Nanometer ceramic bonding agent and preparation method thereof, silicon-based semiconductor chip back face thinning grinding wheel and preparation method and application of silicon-based semiconductor chip back face thinning grinding wheel

By combining nano-ceramic binder with diamond and composite pore-forming agents, microwave sintering technology is used to prepare silicon-based semiconductor chip backside thinning grinding wheels, which solves the problem of difficulty in uniform mixing of abrasives and binders and improves the mechanical properties and processing accuracy of the grinding wheels. , reducing costs.

CN118744404APending Publication Date: 2024-10-08郑师光

Patent Information

Application Number
CN202410730234.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When preparing fine-grained grinding wheels with the existing technology, it is difficult to mix the abrasives and bonding agents evenly, resulting in scratches on the silicon wafer surface and high costs. In addition, ultra-fine-grained bonding agents are difficult to prepare and disperse, which limits the development of high-precision grinding tools.

Method used

Using nanoceramic binder and its preparation method, anhydrous ethanol solution dissolved in sodium dodecylbenzene sulfonate is mixed with ethyl orthosilicate, acidic pH regulator and chelating agent are added, and a condensate is formed after polycondensation and hydrolysis reaction. The glue is sintered to form a nano-ceramic bonding agent, which is mixed with diamond and composite pore-forming agent to prepare a silicon-based semiconductor chip backside thinning grinding wheel through microwave sintering.

Benefits of technology

It improves the mechanical strength and toughness of the grinding wheel, reduces the sintering temperature and time, enhances the densification of the material, solves the problem of uniform mixing of abrasives and binders, and improves the processing accuracy and cost-effectiveness of the grinding tool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744404A_ABST
    Figure CN118744404A_ABST
Patent Text Reader

Abstract

The invention relates to a nano ceramic bonding agent and a preparation method thereof, a silicon-based semiconductor chip back face thinning grinding wheel and a preparation method and application of the silicon-based semiconductor chip back face thinning grinding wheel. The preparation method of the nano ceramic bonding agent comprises the following steps that an absolute ethyl alcohol solution dissolved with sodium dodecyl benzene sulfonate is evenly mixed with tetraethoxysilane, meanwhile, an acidic pH regulator is added, and the mixture is stirred to be uniform; adding a chelating agent, and stirring until the solution is clear and transparent to obtain a solution A; adding aluminum nitrate nonahydrate, boric acid and sodium nitrate into a mixed solution of deionized water and absolute ethyl alcohol, and uniformly mixing to obtain a solution B; adding the solution B into the solution A for multiple times, and carrying out polycondensation and hydrolysis reaction to obtain gel; the gel is dried and sintered after being subjected to aging treatment, and the nano ceramic binding agent is obtained; the preparation method of the silicon-based semiconductor chip back face thinning grinding wheel comprises the following steps that diamond, a composite pore forming agent and a nano ceramic binding agent are evenly mixed to obtain mixed powder, the powder is pressed, formed and sintered to obtain a grinding wheel block, the grinding wheel block and a base body are subjected to curing bonding or brazing welding, and the silicon-based semiconductor chip back face thinning grinding wheel is obtained. Compared with the prior art, the method has the advantages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grinding tools, and in particular to a nano ceramic binder and a preparation method thereof, a silicon-based semiconductor chip backside thinning grinding wheel and a preparation method and application thereof. Background Art

[0002] With the continuous expansion of the scale of the IC industry and the continuous development of manufacturing process technology, the requirements for the purity, geometric dimensions, processing accuracy, surface roughness, sub-surface damage, etc. of silicon wafer substrates are becoming higher and higher. The Mohs hardness of single-crystal silicon reaches 6.5, with high strength, and it is a typical hard and brittle material that is difficult to process.

[0003] In order to ensure the grinding surface quality of single crystal silicon wafers, the existing technology usually uses grinding wheels with micron or even submicron diamond abrasives as grinding tools. The traditional method of preparing fine-grained grinding wheels is prone to the following problems: On the one hand, when the abrasive reaches fine and ultra-fine grains, due to its high surface activity, it is easy to form agglomerates, which is difficult to mix evenly with the binder, and it is easy to cause scratches on the surface of the silicon wafer; on the other hand, due to the fine abrasive grain size, the binder grain size should also match it, and the ultra-fine grained binder is not easy to prepare and has a high cost. It is also easy to agglomerate and difficult to disperse. Therefore, the preparation of ceramic binders and the dispersion of ultra-fine abrasives restrict the development of high-precision grinding tools. Summary of the invention

[0004] The purpose of the present invention is to provide a nano-ceramic binder and a preparation method thereof, a silicon-based semiconductor chip back thinning grinding wheel and a preparation method and application thereof in order to overcome at least one of the defects of the above-mentioned prior art. The reason why the nano-ceramic binder can play a strengthening role is mainly because: the internal residual stress can cause crack deflection or pinning, the crack size of the nano-ceramic binder is reduced and deflected, and the internal crystalline structure is formed in the nano-ceramic binder after sintering.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] One of the purposes of the present invention is a method for preparing a nano-ceramic binder, comprising:

[0007] S1. Evenly mix an anhydrous ethanol solution containing sodium dodecylbenzene sulfonate and ethyl orthosilicate, add an acidic pH regulator, and then add a chelating agent and stir until clear and transparent to obtain liquid A;

[0008] S2. Add aluminum nitrate nonahydrate, boric acid and sodium nitrate to a mixture of deionized water and anhydrous ethanol and mix well to obtain solution B;

[0009] S3, adding liquid B to liquid A in multiple times to obtain liquid C, and subjecting liquid C to a gel through polycondensation and hydrolysis; subjecting the gel to aging treatment, drying, and sintering to obtain a nano-ceramic binder;

[0010] Wherein, the mass ratio of aluminum nitrate nonahydrate, sodium nitrate, tetraethyl orthosilicate and boric acid is (20-30):(10-15):(10-15):(40-60).

[0011] Furthermore, in step S1, the mass volume ratio of the sodium dodecylbenzene sulfonate to anhydrous ethanol is (150-250):1 mL / g, preferably 200:1 mL / g.

[0012] Furthermore, in step S1, the anhydrous ethanol solution containing sodium dodecylbenzenesulfonate is obtained by adding sodium dodecylbenzenesulfonate to anhydrous ethanol and uniformly stirring the mixture with ultrasonic stirring at a speed of 400-500 r / min and a stirring time of 30-60 min.

[0013] Furthermore, in step S1, ultrasonic stirring is performed during the mixing, the ultrasonic stirring speed is 400-500 r / min, and the ultrasonic stirring time is 120-180 min.

[0014] Furthermore, in step S1, the acidic pH regulator is one or more of hydrochloric acid, hydrobromic acid, hydroiodic acid, nitric acid and sulfuric acid.

[0015] Furthermore, in step S1, the chelating agent is acetylacetone.

[0016] Furthermore, in step S1, the stirring is ultrasonic stirring, and the ultrasonic stirring speed is 400-500r / min.

[0017] Furthermore, in step S2, ultrasonic stirring is performed during the mixing, and the ultrasonic stirring speed is 400-500r / min.

[0018] Furthermore, in step S2, the volume ratio of deionized water to anhydrous ethanol in the mixed solution of deionized water and anhydrous ethanol is (150-200):100.

[0019] Furthermore, in step S3, the liquid B is added to the liquid A in at least 5 times, and the liquid A is stirred at a speed of 400-500 r / min, preferably 400 r / min.

[0020] Furthermore, in step S3, the liquid C is stirred into a gel at a temperature of at least 70° C. and a speed of 400-500 r / min.

[0021] Furthermore, in step S3, the gel is aged at room temperature for at least 24 hours and then placed in an oven at at least 180° C. to dry to obtain a dry gel.

[0022] Furthermore, in step S3, the dry gel is placed in a microwave sintering furnace and sintered at 120° C., 180° C., 400° C. and 550° C. for 60 min, 60 min, 60 min and 360 min, respectively, to obtain a nano-ceramic binder.

[0023] The second object of the present invention is to provide a nano-ceramic binder, which is prepared by the preparation method as described above.

[0024] The third object of the present invention is to provide a method for preparing a grinding wheel for thinning the back side of a silicon-based semiconductor chip, comprising the following steps: uniformly mixing diamond, a composite pore-forming agent and the nano-ceramic binder as described above to obtain a mixed powder, pressing the powder into a shape, sintering the powder to obtain a grinding wheel block, and curing, bonding or brazing the grinding wheel block to a substrate to obtain a grinding wheel for thinning the back side of a silicon-based semiconductor chip.

[0025] Furthermore, the mass ratio of the diamond, the composite pore-forming agent and the nano-ceramic binder is 65:15:20.

[0026] Furthermore, the diamond is 6000#; the composite pore-forming agent is composed of wood powder, carbon black and hydroxyethyl cellulose in a mass ratio of (4-5):(2-3):2. Among them, the long-fiber wood powder is conducive to the formation of interconnected pores, and the hydroxyethyl cellulose added in the form of liquid is conducive to connecting the large-diameter pores formed by the wood powder and the small-diameter pores formed by the carbon black.

[0027] Furthermore, during the pressing process, the pressing pressure is at least 10MPa, and the pressure is maintained for at least 60s; during the sintering process, the sintering temperature is at least 600°C, and the temperature is maintained for at least 5h. The sintering temperature is preferably 650°C-750°C, and the temperature is maintained for 5h-7h. The sintering method of the present invention is microwave sintering. Microwave sintering is different from traditional sintering. During microwave heating, electromagnetic energy is absorbed by the material, the material as a whole heats up, and the heat is dissipated outward through the surface of the object. Microwave heating is a functional manifestation of the heated material. Microwave sintering can reduce the sintering temperature and shorten the sintering time in the process of promoting material densification. Microwave heating is the conversion of electromagnetic field energy into thermal energy, and its essence is the formation and vibration of dipoles.

[0028] A fourth object of the present invention is to provide a silicon-based semiconductor chip backside thinning grinding wheel, which is prepared by the preparation method described above.

[0029] A fifth object of the present invention is to use the silicon-based semiconductor chip back side thinning grinding wheel as described above in thinning the back side of a silicon-based semiconductor chip.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] (1) The nano-ceramic binder of the present invention can increase the mechanical strength and toughness of the grinding wheel because the internal residual stress can cause crack deflection or pinning, reduce the size and deflection of the cracks in the nano-ceramic binder, and form an internal crystalline structure in the nano-ceramic binder after sintering.

[0032] (2) The sintering method of the present invention is microwave sintering. Microwave sintering is different from traditional sintering. During the microwave heating process, electromagnetic energy is absorbed by the material, the material as a whole generates heat, and the heat is dissipated outward through the surface of the object. Microwave heating is a functional performance of the heated material. Microwave sintering can reduce the sintering temperature and shorten the sintering time in the process of promoting material densification. Microwave heating converts electromagnetic field energy into heat energy, and its essence is the formation and vibration of dipoles. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a graph showing the bending strength of a back-side thinning grinding wheel for a silicon-based semiconductor chip to which different nano-ceramic binders are added according to the present invention. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0035] Example 1

[0036] A method for preparing a nano-ceramic bond grinding wheel comprises the following steps:

[0037] 1) Add 1 g of sodium dodecylbenzene sulfonate to a beaker containing 200 mL of anhydrous ethanol, and stir ultrasonically for 60 min (40 kHz, 400 r / min); then add ethyl orthosilicate to the beaker solution, and stir ultrasonically for 180 min (40 kHz, 400 r / min); adjust the pH of the solution to 4 using 1 mol / L nitric acid solution, add 3 mL of acetylacetone as a chelating agent, and stir ultrasonically (40 kHz, 400 r / min) until the solution is clarified for standby use as solution A.

[0038]

[0039]

[0040] 2) According to the ratio in the above table, add aluminum nitrate nonahydrate, boric acid and sodium nitrate to a mixed solution of 180 mL of deionized water and 100 mL of anhydrous ethanol, stir the solution evenly in a magnetic stirrer at a speed of 400 r / min, and set aside as liquid B.

[0041] 3) Liquid B was added to Liquid A stirred at 400 r / min in a magnetic stirrer in 5 portions, and the uniformly mixed solution was stirred at 70° C. and 400 r / min to form a gel.

[0042] 4) After aging the gel at room temperature for 24 h, it was placed in an oven at 180° C. to obtain a xerogel.

[0043] 5) In order to remove the residual raw materials and organic matter, the dry gel was placed in a microwave sintering furnace and sintered at 120°C, 180°C, 400°C and 550°C for 60 min, 60 min, 60 min and 360 min, respectively, to obtain a nano-ceramic binder.

[0044] 6) The pore-forming agent used in the present invention is a composite pore-forming agent composed of wood flour, carbon black and hydroxyethyl cellulose, and the mass ratio of the composite pore-forming agent composed of wood flour, carbon black and hydroxyethyl cellulose is 5 / 3 / 2.

[0045] 7) According to the mass percentage, appropriate amounts of nano-ceramic binder: 20%, 6000# diamond: 65%, and composite pore-forming agent: 15% are mixed evenly, and then gently and evenly put into the grinding tool and scraped flat, and then placed in a hydraulic press for pressing at a pressure of 10 MPa and maintained for 60 seconds to obtain a grinding wheel with a size of 190 mm × 80 mm × 4 mm.

[0046] 8) The pressed grinding wheel is sintered at 600°C, kept warm for 5 hours, and cooled in the furnace.

[0047] 9) The sintered grinding wheel teeth are trimmed according to the predetermined size using a trimmer. Finally, the teeth are glued to the substrate processed by the lathe and grinder. After passing the inspection, they are packaged and stored to obtain the finished product.

[0048] Example 2

[0049] A method for preparing a nano-ceramic bond grinding wheel comprises the following steps:

[0050] 1) Add 1 g of sodium dodecylbenzene sulfonate to a beaker containing 200 mL of anhydrous ethanol, and stir ultrasonically for 60 min (40 kHz, 400 r / min); then add ethyl orthosilicate to the beaker solution, and stir ultrasonically for 180 min (40 kHz, 400 r / min); adjust the pH of the solution to 4 using 1 mol / L nitric acid solution, add 3 mL of acetylacetone as a chelating agent, and stir ultrasonically (40 kHz, 400 r / min) until the solution is clarified for standby use as solution A.

[0051]

[0052]

[0053] 2) According to the ratio in the above table, add aluminum nitrate nonahydrate, boric acid and sodium nitrate to a mixed solution of 180 mL of deionized water and 100 mL of anhydrous ethanol, stir the solution evenly in a magnetic stirrer at a speed of 400 r / min, and set aside as liquid B.

[0054] 3) Liquid B was added to Liquid A stirred at 400 r / min in a magnetic stirrer in 5 portions, and the uniformly mixed solution was stirred at 70° C. and 400 r / min to form a gel.

[0055] 4) After aging the gel at room temperature for 24 h, it was placed in an oven at 180° C. to obtain a xerogel.

[0056] 5) removing the residual raw materials and organic matter, placing the dry gel in a microwave sintering furnace, and sintering at 120° C., 180° C., 400° C. and 550° C. for 60 min, 60 min, 60 min and 360 min, respectively, to obtain a nano-ceramic binder.

[0057] 6) The pore-forming agent used in the present invention is a composite pore-forming agent composed of wood powder, carbon black and hydroxyethyl cellulose, the volume of which accounts for 10% of the volume percentage of the grinding wheel and abrasive tool, and the ratio of the composite pore-forming agent composed of wood powder, carbon black and hydroxyethyl cellulose is 5 / 3 / 2.

[0058] 7) According to the mass percentage, appropriate amounts of nano-ceramic binder: 23%, 6000# diamond: 60%, and composite pore-forming agent: 17% are mixed evenly, and then gently and evenly put into the grinding tool and scraped flat, and then placed in a hydraulic press for pressing at a pressure of 10 MPa and maintained for 60 seconds to obtain a grinding wheel with a size of 190 mm × 80 mm × 4 mm.

[0059] 8) The pressed grinding wheel is sintered at 650°C, kept warm for 6 hours, and cooled in the furnace.

[0060] 9) The sintered grinding wheel teeth are trimmed according to the predetermined size using a trimmer. Finally, the teeth are glued to the substrate processed by the lathe and grinder. After passing the inspection, they are packaged and stored to obtain the finished product.

[0061] Example 3

[0062] A method for preparing a nano-ceramic bond grinding wheel comprises the following steps:

[0063] 1) Add 1 g of sodium dodecylbenzene sulfonate to a beaker containing 200 mL of anhydrous ethanol, and stir ultrasonically for 60 min (40 kHz, 400 r / min); then add ethyl orthosilicate to the beaker solution, and stir ultrasonically for 180 min (40 kHz, 400 r / min); adjust the pH of the solution to 4 using 1 mol / L nitric acid solution, add 3 mL of acetylacetone as a chelating agent, and stir ultrasonically (40 kHz, 400 r / min) until the solution is clarified for standby use as solution A.

[0064]

[0065]

[0066] 2) According to the ratio in the above table, add aluminum nitrate nonahydrate, boric acid and sodium nitrate to a mixed solution of 180 mL of deionized water and 100 mL of anhydrous ethanol, stir the solution evenly in a magnetic stirrer at a speed of 400 r / min, and set aside as liquid B.

[0067] 3) Liquid B was added to Liquid A stirred at 400 r / min in a magnetic stirrer in 5 portions, and the uniformly mixed solution was stirred at 70° C. and 400 r / min to form a gel.

[0068] 4) After aging the gel at room temperature for 24 h, it was placed in an oven at 180° C. to obtain a xerogel.

[0069] 5) In order to remove the residual raw materials and organic matter, the dry gel was placed in a microwave sintering furnace and sintered at 120°C, 180°C, 400°C and 550°C for 60 min, 60 min, 60 min and 360 min, respectively, to obtain a nano-ceramic binder.

[0070] 6) The pore-forming agent used in the present invention is a composite pore-forming agent composed of wood flour, carbon black and hydroxyethyl cellulose, and the mass ratio of the composite pore-forming agent composed of wood flour, carbon black and hydroxyethyl cellulose is 5 / 3 / 2.

[0071] 7) According to the mass percentage, appropriate amounts of nano-ceramic binder: 25%, 6000# diamond: 70%, and composite pore-forming agent: 5% are mixed evenly, and then gently and evenly put into the grinding tool and scraped flat, and then placed in a hydraulic press for pressing at a pressure of 10 MPa and maintained for 60 seconds to obtain a grinding wheel with a size of 190 mm × 80 mm × 4 mm.

[0072] 8) The pressed grinding wheel is sintered at 700°C, kept warm for 7 hours, and cooled in the furnace.

[0073] 9) The sintered grinding wheel teeth are trimmed according to the predetermined size using a trimmer. Finally, the teeth are glued to the substrate processed by the lathe and grinder. After passing the inspection, they are packaged and stored to obtain the finished product.

[0074] Bending strength test

[0075] The materials in Examples 1-3 were mixed according to the proportions and pressed into sample strips of 30×15×4 mm. The bending strength was tested by a universal material testing machine. The bending strength of the grinding wheel sample was tested by a three-point bending method on the universal material testing machine.

[0076] from Figure 1 It can be seen that the strength when the binder accounts for 23% is greater than the strength when the binder accounts for 20% and 25%. Therefore, the bending strength of the grinding wheel can be adjusted and the mechanical properties of the grinding wheel can be improved by adjusting the mass proportion of the nano-ceramic binder.

[0077] Silicon wafer thinning test

[0078] A DISCO thinning machine was used to grind 8-inch sapphire wafers, with a grinding wheel speed of 4800rpm, a fine grinding amount of 20μm, and 50 wafers were ground without trimming.

[0079] Ten silicon wafers obtained after thinning in Examples 1-3 were respectively taken for testing, and finally the grinding parameters of the grinding wheel were counted.

[0080] The test data are shown in the following table:

[0081] sample Example 1 Example 2 Example 3 Surface TTV value (μm) <2 <2 <2 Roughness range Ra(nm) 11-15 12-15 10-15 Wear ratio (μm / piece) 0.11 0.13 0.12

[0082] It can be seen from the test data that the silicon wafer thinning grinding wheels prepared in Examples 1-3 of the present invention not only ensure the surface physical characteristics of the silicon wafer after grinding, but also have a low wear ratio, thus meeting the service life requirements of the grinding wheels.

[0083] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a nano-ceramic binder, characterized in that: include: S1. Evenly mix an anhydrous ethanol solution containing sodium dodecylbenzene sulfonate and ethyl orthosilicate, add an acidic pH regulator, and then add a chelating agent and stir until clear and transparent to obtain liquid A; S2. Add aluminum nitrate nonahydrate, boric acid and sodium nitrate to a mixture of deionized water and anhydrous ethanol and mix well to obtain solution B; S3, adding liquid B to liquid A in multiple times to obtain liquid C, and subjecting liquid C to a gel through polycondensation and hydrolysis; subjecting the gel to aging treatment, drying, and sintering to obtain a nano-ceramic binder; Wherein, the mass ratio of aluminum nitrate nonahydrate, sodium nitrate, tetraethyl orthosilicate and boric acid is (20-30):(10-15):(10-15):(40-60).

2. The method for preparing a nano-ceramic binder according to claim 1, characterized in that: In step S1, the mass volume ratio of the sodium dodecylbenzene sulfonate to anhydrous ethanol is (150-250): 1 mL / g; In step S1, the anhydrous ethanol solution containing sodium dodecylbenzene sulfonate is obtained by adding sodium dodecylbenzene sulfonate to anhydrous ethanol and uniformly stirring the mixture with ultrasonic stirring at a speed of 400-500 r / min and a stirring time of 30-60 min; In step S1, during the mixing, ultrasonic stirring is performed, the ultrasonic stirring speed is 400-500 r / min, and the ultrasonic stirring time is 120-180 min; In step S1, the acidic pH regulator is one or more of hydrochloric acid, hydrobromic acid, hydroiodic acid, nitric acid and sulfuric acid; In step S1, the chelating agent is acetylacetone; In step S1, the stirring is ultrasonic stirring, and the ultrasonic stirring speed is 400-500r / min.

3. The method for preparing a nano-ceramic binder according to claim 1, characterized in that: In step S2, during the mixing, ultrasonic stirring is performed, and the ultrasonic stirring speed is 400-500 r / min; In step S2, the volume ratio of deionized water to anhydrous ethanol in the mixed solution of deionized water and anhydrous ethanol is (150-200):

100.

4. The method for preparing a nano-ceramic binder according to claim 1, characterized in that: In step S3, the liquid B is added to the liquid A in at least 5 times, while the liquid A is stirred at a speed of 400-500 r / min; In step S3, the liquid C is stirred into a gel at a temperature of at least 70° C. and a speed of 400-500 r / min; In step S3, the gel is aged at room temperature for at least 24 hours and then placed in an oven at at least 180° C. to dry to obtain a xerogel; In step S3, the dry gel is placed in a microwave sintering furnace and sintered at 120° C., 180° C., 400° C. and 550° C. for 60 min, 60 min, 60 min and 360 min, respectively, to obtain a nano-ceramic binder.

5. A nano-ceramic binder, characterized in that: The invention discloses a novel nanostructured carbon foam prepared by the preparation method according to any one of claims 1 to 4.

6. A method for preparing a back thinning grinding wheel for a silicon-based semiconductor chip, characterized in that: The method comprises the following steps: uniformly mixing diamond, a composite pore-forming agent and the nano-ceramic binder as claimed in claim 5 to obtain a mixed powder, pressing the powder into a shape, sintering the mixture to obtain a grinding wheel block, and curing and bonding or brazing the grinding wheel block to a substrate to obtain a back thinning grinding wheel for a silicon-based semiconductor chip.

7. The method for preparing a back thinning grinding wheel for a silicon-based semiconductor chip according to claim 6, characterized in that: The mass ratio of the diamond, the composite pore-forming agent and the nano-ceramic binder is 65:15:20; The diamond is 6000#; the composite pore-forming agent is composed of wood powder, carbon black and hydroxyethyl cellulose in a mass ratio of (4-5):(2-3):

2.

8. The method for preparing a back thinning grinding wheel for a silicon-based semiconductor chip according to claim 6, characterized in that: During the pressing process, the pressing pressure is at least 10 MPa and the pressure is maintained for at least 60 seconds; During the sintering process, the sintering temperature is at least 600° C. and the temperature is kept at least 5 hours.

9. A grinding wheel for thinning the back side of a silicon-based semiconductor chip, characterized in that: It is prepared by the preparation method according to any one of claims 6 to 8.

10. Use of the silicon-based semiconductor chip backside thinning grinding wheel as claimed in claim 9 in thinning the backside of a silicon-based semiconductor chip.

Citation Information

Patent Citations

  • Ceramic bond CBN (Cubic Boron Nitride) abrasive wheel for double end surface grinding

    CN102837266A

  • High-precision automobile part machining grinding wheel and production process thereof

    CN109159035A

  • Grinding wheel based on high-wear-resistance diamond micro powder and preparation process of grinding wheel

    CN117773796A

Cited By

  • Ultrathin cutting blade and preparation method thereof

    CN116373140A

  • Ultra-thin cutting blade and preparation method thereof

    CN116373140B

  • Diamond grinding tooth, preparation method thereof and thinning grinding wheel

    CN119567120A