Tubular carbon nitride ZIF-8 composite material as well as preparation method and application thereof
By growing a high-loading ZIF8 layer of tubular carbon nitride@ZIF-8 composite material on the surface of graphite phase carbon nitride, as a photocatalyst, the serious problem of photogenerated carrier recombination in g-C3N4 degradation of tetracycline antibiotics is solved. Efficient antibiotic removal and circulation stability are achieved.
Patent Information
- Application Number
- CN202410721523.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-08
AI Technical Summary
When the existing photocatalyst g-C3N4 is used to treat tetracycline antibiotic residues, due to the layer-by-layer stacking structure, the photogenerated carriers recombine seriously and have few active sites, making it difficult to effectively degrade. Moreover, traditional methods are difficult to treat tetracycline drug residues.
Tubular carbon nitride@ZIF-8 composite material is used as a photocatalyst. By growing a ZIF8 layer on the surface of graphite phase carbon nitride, the loading capacity is increased to 70%-95% to improve the photocatalytic performance and enhance the antibiotic degradation efficiency.
It achieves efficient removal of antibiotics in water and good cycle stability, significantly improves photocatalytic performance, can effectively degrade antibiotics such as tetracycline hydrochloride, norfloxacin and ciprofloxacin, and performs well in multiple cycles of use. Stay steady.
Smart Images

Figure CN118744014A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst technology, and in particular to a tubular carbon nitride@ZIF-8 composite material and a preparation method and application thereof. Background Art
[0002] Among all antibiotics, tetracycline ranks second in the world in terms of production and usage. It is widely used in the treatment of human and animal infectious diseases. Its residues in the external environment can induce the development of drug-resistant pathogens and cause serious problems to human health.
[0003] Therefore, it is of great significance to find an effective method to remove antibiotic residues. In practice, due to the post-treatment of adsorbents and the antibacterial properties of tetracycline, traditional physical adsorption and biodegradation methods are difficult to treat tetracycline drug residues. The technologies currently commonly used for tetracycline treatment are mainly Fenton reagent oxidation, ozone oxidation and photocatalytic oxidation.
[0004] In the treatment of wastewater containing tetracycline antibiotics, efficient photocatalysts with water, heat, and light stability and visible light response are usually required. Among the many photocatalysts, g-C3N4 has the characteristics of low cost, high physicochemical stability, and visible light response, and has good prospects in visible light-driven degradation of tetracycline antibiotics. However, g-C3N4 also has major disadvantages, mainly its stacked block structure, which leads to serious recombination of photogenerated carriers and few active sites. Therefore, it is urgent to provide a solution to improve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a tubular carbon nitride @ ZIF-8 composite material and a preparation method and application thereof, which can effectively remove antibiotics in water and has good cycle stability and high-efficiency catalytic performance.
[0006] In a first aspect, the present invention provides a tubular carbon nitride@ZIF8 composite material, comprising tubular graphite phase carbon nitride, and a ZIF8 layer grown on the surface of the graphite phase carbon nitride, and the loading amount of the ZIF8 layer on the surface of the graphite phase carbon nitride is 70%-95%.
[0007] In a second aspect, the present invention provides a method for preparing a tubular carbon nitride@ZIF8 composite material, comprising the following steps:
[0008] Ultrasonic dispersion of tubular graphite-phase carbon nitride in a zinc salt solution to prepare a precursor mixed solution;
[0009] The organic ligand solution and the precursor mixed solution are stirred and reacted, and then separated, washed and dried to obtain a tubular carbon nitride@ZIF8 composite material.
[0010] Optionally, the solute in the zinc salt solution includes zinc acetate and zinc nitrate, preferably zinc acetate.
[0011] Optionally, the ligand solute in the organic ligand solution includes 2-methylimidazole.
[0012] Optionally, after the organic ligand solution and the precursor mixed solution are stirred for reaction, the mass mixing ratio of the solute in the zinc salt solution, the ligand solute and the graphite phase carbon nitride is (3-12):(9-36):1, preferably 5.5:16.5:1.
[0013] Optionally, the process of separating, washing and drying to obtain the tubular carbon nitride@ZIF8 composite material includes:
[0014] The reaction solution after stirring the reaction is centrifuged to collect the solids;
[0015] The solid was washed with an alcohol aqueous solution and dried at 55-65°C to obtain a tubular carbon nitride@ZIF8 composite material.
[0016] Optionally, the loading amount of ZIF8 in the tubular carbon nitride@ZIF8 composite material is 70%-95%.
[0017] Optionally, the method for preparing the tubular graphite phase carbon nitride comprises the following steps:
[0018] The melamine solution and the thiocyanamide solution are mixed and stirred to react to obtain a cyanamide reaction solution;
[0019] After the solid precipitate in the cyanamide reaction solution is separated and dried, it is sintered in a nitrogen atmosphere at 450-550° C. and ground after cooling to obtain tubular graphite phase carbon nitride.
[0020] In a third aspect, the present invention also provides the use of tubular carbon nitride@ZIF8 composite materials as photocatalysts in the photocatalytic degradation of antibiotics, wherein the antibiotics include tetracycline hydrochloride, norfloxacin and ciprofloxacin.
[0021] Optionally, the mixing ratio of the photocatalyst to the antibiotic is 10:1. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A schematic diagram of the synthesis route of the tubular carbon nitride@ZIF8 composite material provided by the present invention;
[0023] Figure 2 SEM characterization images of TCN, ZIF8, TCN / ZIF8-20, TCN / ZIF8-40 and TCN / ZIF8-60 provided by the present invention;
[0024] Figure 3The N2 adsorption-desorption isotherms of TCN, ZIF8 and TCN / ZIF8-40 provided by the present invention;
[0025] Figure 4 The EDS characterization element mapping diagram of TCN / ZIF8-40 provided by the present invention;
[0026] Figure 5 XRD spectra of TCN, ZIF8 and TCN / ZIF8-40 provided by the present invention;
[0027] Figure 6 FT-IR spectra of TCN, ZIF8 and TCN / ZIF8-40 provided by the present invention;
[0028] Figure 7 XPS spectra of TCN, ZIF8 and TCN / ZIF8-40 provided by the present invention;
[0029] Figure 8 UV-visible diffuse reflectance spectra and PL spectra of TCN, ZIF8, TCN / ZIF8-20, TCN / ZIF8-40 and TCN / ZIF8-60 provided by the present invention;
[0030] Fig. 9 The standard absorbance curve of the tetracycline hydrochloride solution provided by the present invention at 357nm;
[0031] Fig.10 A degradation efficiency curve diagram of TCN, ZIF8, TCN / ZIF8-20, TCN / ZIF8-40 and TCN / ZIF8-60 provided by the present invention when performing tetracycline hydrochloride degradation;
[0032] Fig.11 A degradation performance diagram of TCN / ZIF8-40 provided by the present invention when performing cyclic degradation of tetracycline hydrochloride;
[0033] Fig.12 A degradation efficiency curve diagram of tetracycline hydrochloride degradation after TCN / ZIF8-40 provided by the present invention is compounded with different free radical quenchers;
[0034] Fig.13 It is a degradation efficiency curve diagram of the TCN / ZIF8-40 provided by the present invention when photocatalytically degrading a norfloxacin solution and a ciprofloxacin solution;
[0035] Fig.14 The SEM images of TCN / ZIF8-40 provided by the present invention before and after tetracycline hydrochloride degradation;
[0036] Fig.15The XRD diagram of TCN / ZIF8-40 provided by the present invention before and after tetracycline hydrochloride degradation. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0038] The embodiment of the present invention provides a method for preparing tubular graphite phase carbon nitride, comprising the following steps:
[0039] Y1, mixing a melamine solution and a thiocyanamide solution and stirring the mixture to obtain a cyanamide reaction solution;
[0040] Y2. After separating and drying the solid precipitate in the cyanamide reaction solution, sintering it in a nitrogen atmosphere at 450-550° C., and grinding it after cooling to obtain tubular graphite phase carbon nitride (TCN).
[0041] In fact, after the melamine solution and the thiomelamine solution are mixed in step Y1, the molar ratio of melamine in the melamine solution to thiomelamine in the thiomelamine is 1:1.
[0042] In some embodiments, when performing step Y1, melamine and thiocyanate may be mixed in solid form and then added to an alcohol aqueous solution and stirred to dissolve. Specifically, the alcohol aqueous solution may be a solution obtained by mixing deionized water and methanol.
[0043] In fact, when performing step Y1, after the melamine solution and the thiomelamine solution are mixed, they are treated under an ultrasonic environment so that the melamine and the thiomelamine are evenly dispersed. Specifically, the ultrasonic treatment time can be controlled to be 5-15 minutes.
[0044] In fact, when performing step Y1, the melamine solution and the thiocyanamide solution are mixed and reacted under stirring for 10-14 hours to obtain a cyanamide reaction solution. Specifically, during the stirring reaction, the rotation speed is controlled at 200-300 rpm.
[0045] In fact, when executing step Y2 to separate and dry the solid precipitate in the cyanamide reaction solution, the cyanamide reaction solution is filtered to obtain a solid precipitate, and the solid precipitate is washed with deionized water to recover a light yellow solid, which is then dried at 60-80°C.
[0046] In fact, when performing the sintering step Y2, the dried solid is sintered at 450-550° C. for 1.5-2.5 hours.
[0047] In fact, when performing the sintering step Y2, the dried solid is heated to 450-550°C at a rate of 4-5°C / min in a nitrogen environment and then kept at this temperature for 1.5-2.5h.
[0048] The embodiment of the present invention provides a method for preparing a tubular carbon nitride@ZIF8 composite material, comprising the following steps:
[0049] S1, ultrasonically dispersing tubular graphite-phase carbon nitride in a zinc salt solution to prepare a precursor mixed solution;
[0050] S2. After stirring the organic ligand solution and the precursor mixed solution to react, the mixture is separated, cleaned and dried to obtain a tubular carbon nitride@ZIF8 composite material.
[0051] In fact, the ligand solute in the organic ligand solution includes 2-methylimidazole; the solute in the zinc salt solution includes zinc acetate and zinc nitrate, preferably zinc acetate.
[0052] In some embodiments, after the organic ligand solution and the precursor mixture are stirred to react, the mass mixing ratio of the solute in the zinc salt solution, the ligand solute and the graphite phase carbon nitride is (3-12):(9-36):1, preferably 5.5:16.5:1.
[0053] In some embodiments, the process of separating, washing, and drying in step S2 to obtain a tubular carbon nitride @ZIF8 composite material includes: centrifuging the reaction solution after the stirring reaction and collecting the solids; washing the solids with an alcohol-water solution, and drying at 55-65°C to obtain a tubular carbon nitride @ZIF8 composite material.
[0054] Specifically, after the tubular carbon nitride@ZIF8 composite material is prepared in step S2, the loading amount of ZIF8 is 70%-95%.
[0055] Specifically, see Figure 1 In the preparation process of tubular carbon nitride@ZIF8 composite materials, graphite phase carbon nitride is added to zinc salt solution for ultrasonic dispersion, so that zinc ions are evenly attached to the surface of tubular carbon nitride. After adding organic ligand solution, ZIF8 grows evenly on the surface of tubular carbon nitride.
[0056] In fact, the present invention also provides a tubular carbon nitride@ZIF8 composite material prepared by any of the above-mentioned preparation methods, comprising tubular graphite phase carbon nitride, and a ZIF8 layer grown on the surface of the graphite phase carbon nitride, and the loading amount of the ZIF8 layer on the surface of the graphite phase carbon nitride is 70%-95%.
[0057] Preparation Example 1
[0058] This preparation example 1 provides a method for preparing tubular graphite phase carbon nitride, comprising the following steps:
[0059] Y1, weighing 4mmol of melamine and 4mmol of thiocyanamide, adding 120mL of deionized water and 25mL of methanol, ultrasonically treating for 10min, stirring at a speed of 600rpm for 10min, and then stirring at a speed of 250rpm for 12h to obtain a cyanamide reaction solution;
[0060] Y2. The cyanamide reaction solution was filtered and then the precipitate was washed. The light yellow solid was recovered and placed in a 70°C oven for drying for 12 hours. The solid was then transferred to a porcelain boat. The temperature was raised from room temperature to 500°C at a rate of 4.6°C / min under a nitrogen atmosphere. The temperature was kept for 2 hours. The solid was cooled to room temperature and then ground into a powdered tubular graphite carbon nitride (TCN).
[0061] Example 1
[0062] This embodiment 1 provides a method for preparing a tubular carbon nitride@ZIF8 composite material, comprising the following steps:
[0063] S1. Dissolve 1 mmol of ZnAc2 in 25 mL of methanol to prepare a zinc acetate solution; dissolve 8 mmol of 2-methylimidazole in 25 mL of methanol to prepare a ligand solution; weigh 40 mg of TCN prepared in Preparation Example 1, add it to the zinc acetate solution and mix it by ultrasonic for 20 minutes to prepare a precursor mixture;
[0064] S2. The ligand solution and the precursor mixture were stirred and mixed at a rotation speed of 600 rpm and reacted for 2 hours. The solid was collected by centrifugation and washed with methanol. The solid was placed in an oven at 60°C and dried for 12 hours to obtain a tubular carbon nitride @ ZIF-8 composite material (TCN / ZIF8-40).
[0065] Example 2
[0066] This Example 2 provides a method for preparing a tubular carbon nitride @ ZIF8 composite material, which is different from Example 1 in that in step S1, 20 mg of TCN prepared in Preparation Example 1 is added to a zinc acetate solution and ultrasonically mixed for 20 minutes to obtain a precursor mixed solution, and in step S2, a tubular carbon nitride @ ZIF-8 composite material (TCN / ZIF8-20) is obtained.
[0067] Example 3
[0068] This Example 3 provides a method for preparing a tubular carbon nitride @ ZIF8 composite material, which is different from Example 1 in that in step S1, 60 mg of TCN prepared in Preparation Example 1 is added to a zinc acetate solution and ultrasonically mixed for 20 minutes to obtain a precursor mixed solution, and in step S2, a tubular carbon nitride @ ZIF-8 composite material (TCN / ZIF8-60) is obtained.
[0069] Comparative Example 1
[0070] This comparative example 1 provides a method for preparing ZIF8, which is different from Example 1 in that TCN prepared in Preparation Example 1 is not added in step S1, and the ligand solution and zinc acetate solution are stirred and mixed in step S2 to prepare ZIF8.
[0071] Morphological characterization
[0072] SEM characterization: TCN, ZIF8, TCN / ZIF8-20, TCN / ZIF8-40, TCN / ZIF8-60 were characterized using emission field scanning electron microscopy. Figure 2 As shown, Figure 2 (a) is the SEM image of TCN. Figure 2 (b) is the SEM image of ZIF8. Figure 2 (c) is the SEM image of TCN / ZIF8-40. Figure 2 (d) is the SEM image of TCN / ZIF8-60. Figure 2 (e) is the SEM image of TCN / ZIF8-20.
[0073] from Figure 2 (a) It can be seen that the graphite carbon nitride (TCN) prepared in Preparation Example 1 of the present invention has a hollow tubular structure. Compared with the traditional layer-by-layer stacked block structure, TCN has a higher specific surface area, providing more active sites for the growth of ZIF8, and can also provide more active sites for photocatalytic reactions.
[0074] from Figure 2 (b) It can be seen that pure ZIF8 has a polyhedral structure with a diameter of about 900 nm. Compared with the diameter of TCN, there is a theoretical basis for ZIF8 to grow on the surface of TCN. Figure 2 (c) It can be seen that ZIF8 in TCN / ZIF8-40 grows uniformly on the TCM surface, while Figure 2 (d) In TCN / ZIF8-60, the ZIF8 material coverage is too small, and large pieces of ZIF8 can be seen. In the SEM image, large pieces of TCN at the bottom are exposed. Figure 2 (e) The ZIF8 in TCN / ZIF8-20 grows too densely, and large pieces of ZIF8 accumulate on the surface of TCN, which indicates that the ZIF8 content is too high. Too much or too little ZIF8 will affect the separation and migration ability of photogenerated carriers in TCN / ZIF8 materials, resulting in a relatively reduced photocatalytic performance.
[0075] BET characterization: Using nitrogen as the adsorbent, the specific surface area of TCN, ZIF8, and TCN / ZIF8-40 was tested. The characterization results are shown in Figure 3 As shown, Figure 3 (a) is the N2 adsorption-desorption isotherm of TCN. Figure 3 (b) is the N2 adsorption-desorption isotherm of ZIF8. Figure 3 (c) in the figure is the N2 adsorption-desorption isotherm diagram of TCN / ZIF8-40.
[0076] from Figure 3 (a) It can be seen that TCN is an obvious IV type adsorption isotherm, belonging to the H3 type hysteresis loop. Figure 3 (b) and Figure 3 (c) It can be seen that both ZIF8 and TCN / ZIF8-40 belong to the || type adsorption isotherm, showing an S-shaped curve. The monolayer adsorption is saturated at the low pressure inflection point. Figure 3 (b) shows that the BET specific surface area of ZIF8 is 742.493 cm 3 / g, which indicates that ZIF8 has a mesoporous structure. Figure 3 It can be seen from (c) that with the help of ZIF8, the specific surface area of TCN / ZIF8-40 has been greatly improved. At the same time, the test pore size of TCN / ZIF8-40 is smaller than that of ZIF8, which indicates that when ZIF8 grows on the TCN surface, it is relatively regular, avoiding the problem of large-scale stacking of ZIF8 on the TCN surface.
[0077] EDS characterization: After EDS characterization of TCN / ZIF8-40 using energy dispersive X-ray spectrometer, the results are as follows Figure 4 As shown, Figure 4 (a) is the SEM image of TCN / ZIF8-40 at a scale of 10 μm. Figure 4 (b), (c), (d), and (e) are the element mapping diagrams of C, N, Zn, and O, respectively. Figure 4It can be seen that there are obvious C, N and Zn elements on the surface of TCN / ZIF8-40, while the content of O element is relatively small, which indicates that ZIF8 is successfully composited on TCN.
[0078] Spectrum characterization: XRD characterization of TCN, ZIF8, and TCN / ZIF8-40 was performed using an X-ray diffractometer. The results are as follows: Figure 5 As shown, Figure 5 (b) is the detailed crystal structure at 2θ of 20°-35°; and Fourier transform spectrometer was used to perform FT-IR characterization on TCN, ZIF8, and TCN / ZIF8-40, respectively. The results are shown in Figure 6 shown.
[0079] from Figure 5 (a) It can be seen that TCN has two characteristic diffraction peaks near 2θ of 13° and 27°, which correspond to the (100) and (002) crystal planes of g-C3N4 (standard card JCPDSNO.87-1526), respectively. The crystal structure of ZIF8 can be clearly seen on TCN / ZIF8-40, but the crystal structure of TCN is almost invisible. This is because the crystal strength of ZIF8 is too different from that of TCN, resulting in the lack of obvious typical characteristic peaks of TCN. Figure 5 As can be seen in (b), TCN / ZIF8-40 still corresponds to ZIF8. At the same time, it can be seen that TCN / ZIF8-40 has an obvious protrusion at around 27°, which corresponds to the characteristic diffraction peak of TCN at 2θ of 27°, indicating that TCN and ZIF-8 are successfully composited.
[0080] from Figure 6 It can be seen that in the absorption curve of ZIF8, at about 420 cm -1 A sharp absorption peak can be observed at 900-1350cm, which is due to the stretching vibration of the Zn-N bond in ZIF8. -1 and 650-800cm -1 The broad absorption bands of 3000-3600cm-1 and 3000-3600cm-2 can be attributed to the in-plane and out-of-plane bending vibrations of the imidazole ring, respectively. -1 Corresponds to the stretching vibration of the NH bond or the OH bond vibration in H2O, 1200-1600cm -1 The corresponding is the stretching vibration of the CN heterocycle, 800cm -1 This corresponds to the bending vibration of the triazine ring structure. At the same time, it can be seen that both TCN and ZIF8-40 have the above characteristic absorption peaks, except that ZIF8 has a peak at 650-800 em -1 The wide absorption band is probably due to the fact that it is in the 1200-1600 em band with TCN. -1The absorption peaks at overlap, and its absorption intensity is lower than that of TCN in this band, so the peaks are covered.
[0081] XPS characterization: X-ray photoelectron spectrometer was used to perform XPS characterization on TCN, ZIF8, and TCN / ZIF8-40. The results are shown in the figure. Figure 7 As shown; among them, Figure 7 (a) is the C1s spectrum of TCN and TCN / ZIF8-40. Figure 7 (b) is the N1s spectrum of TCN and TCN / ZIF8-40. Figure 7 (c) in the figure is the Zn 2p spectrum of ZIF8 and TCN / ZIF8-40. Figure 7 (d) is the O1s spectrum of ZIF8 and TCN / ZIF8-40. Figure 7 (e) in the figure is the full elemental spectrum of TCN, ZIF8, and TCN / ZIF8-40.
[0082] from Figure 7 (a) It can be seen that the 284.8 eV in TCN corresponds to the C-C bond in the graphitized carbon structure, and the 285.9 eV corresponds to the C-NH bond at the edge of the carbon nitride molecular skeleton. X (x=1,2) bond, 288.3eV corresponds to the NC=N bond in the carbon nitride skeleton, and 293.7eV corresponds to the delocalized electrons in the carbon nitrogen heterocycle. At the same time, it can be seen that compared with TCN, except for the peak at 286.2eV, the peaks at 287.9eV and 292.7eV of TCN / ZIF8-40 are negatively shifted. This is because ZIF8 has a stronger electron-withdrawing ability. Charge transfer occurs at the interface between TCN and ZIF8, resulting in a slight decrease in the binding energy of the carbon nitride structure corresponding to TCN. The peak at 286.2eV is speculated to be related to the imidazole structure in ZIF8. The C-NH x The (x=1, 2) structural features are covered by the C-OH structure in ZIF8.
[0083] from Figure 7 (b) It can be seen that the 398.8eV of TCN represents the CN=C structure in the carbon nitride skeleton, the 400.3eV represents the N-(C)3 structure in the carbon nitride skeleton, the 401.3eV represents the CNH structure at the edge of the carbon nitride skeleton, and the 404.5 represents the delocalized electrons in the carbon-nitrogen heterocycle. It can be seen that the corresponding peaks of TCN / ZIF8-40 are all negatively shifted compared to TCN, which is inferred to be a charge transfer between TCN and ZIF8, which is consistent with the conclusion of the above C1s spectrum.
[0084] from Figure 7(c) It can be seen that ZIF8 has two characteristic peaks. The peak at 1044.7 eV corresponds to Zn 2p 1 / 2 , 1021.7eV corresponds to Zn 2p 3 / 2 TCN / ZIF8-40 also has two characteristic peaks, and the binding energy positions are basically consistent with it, but the peak values are positively shifted by 0.3eV, indicating that the binding energy of ZIF8 increases after the complex with TCN, which is consistent with the above speculation.
[0085] from Figure 7 (d) It can be seen that the peak at 531.6 eV in ZIF8 corresponds to the Zn-O bond, and the peak at 533.0 eV corresponds to the COH bond. The peaks at the same positions in TCN / ZIF8-40 all shift positively, which is consistent with the above inference. Figure 7 (e) It can be seen that although ZIF8 also has C, N and O elements in TCN, the intensities of C and N elements are different. By comparing the C and N element intensities of TCN / ZIF8-40, we can see the successful recombination of ZIF8 and TCN.
[0086] Photoelectric performance characterization: UV-visible spectrometer was used to characterize the spectral response range of TCN, ZIF8, TCN / ZIF8-20, TCN / ZIF8-40, and TCN / ZIF8-60 at a wavelength of 300-800nm. The results are shown in the figure. Figure 8 As shown in (a), PL spectra of TCN, TCN / ZIF8-20, TCN / ZIF8-40, and TCN / ZIF8-60 were characterized as follows Figure 8 As shown in (b) in .
[0087] from Figure 8 (a) It can be seen that TCN / ZIF8-40 has a stronger absorption peak and a slightly wider light absorption range than TCN and other composite materials, indicating that it has a stronger absorption capacity for light. Generally speaking, the peak intensity of the PL spectrum is proportional to the recombination rate of photogenerated carriers in the semiconductor. Figure 8 (b) It can be seen that TCN has the highest peak intensity, and its photogenerated carrier recombination is serious. After recombination with ZIF8, its PL peak intensity is significantly reduced, which means that TCN / ZIF8 material has more efficient photogenerated carrier separation and migration efficiency. This conclusion is consistent with the previous XPS test conclusion. Among them, it can be found that TCN / ZIF8-40 has the lowest peak intensity, indicating that its photogenerated carrier recombination rate is the lowest.
[0088] Performance Testing
[0089] Feasibility analysis:
[0090] Tetracycline hydrochloride solutions with concentrations of 10 ppm, 20 ppm, 30 ppm, 40 ppm and 50 ppm were prepared respectively, which were recorded as TC1 to TC5 respectively. The absorbance of TC1 to TC5 was scanned at 357 nm using an ultraviolet-visible spectrophotometer. The obtained absorbances were recorded as A1 to A5 respectively. The standard absorbance curve of TC-HCl solution was plotted with the concentration of tetracycline hydrochloride solution as the abscissa and the corresponding absorbance A as the ordinate, as shown in FIG. Fig. 9 shown.
[0091] from Fig. 9 It can be seen that the linear regression equation of the standard absorbance curve of TC-HCl at 357nm is Y=0.03202X-0.0004, and the correlation coefficient R 2 =0.9995, which indicates that the concentration of TC-HCl solution is positively correlated with the absorbance, and the correlation is high. Therefore, it is feasible to use UV-visible spectrophotometer to test the degradation performance of TC-HCl.
[0092] Five groups of tetracycline hydrochloride solutions with a concentration of 40 ppm were prepared, and the absorbance was scanned at 357 nm using a UV-visible spectrophotometer. The absorbance data obtained were 1.268, 1.270, 1.267, 1.261, and 1.271, respectively. The experimental precision was evaluated by the standard deviation (SD) and relative standard deviation (RSD):
[0093]
[0094]
[0095] Through calculation, it can be known that the SD of the above five groups of tetracycline hydrochloride solutions with a concentration of 40ppm is 0.003507, RSD is 0.002767. Generally speaking, the smaller the SD value and RSD value of the solution with the same concentration, the smaller the experimental error. Therefore, this experiment uses UV-visible spectrophotometer to analyze the degradation degree of TC-HCl with good precision.
[0096] A tetracycline hydrochloride solution with a concentration of 40 ppm was prepared, and samples were taken after 0 min, 20 min, 40 min and 60 min in dark conditions. The absorbance was measured by UV-visible spectrophotometer, and the absorbance values were 1.262, 1.259, 1.263 and 1.258, respectively. The SD was calculated to be 0.00217 and the RSD was calculated to be 0.00172, which shows that the tetracycline hydrochloride solution has good stability in dark conditions.
[0097] In summary, the absorbance monitoring of TC-HCl solution using UV-visible spectrophotometer can monitor the concentration change of tetracycline hydrochloride in real time and calculate the degradation efficiency. The experimental accuracy is determined by the standard deviation and relative standard deviation, which shows that it is feasible to use UV-visible spectrophotometer to detect the degradation rate of TC-HCl solution.
[0098] Tetracycline hydrochloride degradation:
[0099] Six groups of 100 mL tetracycline hydrochloride solutions with a concentration of 40 ppm were prepared. After measuring the absorbance at 357 nm using an ultraviolet-visible spectrophotometer, the six groups of tetracycline hydrochloride solutions were randomly divided into five experimental groups and one blank group. In a dark environment, 40 mg of TCN / ZIF8-40 prepared in Example 1, 40 mg of TCN / ZIF8-20 prepared in Example 2, 40 mg of TCN / ZIF8-60 prepared in Example 3, 40 mg of TCN prepared in Preparation Example 1, and 40 mg of ZIF8 prepared in Comparative Example 1 were added to the five experimental groups, respectively. After adsorption for 30 min to reach saturated adsorption and then measuring the absorbance, a photocatalytic degradation experiment was carried out under a 300 W xenon lamp. Samples were taken every 20 min under illumination for absorbance measurement, and the absorbance data were recorded and converted into tetracycline hydrochloride concentrations, as shown in FIG. Fig.10 shown.
[0100] from Fig.10 It can be seen that TCN / ZIF8-40 has a relatively better photocatalytic degradation performance, and the degradation efficiency of tetracycline hydrochloride can reach 82% within 1 hour. This is because TCN / ZIF8-40 has an excellent charge transfer interface, and the photogenerated carriers are not easy to recombine inside, which leads to its high efficiency photocatalytic degradation performance. However, the surface recombination of TCN / ZIF8-20 and TCN / ZIF8-60 is not uniform, which has a certain impact on its photocatalytic performance. At the same time, it can be seen from the blank example that tetracycline hydrochloride is extremely difficult to degrade in the light environment without a photocatalyst, which further illustrates the stability of tetracycline hydrochloride and the necessity of photocatalysts in the degradation system.
[0101] Recyclability test:
[0102] 100 mL of a 40 ppm tetracycline hydrochloride solution was prepared, and 40 mg of TCN / ZIF8-40 prepared in Example 1 was used to perform a cyclic degradation experiment under 300 W xenon lamp irradiation. Each degradation reaction lasted for 1 h. After each degradation experiment, the photocatalyst was collected by centrifugation and washed with deionized water and ethanol and then dried. The degradation performance during the cyclic degradation test was as follows: Fig.11 shown.
[0103] from Fig.11It can be seen that after multiple cycles of experiments, the degradation efficiency of TCN / ZIF8-40 remains good, which illustrates the performance stability of TCN / ZIF8-40 in the tetracycline hydrochloride degradation system.
[0104] Degradation mechanism study:
[0105] Five groups of 100 mL tetracycline hydrochloride solutions with a concentration of 40 ppm were prepared. After adding 40 mg of TCN / ZIF8-40 prepared in Example 1 at room temperature, the five groups of tetracycline hydrochloride solutions were randomly divided into four experimental groups and one blank group. Saturated adsorption was carried out for 30 min in a dark environment. After adding 520 mg (50 mmol) of ammonium oxalate, 540 mg (50 mmol) of p-benzoquinone, 4 mL of tert-butyl alcohol and 88 μL (10 mmol) of furfuryl alcohol to the tetracycline hydrochloride solutions of the four experimental groups, degradation tests were carried out under a 300 W xenon lamp. Samples were taken at 0 min, 20 min, 40 min and 60 min, and the absorbance data obtained were converted geometrically as follows: Fig.12 shown.
[0106] In the process of organic matter degradation, photocatalysts often rely not on the catalyst itself, but on some active substances produced by light excitation. These common active substances are generally superoxide free radicals (O2 - ), singlet oxygen ( 1 O2), hydroxyl radicals (-OH) and holes (h + ), while the free radical captured by p-benzoquinone is superoxide radical (O2 - ), the free radical captured by tert-butyl alcohol is hydroxyl radical (-OH), and the free radical captured by furfuryl alcohol is singlet oxygen ( 1 O2), the free radicals captured by oxalic acid are holes (h + ).
[0107] from Fig.12 It can be seen that the photocatalytic degradation of TCN / ZIF8-40 with the addition of ammonium oxalate is significantly reduced, which indicates that in the photocatalytic degradation system of tetracycline hydrochloride, holes (h + ) plays a major role. At the same time, it can be seen that the addition of benzoquinone also significantly affects the degradation efficiency of the degradation system. Therefore, superoxide radicals (O2 - ) also has a certain catalytic effect in the degradation system.
[0108] Degradation of other organic pollutants:
[0109] 100 mL of 20 ppm norfloxacin (NOR) solution, 100 mL of 20 ppm ciprofloxacin (CIP) solution, and 100 mL of 40 ppm tetracycline hydrochloride solution were prepared without adding other pro-oxidants. In a dark environment, 40 mg of TCN / ZIF8-40 prepared in Example 1 was respectively put into CIP solution, TC-HCl solution, and CIP solution. After saturated adsorption for 30 min, the mixture was irradiated under a 300 W xenon lamp. Samples were taken at 0 min, 20 min, 40 min, and 60 min of photocatalysis. The absorbance data obtained were converted proportionally as shown in the following figure. Fig.13 shown.
[0110] from Fig.13 It can be seen that TCN / ZIF8-40 also has a strong degradation efficiency for NOR and CIP. Within a reaction time of 1 hour, NOR can be degraded by 70% and CIP can be degraded by 72%. At the same time, there is no need to add co-catalysts such as hydrogen peroxide or potassium persulfate during the photocatalytic degradation process. This shows that TCN / ZIF8-40 as a photocatalyst degradation system is more green and environmentally friendly, and has a certain universality in the photodegradation of antibiotics.
[0111] Surface morphology characterization:
[0112] The SEM and XRD characterizations of TCN / ZIF8-40 before and after tetracycline hydrochloride degradation were performed. The SEM image before the degradation reaction is shown in FIG. Fig.14 As shown in (a), the SEM image after degradation reaction is as follows Fig.14 As shown in (b), the XRD pattern before the degradation reaction is as follows Fig.15 As shown in (a), the XRD pattern after degradation reaction is as follows Fig.15 As shown in (b) in .
[0113] from Fig.14 It can be seen that there is not much change in TCN / ZIF8-40 before and after the reaction. Although there is a slight shedding of ZIF8 after the reaction, it can be seen from the photocatalytic degradation cycle experiment diagram that its photocatalytic degradation performance only decreases by 2%, indicating that this slight shedding does not affect its performance, proving that the catalyst has good stability in the photocatalytic degradation of tetracycline hydrochloride system.
[0114] from Fig.15 It can be seen that after the photocatalytic degradation of TCN / ZIF8-40 is completed, its corresponding characteristic peak still exists, proving that its crystal structure has not changed after the reaction, which fully illustrates the stability of TCN / ZIF8-40 material.
[0115] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A tubular carbon nitride @ ZIF8 composite material, characterized in that: The invention comprises tubular graphite phase carbon nitride and a ZIF8 layer grown on the surface of the graphite phase carbon nitride, and the loading amount of the ZIF8 layer on the surface of the graphite phase carbon nitride is 70%-95%.
2. A method for preparing a tubular carbon nitride @ ZIF8 composite material, characterized in that: The following steps are involved: Ultrasonic dispersion of tubular graphite-phase carbon nitride in a zinc salt solution to prepare a precursor mixed solution; The organic ligand solution and the precursor mixed solution are stirred and reacted, and then separated, washed and dried to obtain a tubular carbon nitride@ZIF8 composite material.
3. The preparation method according to claim 2, characterized in that: The solute in the zinc salt solution includes at least one of zinc acetate and zinc nitrate, preferably zinc acetate.
4. The preparation method according to claim 2, characterized in that: The ligand solute in the organic ligand solution includes 2-methylimidazole.
5. The preparation method according to claim 3, characterized in that: After the organic ligand solution and the precursor mixed solution are stirred for reaction, the mass mixing ratio of the solute in the zinc salt solution, the ligand solute and the graphite phase carbon nitride is (3-12):(9-36):1, preferably 5.5:16.5:
1.
6. The preparation method according to claim 2, characterized in that: The process of separating, washing and drying to obtain the tubular carbon nitride @ ZIF8 composite material includes: The reaction solution after stirring the reaction is centrifuged to collect the solids; The solid was washed with an alcohol aqueous solution and dried at 55-65°C to obtain a tubular carbon nitride@ZIF8 composite material.
7. The preparation method according to claim 2, characterized in that: The loading amount of ZIF8 in the tubular carbon nitride@ZIF8 composite material is 70%-95%.
8. The preparation method according to claim 2, characterized in that: The method for preparing the tubular graphite phase carbon nitride comprises the following steps: The melamine solution and the thiocyanamide solution are mixed and stirred to react to obtain a cyanamide reaction solution; After the solid precipitate in the cyanamide reaction solution is separated and dried, it is sintered in a nitrogen atmosphere at 450-550° C. and ground after cooling to obtain tubular graphite phase carbon nitride.
9. A use of the tubular carbon nitride @ ZIF8 composite material as claimed in claim 1, or the tubular carbon nitride @ ZIF8 composite material prepared by the preparation method according to any one of claims 2 to 8 as a photocatalyst in photocatalytic degradation of antibiotics, characterized in that: The antibiotics include tetracycline hydrochloride, norfloxacin and ciprofloxacin.
10. The use according to claim 9, characterized in that: The mixing ratio of the photocatalyst to the antibiotic is 10:1.
Citation Information
Patent Citations
Preparation method of composite visible photocatalyst ZIF-8@S-g-carbon nitride
CN110124736A
Hollow tubular sulfur-doped carbon nitride / graphite-phase carbon nitride homojunction photocatalyst, and preparation method and application thereof
CN111185216A
Preparation method of ZIF-8@g-C3N4 catalyst with zeolite structure
CN112090448A
Fish scale tubular carbon nitride as well as preparation method and application thereof
CN112892611A
Fish scale tubular carbon nitride composite heterojunction photocatalyst as well as preparation method and application thereof
CN112916035A