Die-casting aluminum alloy material and its preparation method and application
Through the design of high copper and high magnesium aluminum alloy ratio and reasonable element ratio, combined with composite deterioration technology, die-cast aluminum alloy materials without heat treatment were prepared, which solved the yield strength of existing aluminum alloy materials in the motor housing of new energy vehicles and The problem of insufficient corrosion resistance has achieved the improvement of high strength and corrosion resistance, simplified the process and reduced costs.
Patent Information
- Application Number
- CN202211413943.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-11-11
AI Technical Summary
The existing aluminum alloy materials cannot meet the high yield strength and corrosion resistance requirements of new energy vehicle motor housing under high stress and high corrosion environments, and the heat treatment process is complex and costly.
Using high copper and high magnesium aluminum alloy ratio, by controlling the Cu/Mg ratio and reasonable alloy element ratio, combined with the composite deterioration/refining process, die-cast aluminum alloy materials without heat treatment are prepared to improve their yield strength and corrosion resistance. performance.
It realizes high yield strength and corrosion resistance without heat treatment, simplifies the casting process, reduces energy consumption, and meets the high strength and high toughness requirements of the motor housing of new energy vehicles.
Smart Images

Figure BDA0003939375370000101
Abstract
Description
Technical Field
[0001] The present application relates to a die-cast aluminum alloy material and a preparation method and application thereof. Specifically, the present application relates to a die-cast aluminum alloy material that is self-strengthening without heat treatment and has high yield strength and corrosion resistance and a preparation method thereof. Background Art
[0002] Aluminum alloys are widely used in die-cast motor housings due to their low density, good thermal conductivity and fluidity. For high-power motors, the housing is subjected to large tensile stress, with stress in some local locations even exceeding 200MPa. At the same time, the elongation requirement is ≥4%. Considering the outdoor or field working scenes of the motor housing, die-cast aluminum alloy materials are required to meet the characteristics of high strength, high toughness and corrosion resistance.
[0003] At present, conventional aluminum alloy materials represented by A380 and ADC12 are the most widely used. However, due to the high content of impurity elements such as Fe in these aluminum alloys, the standard test bar performance of this material can only reach a yield strength of 160MPa, a tensile strength of 320MPa, and an elongation of 3.5%, which cannot meet the use requirements of castings with high strength requirements such as new energy vehicle motor housings. High-performance aluminum alloy materials such as AlSi10MnMg and AlMg5Si2 can obtain excellent mechanical properties by controlling the alloy element content and heat treatment process. However, this type of alloy requires high-purity new materials to prepare, which is costly, and for large and complex die-cast housings, if heat treated, the quenching process causes local deformation in the uneven wall thickness of the workpiece, requiring a finishing process, which is both time-consuming and labor-intensive.
[0004] At present, many companies and research institutions have disclosed Al-Si-Cu-Mg series heat-treatment-free die-cast aluminum alloys, but their strength cannot yet meet the requirements of components such as new energy vehicle motor housings. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present application provides a die-cast aluminum alloy material and a preparation method and application thereof. The die-cast aluminum alloy material of the present application can obtain high mechanical properties, especially high yield strength, without heat treatment, and has high corrosion resistance, which can well meet the requirements of high yield strength, high toughness and corrosion resistance of parts such as motor housings of new energy vehicles.
[0006] The first aspect of the present application provides a die-casting aluminum alloy material, which includes, by weight: 8.0%-11.0% silicon (Si) element, 0.5% or less iron (Fe) element, 1.0%-3.0% copper (Cu) element, 0.5%-2.5% magnesium (Mg) element, 0.5%-1.2% manganese (Mn) element, 1.3% or less zinc (Zn) element, 0.08%-0.15% titanium (Ti) element, 0.1%-0.2% zirconium (Zr) element, 0.02%-0.04% strontium (Sr) element and less than 1.0% impurities, wherein the mass ratio of the copper element to the magnesium element is (0.5-2.0):1.
[0007] A second aspect of the present application provides a method for preparing a die-cast aluminum alloy material, which comprises the following steps:
[0008] S1: mixing a silicon raw material, a manganese raw material, a copper raw material and an aluminum raw material and performing a first heating treatment to obtain a first melt;
[0009] S2: mixing the first melt with a slag remover at a first temperature to remove slag, and then adding a titanium raw material, a zirconium raw material, a strontium raw material, a magnesium raw material and an optional zinc raw material to obtain an aluminum alloy material melt;
[0010] S3: die-casting the aluminum alloy material melt to obtain the die-cast aluminum alloy material.
[0011] A third aspect of the present application provides a motor housing, which is made of the die-cast aluminum alloy material described in the first aspect or the die-cast aluminum alloy material prepared by the preparation method described in the second aspect.
[0012] The fourth aspect of the present application provides the use of the die-cast aluminum alloy material described in the first aspect or the die-cast aluminum alloy material prepared by the preparation method described in the second aspect in a vehicle.
[0013] The beneficial effects of this application are:
[0014] (1) The die-cast aluminum alloy material of the present application adopts a material ratio of high copper and high magnesium and controls the Cu / Mg ratio within a reasonable range, thereby ensuring that the toughness is not adversely affected while the strength is improved to the greatest extent. In addition, the present application also uses a composite modification / refinement process to ensure that the grain size in the alloy is small and uniform while the eutectic silicon modification effect is good.
[0015] (2) The test rod of the die-cast aluminum alloy material of the present application has high room temperature mechanical properties, among which the tensile strength is ≥360Mpa, the yield strength is ≥230Mpa, the elongation is ≥3.0%, and the hardness is above 115HBS. In addition, the performance can be further improved through natural aging, which can meet the requirements of high yield strength, high toughness and corrosion resistance of parts such as motor housings of new energy vehicles.
[0016] (3) The present application can enable the aluminum alloy to obtain higher mechanical properties without heat treatment, simplifying the die-casting process and reducing energy consumption. DETAILED DESCRIPTION
[0017] For simplicity, this application only specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an undefined range.
[0018] In the description of the present application, unless otherwise specified, “above” and “below” include the number.
[0019] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0020] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0021] The present application is further described below in conjunction with specific implementations. It should be understood that these specific implementations are only used to illustrate the present application and are not used to limit the scope of the present application.
[0022] In the first aspect, the die-casting aluminum alloy material provided by the present application includes, by weight: 8.0%-11.0% silicon, 0.5% or less iron, 1.0%-3.0% copper, 0.5%-2.5% magnesium, 0.5%-1.2% manganese, 1.3% or less zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium and 1.0% or less impurities, wherein the mass ratio of the copper element to the magnesium element is (0.5-2.0):1. The Cu element can generate θ (CuAl) with aluminum. 2 ), is an important strengthening element in aluminum alloys. Usually in the presence of magnesium, when the Cu / Mg ratio is around 2.6, it will combine to form S (CuMgAl) with better solid solution strengthening effect. 2 ) strengthening phase. However, when the Cu content is too high, the elongation and corrosion resistance of the aluminum alloy material will be affected to a certain extent. In Si-containing aluminum alloys, magnesium is an important aging strengthening element and will form Mg 2 Si strengthening phase, since the die-cast aluminum alloy material of this application is mainly used for shell materials, it has high mechanical requirements and requires no heat treatment, so the proportion of aging strengthening elements in the alloy must be appropriately increased to improve the strength of the alloy by natural aging. 5 Al 8 , whose potential is close to that of α-Al, can improve the corrosion performance of aluminum alloy. Based on this, the inventors of this application have found through research that by adding copper and magnesium elements to the die-cast aluminum alloy material and controlling the mass ratio of copper to magnesium elements within the above range, it is possible to maximize the improvement of the strength of the alloy material, especially the yield strength, while ensuring that the toughness is not affected. At the same time, it also has high corrosion resistance, which can well meet the requirements of high yield strength, high toughness and corrosion resistance of parts such as motor housings of new energy vehicles.
[0023] In some embodiments, the mass ratio of copper to magnesium is 0.6:1, 0.65:1, 0.75:1, 0.85:1, 0.9:1, 0.95:1, 1.0:1, 1.05:1, 1.1:1, 1.15:1, 1.2:1, 1.25:1, 1.3:1, 1.35:1, 1.4:1, 1.45:1, 1.55:1, 1.6:1, 1.65:1, 1.7:1, 1.75:1, 1.8:1, 1.9:1 or any value therebetween. In some embodiments, the mass ratio of copper to magnesium is (0.7-1.85):1. In some embodiments, the mass ratio of copper to magnesium is (0.8-1.5):1.
[0024] In some embodiments, the die-casting aluminum alloy material consists of, by weight, 8.0%-11.0% silicon, less than 0.5% iron, 1.0%-3.0% copper, 0.5%-2.5% magnesium, 0.5%-1.2% manganese, less than 1.3% zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, less than 1.0% impurities and the remainder aluminum.
[0025] In the present application, the impurities in the die-casting aluminum alloy material are mainly the inevitable impurities introduced during the synthesis process of the die-casting aluminum alloy material. In some embodiments, the impurities mainly include at least one of Cr, Ni, Be, Bi, Ca, Na, Sn or V. In some embodiments, by weight, the mass content of the impurities is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or any value therebetween. In some embodiments, by weight, the mass content of a single impurity is below 0.15%, for example, below 0.1%, or below 0.05%.
[0026] In some embodiments, the mass content of silicon is 8.1%, 8.2%, 8.3%, 8.4%, 8.5%, 8.6%, 8.7%, 8.8%, 8.9%, 9.0%, 9.1%, 9.2%, 9.3%, 9.4%, 9.6%, 9.7%, 9.8%, 9.9%, 10%, 10.1%, 10.2%, 10.3%, 10.4%, 10.6%, 10.7%, 10.8%, 10.9% or any value therebetween, by weight. The Si element is mainly an element that improves the fluidity of the aluminum alloy melt. Generally, the fluidity is better within the range of Al-Si eutectic and hypoeutectic. At the same time, the element releases latent heat of crystallization during crystallization, which is more conducive to filling. However, too high a silicon content will affect the elongation of the casting. The present application controls the silicon element within the above range to ensure the fluidity of the aluminum alloy while avoiding the influence of excessive Si content on the elongation of the casting. In some embodiments, the mass content of the silicon element is 8.0%-10.5%. In some embodiments, the mass content of the silicon element is 8.0%-9.5%.
[0027] In some embodiments, the mass content of copper is 1.1%, 1.2%, 1.3%, 1.4%, 1.45%, 1.5%, 1.55%, 1.6%, 1.65%, 1.7%, 1.75%, 1.8%, 1.85%, 1.9%, 1.95%, 2.0%, 2.05%, 2.1%, 2.15%, 2.2%, 2.3%, 2.4%, 2.6%, 2.7%, 2.8%, 2.9% or any value therebetween. In some embodiments, the mass content of copper is 1.3%-2.5%. In some embodiments, the mass content of copper is 1.4%-2.2%.
[0028] In some embodiments, the mass content of magnesium is 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.15%, 1.2%, 1.25%, 1.3%, 1.35%, 1.4%, 1.45%, 1.5%, 1.55%, 1.6%, 1.65%, 1.7%, 1.75%, 1.8%, 1.85%, 1.9%, 1.95%, 2.0%, 2.05%, 2.1%, 2.2%, 2.3%, 2.4% or any value therebetween. In some embodiments, the mass content of magnesium is 1.0%-2.0%. In some embodiments, the mass content of copper is 1.2%-1.8%.
[0029] In some embodiments, the mass content of iron is 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.2% or any value therebetween by weight. Iron has a certain demoulding effect on the alloy, but the iron content should not be too much, otherwise the mechanical properties of the material will deteriorate. In some embodiments, the mass content of iron is less than 0.15% by weight.
[0030] In some embodiments, the mass content of manganese is 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1.0%, 1.05%, 1.1% or any value therebetween, by weight. The main method of shell molding is high pressure casting. Demolding is an important technical issue in the die casting process. Iron is conducive to die casting demolding. However, the needle-shaped FeAl2O3 formed in the aluminum alloy is hard and brittle. 3 Infusible phase seriously deteriorates the material properties, especially the elongation, and uses manganese to generate (FeMn)Al 6Phase, can reduce the harmful effect of iron, and also facilitate demoulding. In addition, appropriate addition is also beneficial to improve corrosion resistance. In some embodiments, the mass content of manganese element is 0.5%-1.0%. In some embodiments, the mass content of manganese element is 0.5%-0.8%.
[0031] In some embodiments, by weight, the mass content of zinc is 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1.0%, 1.1%, 1.2% or any value therebetween. Zinc has a certain supplementary strengthening effect on the alloy, but it is not advisable to add too much, otherwise it will affect the corrosion resistance. In some embodiments, by weight, the mass content of zinc is less than 1.0%. In some embodiments, by weight, the mass content of zinc is less than 0.8%.
[0032] In some embodiments, the mass content of titanium is 0.085%, 0.09%, 0.095%, 0.1%, 0.105%, 0.11%, 0.115%, 0.12%, 0.125%, 0.13%, 0.135%, 0.14%, 0.145% or any value therebetween, by weight. Titanium plays a major role as an external nucleus in aluminum alloys, refining aluminum alloy grains, but if the content is too high, grain coarsening will occur.
[0033] In some embodiments, the mass content of zirconium is 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19% or any value therebetween. Adding zirconium to aluminum alloy can refine the grains and strengthen the thermal stability of the material; these characteristics can prevent the performance loss of the structural parts due to the increase in temperature. However, the zirconium content should not be too high, as it will reduce the Al 3 The pinning effect of Zr particles in the aluminum matrix and the grain refinement effect cause a certain decrease in material properties.
[0034] In some embodiments, the mass content of strontium is 0.021%, 0.022%, 0.023%, 0.024%, 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.03%, 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039% or any value therebetween, by weight. Strontium, as a modifier of aluminum-silicon alloy, makes eutectic silicon round, inhibits the growth of primary silicon, and is beneficial to improving the properties of the alloy. However, strontium is a surface active element, and when it is modified, it is easy to increase the gas content of the aluminum melt.
[0035] In some embodiments, the die-casting aluminum alloy material includes, by weight: 8.0%-10.5% silicon, less than 0.2% iron, 1.3%-2.5% copper, 1.0%-2.0% magnesium, 0.5%-1.0% manganese, less than 1.0% zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, and less than 1.0% impurities.
[0036] In some embodiments, the die-casting aluminum alloy material includes, by weight: 8.0%-9.5% silicon, less than 0.15% iron, 1.4%-2.2% copper, 1.2%-1.8% magnesium, 0.5%-0.8% manganese, less than 0.8% zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, and less than 1.0% impurities.
[0037] In some embodiments, the die-casting aluminum alloy material includes, by weight, 8.0%-8.5% silicon, less than 0.15% iron, 1.4%-2.0% copper, 1.5%-1.8% magnesium, 0.5%-0.7% manganese, less than 0.8% zinc, 0.08%-0.1% titanium, 0.1%-0.15% zirconium, 0.02%-0.04% strontium, and less than 1.0% impurities.
[0038] In some embodiments, the die-casting aluminum alloy material consists of, by weight, 8.0%-10.5% silicon, less than 0.2% iron, 1.3%-2.5% copper, 1.0%-2.0% magnesium, 0.5%-1.0% manganese, less than 1.0% zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, less than 1.0% impurities and the remainder aluminum.
[0039] In some embodiments, the die-casting aluminum alloy material consists of, by weight, 8.0%-9.5% silicon, less than 0.15% iron, 1.4%-2.2% copper, 1.2%-1.8% magnesium, 0.5%-0.8% manganese, less than 0.8% zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, less than 1.0% impurities and the remainder aluminum.
[0040] In some embodiments, the die-casting aluminum alloy material consists of, by weight, 8.0%-8.5% silicon, less than 0.15% iron, 1.4%-2.0% copper, 1.5%-1.8% magnesium, 0.5%-0.7% manganese, less than 0.8% zinc, 0.08%-0.1% titanium, 0.1%-0.15% zirconium, 0.02%-0.04% strontium, less than 1.0% impurities and the remainder aluminum.
[0041] In some embodiments, the yield strength of the die-cast aluminum alloy material is above 230 MPa. In some embodiments, the yield strength of the die-cast aluminum alloy material is above 240 MPa. In some embodiments, the yield strength of the die-cast aluminum alloy material is 240 MPa-255 MPa or 240 MPa-250 MPa.
[0042] In some embodiments, the tensile strength of the die-cast aluminum alloy material is above 360 MPa. In some embodiments, the tensile strength of the die-cast aluminum alloy material is above 370 MPa.
[0043] In some embodiments, the elongation of the die-cast aluminum alloy material is greater than 3.0%. In some embodiments, the elongation of the die-cast aluminum alloy material is greater than 3.5%.
[0044] In some embodiments, the hardness of the die-cast aluminum alloy material is above 115 HB.
[0045] In some embodiments, the microstructure of the die-cast aluminum alloy material includes eutectic silicon phase, AlFeMnSi phase, Mg 2 Si phase, Al 2 Cu、Al x Mg 5 Si 4 Cu 4 At least one of .
[0046] In a second aspect, the present application provides a method for preparing a die-cast aluminum alloy material, comprising the following steps:
[0047] S1: mixing a silicon raw material, a manganese raw material, a copper raw material and an aluminum raw material and performing a heating treatment to obtain a first melt;
[0048] S2: mixing the first melt with a slag remover at a first temperature to remove slag, and then adding a titanium raw material, a zirconium raw material, a strontium raw material, a magnesium raw material and an optional zinc raw material to obtain an aluminum alloy material melt;
[0049] S3: die-casting the aluminum alloy material melt to obtain the die-cast aluminum alloy material.
[0050] In some embodiments, the silicon raw material is selected from at least one of aluminum silicon master alloy, industrial silicon or quick-dissolving silicon. In some embodiments, the manganese raw material is selected from aluminum manganese master alloy, such as Al-Mn10wt%. In some embodiments, the copper raw material is selected from aluminum copper master alloy, such as Al-Cu40wt%. In some embodiments, the aluminum raw material is selected from aluminum ingot. In some embodiments, the titanium raw material is selected from aluminum titanium master alloy, such as Al-Ti10wt%. In some embodiments, the zirconium raw material is selected from aluminum zirconium master alloy, such as Al-Zr5wt%. In some embodiments, the strontium raw material is selected from aluminum strontium master alloy, such as Al-Sr10wt%. In some embodiments, the magnesium raw material is selected from magnesium block. In some embodiments, the zinc raw material is selected from zinc block. In the present application, the Fe element in the alloy is mainly derived from the raw material aluminum ingot, master alloy or iron tool.
[0051] In some embodiments, the first temperature is 740°C-760°C, for example, 745°C, 750°C or 755°C. In some embodiments, the deslagging agent is selected from at least one of a chloride salt and a fluoride salt. In some embodiments, the chloride salt is selected from sodium chloride and / or potassium chloride. In some embodiments, the fluoride salt is selected from K 3 AlF 6 In some embodiments, based on the mass of the first melt, the mass content of the slag remover is 0.05%-0.2%, for example, 0.1% or 0.15%.
[0052] In some embodiments, before die-casting the aluminum alloy material melt in S3, the aluminum alloy material melt is analyzed, and when the chemical composition of the melt meets the requirements, the aluminum melt is degassed and refined with high-purity nitrogen or argon at 730±5° C. In some embodiments, the refining time is 10 min-30 min, such as 15 min, 20 min or 25 min.
[0053] In some embodiments, die casting includes: baking the mold to 200±20°C with a mold temperature controller, adjusting the temperature of the molten aluminum in the machine-side furnace to 690±10°C, and adjusting the process parameters of the die casting machine to: mold temperature 200±20°C, filling pressure 125Mpa, filling speed 3.0±0.2m / s, mold closing pressure 400T, holding time 3.5s, and injection cooling time 6.0s.
[0054] In some embodiments, the preparation method of the die-cast aluminum alloy material includes the following specific steps: thoroughly cleaning the furnace before feeding, removing the ash and slag, adding metallic silicon, Al-Mn, Al-Cu intermediate alloy and aluminum ingot according to the calculated weight, igniting and heating, and controlling the temperature of the aluminum liquid in the furnace at 750±10°C.
[0055] When the temperature of the aluminum liquid reaches the control temperature, the flux powder made of a mixture of chloride salt and fluoride salt is evenly sprayed into the bottom of the furnace at a rate of 0.15% of the weight of the aluminum liquid, and the aluminum liquid is stirred for 10 minutes with a rake. After the slag on the liquid surface is scraped off, Al-Ti, Al-Zr, Al-Sr and magnesium blocks and optional zinc blocks are added. After the melt is stirred for another 5 minutes, a spectral sample is taken, and the component analysis results meet the preset content.
[0056] When the melt chemical composition is qualified and the temperature is 730±5℃, use high-purity nitrogen or argon to degas and refine the aluminum melt. Refine for about 20 minutes, take the alloy decompression density sample, and test its density ≥2.68g / cm 3 When the pressure reaches 0.5000, stop degassing, remove the degassing rake, scrape off the slag on the liquid surface, let it stand for 15 minutes and then start die casting.
[0057] Start the die-casting machine, use the mold temperature controller to bake the mold to 200±20℃, adjust the temperature of the molten aluminum in the machine-side furnace to 690±10℃, and adjust the process parameters of the die-casting machine to: mold temperature 200±20℃, filling pressure 125Mpa, filling speed 3.0±0.2m / s, mold closing pressure 400T, holding time 3.5s, and injection cooling time 6.0s.
[0058] In a third aspect, the motor housing provided in the present application is made of the die-cast aluminum alloy material described in the first aspect or the die-cast aluminum alloy material prepared by the preparation method described in the second aspect.
[0059] In some embodiments, the motor housing is a motor housing used in a vehicle. In some embodiments, the vehicle includes at least one of an electric vehicle, a hybrid electric vehicle, and a plug-in hybrid electric vehicle.
[0060] In a fourth aspect, the present application provides the use of the die-cast aluminum alloy material described in the first aspect or the die-cast aluminum alloy material prepared by the preparation method described in the second aspect in a vehicle. In some embodiments, the present application provides the use of the above die-cast aluminum alloy material in new energy vehicles.
[0061] In some embodiments, the vehicle comprises at least one of an electric vehicle, a hybrid electric vehicle, and a plug-in hybrid electric vehicle.
[0062] Examples and Comparative Examples
[0063] Example 1
[0064] Before charging, the furnace is thoroughly cleaned and the ash is removed. Silicon, Al-Mn master alloy (Al-Mn 10wt%), Al-Cu master alloy (Al-Cu 40wt%) and aluminum ingot are added according to the weight calculated according to the expected alloy composition in Table 1. The furnace is ignited and heated to control the temperature of the aluminum liquid in the furnace at 750±10℃.
[0065] When the aluminum liquid temperature reaches the control temperature, add chloride salt (NaCl + KCl) and fluoride salt (K 3 AlF 6 ) mixed flux powder is evenly sprayed into the bottom of the furnace, and then the aluminum melt is stirred with a rake for 10 minutes. After the slag on the liquid surface is scraped off, Al-Ti master alloy (Al-Ti10wt%), Al-Zr master alloy (Al-Zr5wt%), Al-Sr master alloy (Al-Sr10wt%), magnesium block and zinc block are added according to the expected alloy composition in Table 1. After the melt is stirred for another 5 minutes, a spectral sample is taken, and the component analysis result meets the preset content.
[0066] When the melt chemical composition is qualified and the temperature is 730±5℃, use high-purity nitrogen or argon to degas and refine the aluminum melt. Refine for about 20 minutes, take the alloy decompression density sample, and test its density ≥2.68g / cm 3 When the pressure reaches 0.5000, stop degassing, remove the degassing rake, scrape off the slag on the liquid surface, let it stand for 15 minutes and then start die casting.
[0067] Start the die-casting machine, use the mold temperature controller to bake the mold to 200±20℃, adjust the temperature of the molten aluminum in the machine-side furnace to 690±10℃, and adjust the process parameters of the die-casting machine to: mold temperature 200±20℃, filling pressure 125Mpa, filling speed 3.0±0.2m / s, mold closing pressure 400T, holding time 3.5s, and injection cooling time 6.0s.
[0068] The die-cast test bars were placed in a room temperature environment and subjected to 48 h of natural aging for mechanical property testing using a tensile testing machine. The specific performance parameters are shown in Table 1.
[0069] Example 2-Example 6 and Comparative Example 1
[0070] The preparation process of the alloy materials of Examples 2 to 6 and Comparative Example 1 is the same as that of Example 1, the only difference being that the addition amounts of different raw materials are adjusted according to the expected alloy composition in Table 1.
[0071] Test Results
[0072] Table 1
[0073]
[0074] Although some exemplary embodiments of the present application have been illustrated and described, the present application is not limited to the disclosed embodiments. On the contrary, those skilled in the art will recognize that some modifications and changes may be made to the described embodiments without departing from the spirit and scope of the present application as described in the appended claims.
Claims
1. A die-casting aluminum alloy material, which is composed of 8.0%-11.0% silicon, 0.5% or less iron, 2.05%-2.5% copper, 1.0%-2.0% magnesium, 0.5%-1.2% manganese, 1.3% or less zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, 1.0% or less impurities and the balance aluminum, by weight, wherein: The mass ratio of the copper element to the magnesium element is (1.05-2.0):
1.
2. The die-casting aluminum alloy material according to claim 1, characterized in that: The mass ratio of the copper element to the magnesium element is (1.05-1.85):
1.
3. The die-casting aluminum alloy material according to claim 1, characterized in that: The mass ratio of the copper element to the magnesium element is (1.05-1.5):
1.
4. The die-casting aluminum alloy material according to claim 1, characterized in that: The die-casting aluminum alloy material consists, by weight, of 8.0%-10.5% silicon, less than 0.2% iron, 2.05%-2.5% copper, 1.0%-2.0% magnesium, 0.5%-1.0% manganese, less than 1.0% zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, less than 1.0% impurities and the remainder of aluminum.
5. The die-cast aluminum alloy material according to claim 1, characterized in that: The die-casting aluminum alloy material consists, by weight, of 8.0%-9.5% silicon, less than 0.15% iron, 2.05%-2.2% copper, 1.2%-1.8% magnesium, 0.5%-0.8% manganese, less than 0.8% zinc, 0.08%-0.15% titanium, 0.1%-0.2% zirconium, 0.02%-0.04% strontium, less than 1.0% impurities and the remainder of aluminum.
6. The die-cast aluminum alloy material according to any one of claims 1 to 5, characterized in that: The yield strength of the die-cast aluminum alloy material is above 230 MPa; and / or The tensile strength of the die-cast aluminum alloy material is above 360 MPa; and / or The elongation of the die-cast aluminum alloy material is above 3.0%; and / or The hardness of the die-cast aluminum alloy material is above 115HB.
7. The die-cast aluminum alloy material according to claim 6, characterized in that: The yield strength of the die-cast aluminum alloy material is above 240 MPa; and / or The tensile strength of the die-cast aluminum alloy material is above 370 MPa; and / or The elongation of the die-cast aluminum alloy material is above 3.5%; and / or The hardness of the die-cast aluminum alloy material is above 115HB.
8. A method for preparing a die-cast aluminum alloy material according to any one of claims 1 to 7, comprising the following steps: S1: mixing a silicon raw material, a manganese raw material, a copper raw material and an aluminum raw material and performing a first heating treatment to obtain a first melt; S2: mixing the first melt with a slag removal agent at a first temperature to remove slag, and then adding a titanium raw material, a zirconium raw material, a strontium raw material and a magnesium raw material to obtain an aluminum alloy material melt; S3: die-casting the aluminum alloy material melt to obtain the die-cast aluminum alloy material.
9. The preparation method according to claim 8, comprising the following steps: S1: mixing a silicon raw material, a manganese raw material, a copper raw material and an aluminum raw material and performing a first heating treatment to obtain a first melt; S2: mixing the first melt with a slag remover at a first temperature to remove slag, and then adding a titanium raw material, a zirconium raw material, a strontium raw material, a magnesium raw material and a zinc raw material to obtain an aluminum alloy material melt; S3: die-casting the aluminum alloy material melt to obtain the die-cast aluminum alloy material.
10. A motor housing, which is made of the die-cast aluminum alloy material according to any one of claims 1 to 7 or the die-cast aluminum alloy material prepared by the preparation method according to any one of claims 8 to 9.
11. Use of the die-cast aluminum alloy material according to any one of claims 1 to 7 or the die-cast aluminum alloy material prepared by the preparation method according to any one of claims 8 to 9 in a vehicle.
12. Use of the die-cast aluminum alloy material according to any one of claims 1 to 7 or the die-cast aluminum alloy material prepared by the preparation method according to any one of claims 8 to 9 in new energy vehicles.
Citation Information
Cited By
Heat-treatment-free Al-Si-Zn series die-casting aluminum alloy material, preparation method thereof and aluminum alloy structural part
CN120384224A
Die-casting aluminum alloy material and preparation method thereof
CN121023318A
Die-cast aluminum alloy material and method for manufacturing the same
CN121023318B
A high-strength, high-toughness, and corrosion-resistant die-cast aluminum alloy and its T5 heat treatment process.
CN123108363A