Titanium and titanium alloy square tube profile forming method
Through stamping forming and heat treatment technology, the problems of bending and twisting defects in the molding of titanium and titanium alloy profiles are solved, the uniformity and mechanical properties of the profiles are improved, and it is suitable for the high wall thickness requirements of aerospace and other industries, achieving low-cost, efficient Production.
Patent Information
- Application Number
- CN202411010068.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-08
AI Technical Summary
Defects such as bending and twisting are prone to occur during the extrusion molding process of existing titanium and titanium alloy profiles. The process is complex and costly, making it difficult to meet the high-quality needs of aerospace and other industries.
Using the stamping forming method, through heat treatment and vacuum annealing, combined with profile straightening and welding technology, high-quality titanium and titanium alloy square tube profiles are prepared, which solves the problems of structural uniformity and mechanical properties.
It improves the structural uniformity and mechanical properties of titanium and titanium alloy square tube profiles, shortens the molding cycle, and reduces production costs. It is suitable for small and medium-sized batch production of various specifications and meets the high wall thickness and low curvature requirements of aerospace and other industries.
Smart Images

Figure CN118744175A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of profile production, and in particular relates to a titanium and titanium alloy square tube profile forming method. Background Art
[0002] Titanium and titanium alloy profiles are a special type of near-net-shape semi-finished product with small machining allowances, high structural benefits, excellent comprehensive performance, and great market potential. They have been widely used in the fields of aviation and aerospace. In the actual research process, due to the wide variety of titanium and titanium alloy profiles, the development cycle of related aircraft can be shortened. At the same time, titanium and titanium alloys are close to the electrodes of many composite materials, which can avoid corrosion when in contact with compliant materials. With the improvement of the application scope of composite materials, the frequency of use of titanium and titanium alloys is also increasing. Titanium and titanium alloy profiles are important aircraft structural materials and are widely used as wings, wall panels, bulkheads, etc.
[0003] At present, titanium and titanium alloy profiles are generally processed by hot rolling and hot extrusion. Since titanium has a close-packed hexagonal crystal structure at room temperature, it has high strength and is difficult to deform, so the extrusion process of titanium and titanium alloy profiles must be carried out under high temperature conditions. When extruding titanium and titanium alloy profiles, the metal flow differences at different parts of the profile cross section are large, which eventually causes the profile to have defects such as bending and twisting. The extrusion process is not only closely related to the performance of the material, but also greatly affected by many process conditions such as extrusion deformation form, temperature, ingot size, lubrication, mold, heating system, extrusion ratio, extrusion speed, profile type, equipment condition, lubrication conditions and mold structure. The influence of various factors on the quality of the product is complex. The distortion or bending of titanium and titanium alloy profiles after extrusion is a problem that cannot be completely avoided, especially in thin-walled asymmetric cross-section titanium and titanium alloy profiles.
[0004] Therefore, it is necessary to propose a low-cost, high-quality titanium and titanium alloy square tube profile forming method to promote the development of aerospace, weapons and other industries. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a titanium and titanium alloy square tube profile forming method in view of the deficiencies in the above-mentioned prior art. The stamping forming method can improve the uniformity of the formed structure of the titanium and titanium alloy square tube profile, improve the product quality of the titanium and titanium alloy square tube profile, shorten the forming cycle, improve the mechanical properties of the profile, solve the limitations on the length and specifications of the titanium and titanium alloy square tube profile, and obtain the required square tube profile.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for forming titanium and titanium alloy square tube profiles, characterized in that the method comprises the following steps:
[0007] Step 1: Making square slabs: According to the target product square tube profile, titanium sheet or titanium alloy sheet is selected and cut to obtain a plurality of square slabs;
[0008] Step 2: hot stamping to produce U-shaped profiles: firstly, a profile heating device is used to heat treat the plurality of square blanks, and then a profile stamping device is used to set a pressing speed and a pressing force to hot stamp the plurality of heat-treated square blanks to obtain a plurality of U-shaped profiles;
[0009] Step 3: performing vacuum annealing on the plurality of U-shaped profiles;
[0010] Step 4: Thermal alignment of U-shaped profiles: Use profile straightening equipment to perform thermal alignment on multiple U-shaped profiles after vacuum annealing;
[0011] Step 5: Surface treatment is performed on the multiple U-shaped profiles after heat calibration;
[0012] Step 6, making square tube profile segments: milling the edges of the plurality of U-shaped profiles after surface treatment and processing the grooves; buckling the plurality of U-shaped profiles in pairs, so that the milling edges of the two buckled U-shaped profiles, i.e., the groove positions, form a joint seam, and welding the joint seam to form a longitudinal weld seam, thereby obtaining a plurality of square tube profile segments;
[0013] Step 7: Conduct weld inspection on multiple square tube profile sections;
[0014] Step 8: Perform heat calibration on the square tube profile section;
[0015] Step 9, making square tube profiles: according to the designed length of the square tube profiles, a set number of square tube profile segments are welded and connected in sequence to obtain the square tube profiles, and the welding seam between two adjacent square tube profile segments is a girth weld;
[0016] Wherein, the longitudinal welds of two adjacent square tube profile sections are located on two perpendicular planes;
[0017] Step 10, performing weld inspection on the square tube profile;
[0018] Step 11: vacuum annealing and surface treatment are performed on the square tube profile in sequence.
[0019] The above-mentioned titanium and titanium alloy square tube profile forming method is characterized in that: in step 2, before heat treating the square slab, an anti-oxidation coating is coated on the surface of the square slab.
[0020] The above-mentioned titanium and titanium alloy square tube profile forming method is characterized in that: in step 2, the profile heating equipment is a heating furnace, and when the multiple square slabs are heat treated, the heat treatment temperature is lower than the phase change point of the square slabs by 80°C to 120°C, and at the heat treatment temperature, the square slabs are heated in the heating furnace for 2h to 3h.
[0021] The above-mentioned titanium and titanium alloy square tube profile forming method is characterized in that: in step three, the profile stamping equipment includes an upper workbench and a lower workbench capable of relative movement, and the lower workbench is provided with a U-shaped lower die, and the inner die surface of the U-shaped lower die includes, from top to bottom, the lower die boss end face, the lower die end face, the lower die groove side face and the lower die groove bottom face, and a lower die end face R angle is provided between the lower die end face and the lower die groove side face, and a lower die groove R angle is provided between the lower die groove side face and the lower die groove bottom face, and an impact upper die capable of cooperating with the U-shaped lower die to form a forming cavity is provided on the upper workbench, and the bottom of the impact upper die has an upper die R angle.
[0022] The above-mentioned method for forming titanium and titanium alloy square tube profiles is characterized in that: the R angle surface of the lower die end face is smooth, the R angle of the upper die is the same as the inner R angle of the square tube profile, and the R angle of the lower die groove is the same as the outer R angle of the square tube profile.
[0023] The above-mentioned titanium and titanium alloy square tube profile forming method is characterized in that: when using profile stamping equipment to hot stamp a plurality of square slabs after heat treatment, the square slabs are placed on the lower die end face of the U-shaped lower die, and the profile stamping equipment is started, so that the upper workbench drives the impact upper die to hot stamp the square slabs until the bottom of the square slab is stamped to the bottom surface of the lower die groove to obtain a U-shaped profile.
[0024] The above-mentioned titanium and titanium alloy square tube profile forming method is characterized in that: in step three and step eleven, the vacuum annealing temperature is 500°C to 800°C, and the vacuum annealing holding time is 1h to 2h.
[0025] The above-mentioned titanium and titanium alloy square tube profile forming method is characterized in that: in step 4 and step 8, before the profile is heat-corrected, the profile is first heat-treated according to the method in step 2;
[0026] One end of the profile is clamped and fixed by the fixed end clamping assembly of the profile straightening equipment, and the other end of the profile is clamped by the moving slide, power propulsion assembly and moving end transverse clamping mechanism of the profile straightening equipment. When the moving slide slides, the other end of the profile is driven to move for straightening.
[0027] The above-mentioned titanium and titanium alloy square tube profile forming method is characterized in that: in step five and step eleven, when the profile is subjected to surface treatment, the surface of the profile is shot peened, degreased, washed with water and dried in sequence.
[0028] The above-mentioned method for forming titanium and titanium alloy square tube profiles is characterized in that: in step nine, after a set number of square tube profile segments are welded and lengthened in sequence, the curvature of the obtained square tube profile is k≤1.5×L÷1000, wherein L is the length of the square tube profile.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] 1. The present invention breaks the traditional method of extrusion molding of titanium and titanium alloy profiles and proposes a new preparation method. The above method can improve the uniformity of the organizational structure of the titanium and titanium alloy square tube profiles, improve the product quality of the titanium and titanium alloy square tube profiles, shorten the molding cycle, and improve the mechanical properties of the profiles.
[0031] 2. The present invention adopts a stamping forming method, which can be produced continuously with a simple process. The preparation method has a high utilization rate of raw materials, can greatly save energy, reduce processing costs, and improve production efficiency.
[0032] 3. The present invention forms a U-shaped profile by stamping first, and then assembles and welds it to form a square tube profile, so that a square tube profile with a wall thickness greater than 2 mm can be obtained, and the mechanical properties and chemical composition of the square tube profile can meet the requirements of relevant standards, effectively solving the problems of high weight requirements, thin wall thickness and great forming difficulty in the aerospace, weapons and other industries.
[0033] 4. The present invention adopts a stamping forming method, which effectively improves the quality and yield rate of square tube profiles, and greatly reduces the production cost of the entire equipment during the manufacturing process of the entire product, thereby significantly improving the economic benefits.
[0034] 5. The process of the present invention is simple, easy to operate, has low investment cost, and has a wide range of applications. It is particularly suitable for making small and medium batches of square tube profiles of various specifications, and has broad prospects for promotion and application.
[0035] In summary, the stamping forming method used in the present invention can improve the uniformity of the formed structure of the titanium and titanium alloy square tube profiles, improve the product quality of the titanium and titanium alloy square tube profiles, shorten the forming cycle, improve the mechanical properties of the profiles, solve the limitations on the length and specifications of the titanium and titanium alloy square tube profiles, and obtain the required square tube profiles.
[0036] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a flowchart of the present invention.
[0038] Figure 2 It is a schematic structural diagram of the profile stamping equipment of the present invention.
[0039] Figure 3 It is a structural schematic diagram of the U-shaped lower mold of the present invention.
[0040] Figure 4 It is a schematic diagram of the positional relationship among the square slab, the U-shaped lower die and the impact upper die during hot stamping of the present invention.
[0041] Figure 5 It is a schematic diagram of the positional relationship between the U-shaped profile, the U-shaped lower die and the impact upper die after hot stamping of the present invention.
[0042] Figure 6 The figure is a schematic diagram of the structure of the U-shaped profile after edge milling and groove processing according to the present invention.
[0043] Figure 7 It is a structural schematic diagram of the profile straightening device of the present invention.
[0044] Figure 8 It is a schematic structural diagram of the square tube profile segment of the present invention.
[0045] Description of reference numerals:
[0046] 1—square slab; 2—U-shaped profile; 3—profile stamping equipment; 3-1—upper workbench; 3-2—lower workbench; 4—U-shaped lower die; 4-1—lower die boss end face; 4-2—lower die end face; 4-3—lower die end face R angle; 4-4—lower die groove side face; 4-5—lower die groove R angle; 4-6—lower die groove bottom face; 5—impact upper die; 5-1—upper die R angle; 6—square tube profile section; 7—inner R angle; 8—outer R angle; 9—profile straightening equipment; 9-1—movable slide; 9-2—power propulsion assembly; 9-3—movable end lateral clamping assembly; 9-4—fixed end clamping assembly; 10—U-profile milling edge plane; 11—U-profile milling edge groove. DETAILED DESCRIPTION
[0047] like Figures 1 to 7 A method for forming a titanium and titanium alloy square tube profile is shown, the method comprising the following steps:
[0048] Step 1: Making square slabs: According to the target product square tube profile, titanium sheet or titanium alloy sheet is selected and cut to obtain a plurality of square slabs 1;
[0049] Step 2: hot stamping to produce U-shaped profiles: firstly, a profile heating device is used to heat treat the plurality of square slabs 1, and then a profile stamping device 3 is used to set a pressing speed and a pressing force to hot stamp the plurality of heat-treated square slabs 1 to obtain a plurality of U-shaped profiles 2;
[0050] Step 3: vacuum annealing the plurality of U-shaped profiles 2;
[0051] Step 4: Thermal alignment of U-shaped profiles: Use profile alignment equipment 9 to perform thermal alignment on a plurality of U-shaped profiles 2 after vacuum annealing;
[0052] Step 5: Surface treatment is performed on the plurality of U-shaped profiles 2 after thermal calibration;
[0053] Step 6, making square tube profile segments: milling the multiple U-shaped profiles 2 after surface treatment, and processing the grooves, so that the open end of the U-shaped profile 2 has a U-shaped profile milling plane 10 and a U-shaped profile milling groove 11; buckle the multiple U-shaped profiles 2 in pairs, and weld the longitudinal welds to obtain multiple square tube profile segments 6;
[0054] Step 7: Conduct weld inspection on multiple square tube profile segments 6;
[0055] Step 8, heat-correcting the square tube profile section 6;
[0056] Step 9, making a square tube profile: according to the designed length of the square tube profile, a set number of square tube profile segments 6 are welded and lengthened in sequence to obtain a square tube profile, and the welding seam between two adjacent square tube profile segments is a girth weld;
[0057] The longitudinal welds of two adjacent square tube profile segments 6 are located on two perpendicular planes, that is, when the longitudinal weld of one square tube profile segment 6 is located at the front and rear sides of the square tube profile, the longitudinal weld of the other adjacent square tube profile segment 6 is located at the upper and lower sides of the square tube profile;
[0058] Step 10, performing weld inspection on the square tube profile;
[0059] Step 11: vacuum annealing and surface treatment are performed on the square tube profile in sequence.
[0060] In actual use, when cutting the sheet material, a water jet cutting method is adopted to obtain a square sheet blank 1 .
[0061] It should be noted that by using profile stamping equipment 3 to hot stamp multiple square plate blanks 1 after heat treatment to obtain multiple U-shaped profiles 2, the uniformity of the formed structure of the titanium and titanium alloy profiles can be effectively improved. The operation is simple, there are no welds, the dimensional accuracy is high, and the appearance quality of the titanium and titanium alloy profiles is improved. At the same time, defects such as cracks are eliminated, the forming accuracy is improved, the product quality of titanium and titanium alloy profiles is improved, the forming cycle is shortened, and the mechanical properties of the profiles are improved.
[0062] In addition, the stamping method can be used for continuous production with a simple process. The preparation method has a high utilization rate of raw materials and can also significantly save energy, reduce processing costs, and improve production efficiency.
[0063] It should be noted that the stamping forming method can effectively improve the quality and yield rate of square tube profiles, and greatly reduce the production cost of the entire equipment during the manufacturing process of the whole product, significantly improving the economic benefits; it is easy to obtain square tube profiles with a wall thickness greater than 2mm, and the mechanical properties and chemical composition of the square tube profiles can meet the relevant standard requirements, effectively solving the problems of high weight requirements, thin wall thickness and great forming difficulty in the aerospace, weapons and other industries.
[0064] In particular, during hot stamping, by controlling the hot stamping temperature and pressure and applying high-temperature resistant and anti-oxidation coatings, the pressure is effectively reduced, excessive thinning of the square tube profile is avoided, and the uniformity of deformation is improved, which is conducive to the smooth forming of the square tube profile.
[0065] During specific implementation, a set number of square tube profile segments 6 are welded and lengthened in sequence to obtain a square tube profile, and the welding seam between two adjacent square tube profile segments is a circumferential weld; when the splicing surfaces of the two U-shaped profiles 2 of a square tube profile segment 6 are horizontally arranged, the splicing surfaces of the two U-shaped profiles 2 of the other adjacent square tube profile segments 6 are vertically arranged, and vice versa.
[0066] During specific implementation, in step 2, the pressing speed is preferably set to 30 mm / s, and the pressing force is set to the equipment power, preferably 10 MPa.
[0067] In the specific implementation, in step seven and step ten, when the profile weld is inspected, PT penetration testing is used, referring to the NB / T 47014 standard. When the profile weld quality does not meet the requirements, the profile welding position can be re-welded and repaired until it is qualified.
[0068] In this embodiment, in step 2, before heat treating the square slab 1 , a high temperature resistant and anti-oxidation coating is coated on the surface of the square slab 1 .
[0069] In actual use, before coating the surface of the square slab 1 with the high temperature resistant anti-oxidation coating, firstly clean the oil stains and debris on the surface of the square slab 1, and the thickness of the high temperature resistant anti-oxidation coating is 0.2mm-1.0mm.
[0070] It should be noted that by coating the surface of the square slab 1 with a high temperature resistant and anti-oxidation coating, oxidation during hot stamping is effectively prevented, the problem of scratches or tears on the outer surface of the square slab 1 during stamping is solved, and the quality of the square tube profile is improved.
[0071] In this embodiment, in step 2, the profile heating equipment is a heating furnace. When the plurality of square slabs 1 are heat treated, the heat treatment temperature is 80°C to 120°C lower than the phase change point temperature of the sheet material used for the square slabs 1, and at this heat treatment temperature, the square slabs 1 are heated in the heating furnace for 2h to 3h.
[0072] In this embodiment, in step three, the profile stamping equipment 3 includes an upper workbench 3-1 and a lower workbench 3-2 capable of relative movement, a U-shaped lower die 4 is arranged on the lower workbench 3-2, and the inner die surface of the U-shaped lower die 4 includes, from top to bottom, a lower die boss end face 4-1, a lower die end face 4-2, a lower die groove side face 4-4 and a lower die groove bottom face 4-6, a lower die end face R angle 4-3 is arranged between the lower die end face 4-2 and the lower die groove side face 4-4, a lower die groove R angle 4-5 is arranged between the lower die groove side face 4-4 and the lower die groove bottom face 4-6, an impact upper die 5 capable of cooperating with the U-shaped lower die 4 to form a molding cavity is arranged on the upper workbench 3-1, and the bottom of the impact upper die 5 has an upper die R angle 5-1.
[0073] In this embodiment, the lower die end face R angle 4-3 is smooth, the upper die R angle 5-1 is the same size as the inner R angle 7 of the square tube profile, and the lower die groove R angle 4-5 is the same size as the outer R angle 8 of the square tube profile.
[0074] In this embodiment, when the profile stamping equipment 3 is used to hot stamp a plurality of square slabs 1 after heat treatment, the square slabs 1 are placed on the lower die end face 4-2 of the U-shaped lower die 4, and the profile stamping equipment 3 is started, so that the upper workbench 3-1 drives the impact upper die 5 to hot stamp the square slabs 1 until the bottom of the square slab 1 is stamped to the bottom surface 4-6 of the lower die groove, thereby obtaining a U-shaped profile 2.
[0075] In this embodiment, in step 3 and step 11, the temperature of vacuum annealing is 500° C. to 800° C., and the holding time of vacuum annealing is 1 h to 2 h.
[0076] In actual use, the temperature of vacuum annealing is preferably 500° C., and the holding time of vacuum annealing is preferably 2 h.
[0077] In this embodiment, in step 4 and step 8, before the profile is heat-calibrated, the profile is first heat-treated according to the method in step 2;
[0078] One end of the profile is clamped and fixed by the fixed end clamping assembly 9-4 of the profile straightening equipment 9, and the other end of the profile is clamped by the movable slide 9-1, the power propulsion assembly 9-2 and the movable end transverse clamping mechanism 9-3 of the profile straightening equipment 9. When the movable slide 9-1 slides, it drives the other end of the profile to move for straightening.
[0079] In actual use, after the U-shaped profile 2 is heat-treated, it is quickly hoisted to the profile straightening device 9 for heat correction.
[0080] During specific implementation, a heating device is further provided between the fixed end clamping assembly 9 - 4 and the movable slide 9 - 1 , and the middle portion of the profile is passed through the heating device, thereby enabling thermal calibration.
[0081] It should be noted that when straightening is performed, the power propulsion assembly 9-2 is pressed downward so that it cooperates with the movable slide 9-1 to clamp the profile vertically, and the mobile end transverse clamping mechanism 9-3 clamps the profile laterally, so that the movable slide 9-1, the power propulsion assembly 9-2 and the mobile end transverse clamping mechanism 9-3 can slide synchronously, driving the other end of the profile to move, causing the profile to stretch, thereby straightening.
[0082] In specific implementation, before straightening the U-shaped profile 2, when clamping the two ends of the U-shaped profile 2, a support block matching its shape is inserted at both ends of the U-shaped profile 2 to prevent the two ends of the U-shaped profile 2 from deforming during clamping.
[0083] In this embodiment, in step five and step eleven, when the profile is subjected to surface treatment, the surface of the profile is sequentially subjected to shot blasting, degreasing, water washing and drying.
[0084] In this embodiment, in step nine, after a set number of square tube profile segments 6 are welded and lengthened in sequence, the curvature of the obtained square tube profile is k≤1.5×L÷1000, wherein L is the length of the square tube profile.
[0085] In specific implementation, the size specifications of the square tube profile thickness × cross-sectional length × cross-sectional width are generally 3×60×60mm, 4×80×80mm or 5×100×100mm; the widths of the square slabs 1 corresponding to the three sizes are 120mm, 160mm and 200mm respectively.
[0086] When the size of the square tube profile is 3×60×60mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 500°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly hoisted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 3 and step 11 is preferably 500°C, and the insulation time of the vacuum annealing is preferably 2h; in step 4, before the U-shaped profile 2 is heat-corrected, the U-shaped profile 2 is placed in a heating furnace and heated at 500°C for 2h for heat treatment;
[0087] When the size of the square tube profile is 4×80×80mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 700°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly lifted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 3 is preferably 700°C, and the holding time of the vacuum annealing is preferably 2h; in step 4, before the U-shaped profile 2 is heat-corrected, the U-shaped profile 2 is placed in a heating furnace and heated at 550°C for 2h for heat treatment. The temperature of the vacuum annealing in step 11 is preferably 500°C, and the holding time of the vacuum annealing is preferably 2h;
[0088] When the size of the square tube profile is 5×100×100mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 800°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly lifted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 3 is preferably 600°C, and the holding time of the vacuum annealing is preferably 2h; in step 4, before the U-shaped profile 2 is hot-calibrated, the U-shaped profile 2 is placed in a heating furnace and heated at 800°C for 2h for heat treatment. The temperature of the vacuum annealing in step 11 is preferably 500°C, and the holding time of the vacuum annealing is preferably 2h.
[0089] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for forming titanium and titanium alloy square tube profiles, characterized in that: The method comprises the following steps: Step 1: Making square slabs: According to the target product square tube profile, titanium sheet or titanium alloy sheet is selected and cut to obtain a plurality of square slabs (1); Step 2: hot stamping to produce U-shaped profiles: firstly, a profile heating device is used to heat treat the plurality of square blanks (1), and then a profile stamping device (3) is used to hot stamp the plurality of square blanks (1) after the heat treatment at a set pressing speed and a set pressing force to obtain a plurality of U-shaped profiles (2); Step 3: performing vacuum annealing on the plurality of U-shaped profiles (2); Step 4: Thermal alignment of the U-shaped profile: using a profile alignment device (9) to perform thermal alignment on the plurality of U-shaped profiles (2) after vacuum annealing; Step 5: performing surface treatment on the plurality of U-shaped profiles (2) after thermal calibration; Step 6, making square tube profile segments: milling the edges of the plurality of U-shaped profiles (2) after surface treatment and processing the grooves; interlocking the plurality of U-shaped profiles (2) in pairs, so that the milled edges, i.e. the grooves, of the two interlocking U-shaped profiles (2) form a joint seam, and welding the joint seam to form a longitudinal weld seam, thereby obtaining a plurality of square tube profile segments (6); Step 7, performing weld inspection on a plurality of square tube profile sections (6); Step 8, performing heat calibration on the square tube profile section (6); Step nine, making a square tube profile: according to the designed length of the square tube profile, a set number of square tube profile segments (6) are welded and connected in sequence to obtain a square tube profile, and the welding seam between two adjacent square tube profile segments (6) is a girth weld; The longitudinal welds of two adjacent square tube profile sections (6) are located on two perpendicular planes; Step 10, performing weld inspection on the square tube profile; Step 11: vacuum annealing and surface treatment are performed on the square tube profile in sequence.
2. A titanium and titanium alloy square tube profile forming method according to claim 1, characterized in that: In step 2, before heat treating the square slab (1), an anti-oxidation coating is applied to the surface of the square slab (1).
3. A titanium and titanium alloy square tube profile forming method according to claim 1, characterized in that: In step 2, the profile heating equipment is a heating furnace. When the plurality of square slabs (1) are heat treated, the heat treatment temperature is 80°C to 120°C lower than the phase change point of the square slabs (1), and at the heat treatment temperature, the square slabs (1) are heated in the heating furnace for 2h to 3h.
4. A titanium and titanium alloy square tube profile forming method according to claim 1, characterized in that: In step three, the profile stamping equipment (3) includes an upper workbench (3-1) and a lower workbench (3-2) capable of relative movement, and a U-shaped lower die (4) is arranged on the lower workbench (3-2). The inner die surface of the U-shaped lower die (4) includes, from top to bottom, a lower die boss end face (4-1), a lower die end face (4-2), a lower die groove side face (4-4) and a lower die groove bottom face (4-6), a lower die end face R angle (4-3) is arranged between the lower die end face (4-2) and the lower die groove side face (4-4), a lower die groove R angle (4-5) is arranged between the lower die groove side face (4-4) and the lower die groove bottom face (4-6), and an impact upper die (5) capable of cooperating with the U-shaped lower die (4) to form a molding cavity is arranged on the upper workbench (3-1), and the bottom of the impact upper die (5) has an upper die R angle (5-1).
5. A titanium and titanium alloy square tube profile forming method according to claim 4, characterized in that: The lower die end face R angle (4-3) has a smooth surface, the upper die R angle (5-1) has the same size as the inner R angle (7) of the square tube profile, and the lower die groove R angle (4-5) has the same size as the outer R angle (8) of the square tube profile.
6. A titanium and titanium alloy square tube profile forming method according to claim 4, characterized in that: When a plurality of heat-treated square slabs (1) are hot-stamped using a profile stamping device (3), the square slabs (1) are placed on the lower die end surface (4-2) of a U-shaped lower die (4), and the profile stamping device (3) is started, so that the upper workbench (3-1) drives the impact upper die (5) to hot-stamp the square slabs (1) until the bottom of the square slab (1) is stamped to the bottom surface (4-6) of the lower die groove, thereby obtaining a U-shaped profile (2).
7. A titanium and titanium alloy square tube profile forming method according to claim 1, characterized in that: In step 3 and step 11, the temperature of vacuum annealing is 500° C. to 800° C., and the holding time of vacuum annealing is 1 h to 2 h.
8. A titanium and titanium alloy square tube profile forming method according to claim 1, characterized in that: In step 4 and step 8, before heat-calibrating the profile, the profile is first heat-treated according to the method in step 2; One end of the profile is clamped and fixed by a fixed end clamping assembly (9-4) of the profile straightening device (9), and the other end of the profile is clamped by a movable slide (9-1), a power propulsion assembly (9-2) and a movable end transverse clamping mechanism (9-3) of the profile straightening device (9). When the movable slide (9-1) slides, the other end of the profile is driven to move for straightening.
9. A titanium and titanium alloy square tube profile forming method according to claim 1, characterized in that: In step 5 and step 11, when the profile is subjected to surface treatment, the surface of the profile is sequentially subjected to shot blasting, degreasing, water washing and drying.
10. A titanium and titanium alloy square tube profile forming method according to claim 1, characterized in that: In step nine, after a set number of square tube profile segments (6) are welded and lengthened in sequence, the curvature of the obtained square tube profile is k≤1.5×L÷1000, wherein L is the length of the square tube profile.
Citation Information
Patent Citations
Methods for the production of clad steel products
CN103476519A
Production method and detection method of titanium alloy seamless tube
CN103722043A
Manufacturing method for zirconium alloy element box
CN106623487A
Rotary intelligent automatic welding workstation for five large pieces of passenger car body framework
CN112045287A
Rectangular pipe manufacturing die
CN211464429U
Cited By
Titanium alloy laser-induced bending device and method
CN118950737A