking, respectively. As the metal content increases, the intralayer structure gradually breaks.

[0116] Figure 2 This indicates that the water bath has no significant effect on the crystal structure of each catalyst.

[0117] Figure 3 This indicates that the functional groups of the catalyst did not change before and after the water bath.

[0118] Figure 4 and Figure 5 This shows the nanosheet structure of the catalyst. After being water-bathed, the catalyst gradually unfolds and flattens from a bowl-shaped curled nanosheet.

[0119] Figure 6 and Figure 7 The curling and flatness of the nanosheet edges can be clearly contrasted, which is consistent with the characterization results of field emission scanning electron microscopy.

[0120] Figure 8 and Fig. 9 The existence of single atoms on the nanosheets can be observed. Before and after water bath modification, they are single atom catalysts without agglomeration.

[0121] Fig.10 The thickness of the catalyst after water bath modification was measured to be about 0.7 nm, approximately two atomic layers thick.

[0122] Fig.11 and Fig.12 By comparison, it was found that water bath modification increased the Co content on the catalyst surface and exposed more active sites.

[0123] Fig.13 This indicates that the catalyst valence state is around +2.

[0124] Fig.14 This indicates that there is no Co-Co bond in the catalyst and Co exists in the form of a single atom.

[0125] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A cheap preparation method of carbon nitride supported single atom cobalt catalyst for PMS advanced oxidation reaction, characterized in that: The following steps are involved: (1) grinding cobalt hydroxide and urea, mixing them, transferring them into a crucible, sealing them, and calcining them to obtain an x% Co-CN catalyst; (2) The x% Co-CN catalyst prepared in step (1) is added into water, stirred at a certain temperature, and then filtered, washed and dried to obtain a modified Hx% Co-CN catalyst.

2. The inexpensive preparation method of carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction according to claim 1, characterized in that: The mass ratio of the cobalt hydroxide and urea mixed in step (1) is 2-100:10000.

3. The inexpensive preparation method of carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction according to claim 1, characterized in that: The calcination temperature in step (1) is 500-600° C., the calcination time is 1-10 h, and the heating rate is 2-10° C. / min.

4. The inexpensive preparation method of carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction according to claim 1, characterized in that: Step (2) The mass ratio of the x% Co-CN catalyst to the volume ratio of water is 1:1000-10000 g / ml.

5. The inexpensive preparation method of carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction according to claim 1, characterized in that: Step (2) is stirred at 50-95° C. for 1-24 h.

6. The inexpensive preparation method of carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction according to claim 1, characterized in that: Step (2) is stirred at 90° C. for 1-24 h.

7. The inexpensive preparation method of carbon nitride-supported single-atom cobalt catalyst for PMS advanced oxidation reaction according to claim 1, characterized in that: The mass fraction of the single-atom cobalt loading of the prepared modified Hx%Co-CN catalyst is 0.8-8wt%.

Citation Information

Patent Citations

  • Carbon composite material loaded with transition metal single atoms as well as preparation method and application of carbon composite material

    CN111224087A

  • Co-CN photocatalyst based on ZIF-L derivation as well as preparation method and application of Co-CN photocatalyst

    CN117718073A

  • Oxygen-doped carbonitride / Co3O4 heterojunction photocatalyst as well as preparation method and application thereof

    CN117861706A

  • Non-noble element catalysts and methods for making

    US20170354953A1

  • Preparation Method and Application of Non-noble Metal Single Atom Catalyst

    US20220042184A1