Impermeable waterproof breathable coiled material

Through the design of a four-layer structure of impermeable, waterproof and breathable membrane, electrospinning jetting and hot pressing composite technology are used to form a ZnO@PU/PVDF nanofiber membrane, which solves the problem of insufficient breathability and antibacterial performance of the waterproof membrane and achieves higher Waterproof, breathable and antibacterial effect.

CN118744583AActive Publication Date: 2024-10-08ANHUI AOJIA BUILDING MATERIALS CO LTD

Patent Information

Application Number
CN202410787587.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-08
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Existing waterproof membranes lack breathability and antibacterial properties, and are prone to aging and breeding of bacteria during long-term use, affecting human health and comfort.

Method used

It adopts a four-layer structure of anti-permeable, waterproof and breathable membrane design, including a breathable upper layer, a reinforced fiber layer, a waterproof TPO layer and a breathable lower layer. The ZnO@PU/PVDF nanofiber membrane is formed through electrospinning jetting and hot pressing composite technology to increase the porosity. and antimicrobial properties.

Benefits of technology

It effectively improves the waterproof, breathable and antibacterial properties of the membrane, reduces the penetration channels, improves the impermeability and UV resistance, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744583A_ABST
    Figure CN118744583A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-seepage waterproof breathable coiled material, and belongs to the technical field of waterproof coiled materials. The impermeable waterproof breathable coiled material with a four-layer structure is formed by combining the ZnO coated PU / PVDF nanofiber membrane, the glass fiber base cloth and the waterproof TPO material. According to the present invention, the glass fiber base cloth is adopted as the reinforcing fiber layer and has good mechanical property, the polypropylene resin, the calcium carbonate, the TPO resin, the polyethylene resin and other raw materials are subjected to melt extrusion, and the melt extrusion and the glass fiber base cloth are subjected to calendaring molding drafting to form the two-layer structure, and on the basis, the ZnO coated PU / PVDF nanofiber membrane is subjected to electrostatic spinning and hot pressing compounding to prepare the impermeable waterproof breathable coiled material with the four-layer structure, the nano zinc oxide endows the coiled material with good antibacterial and anti-ultraviolet aging performance, the nanofiber membrane prepared by combining the polyurethane and the PVDF has excellent waterproof and air permeability, the L-shaped landing edge structure of the coiled material is realized by combining the bonding performance of the PVDF, and the convenience of landing edge operation is improved while the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproof coiled materials, and in particular relates to an anti-seepage waterproof breathable coiled material. Background Art

[0002] Waterproof membrane is mainly used for building walls, roofs, tunnels, roads, landfills, etc. It is a flexible building material product that can be rolled into a roll to resist the seepage of external rainwater and groundwater. As a leak-free connection between the project foundation and the building, it is the first barrier to waterproofing the entire project and plays a vital role in the entire project.

[0003] Based on the composition of the materials, the commonly used waterproofing membranes in construction projects are divided into three types: asphalt waterproofing membranes, synthetic polymer waterproofing membranes, and modified asphalt waterproofing membranes. Among them, synthetic polymer waterproofing membranes are based on rubber and synthetic resins, with a small amount of fillers and chemical additives added. After multiple processes, they are made into sheet-like waterproofing materials with curling conditions. The two sides of the membrane are polyester layers, and the middle layer is a polymer layer. The membranes include terpolymer rubber waterproofing membranes, chloroprene rubber membranes, etc. According to the main ingredients, the products can be roughly divided into: ethylene propylene diene monomer rubber (EPDM) membranes, polyvinyl chloride (PVC) membranes, thermoplastic polyolefin (TPO) waterproofing membranes, and polymer self-adhesive pre-laid (MBP) waterproofing membranes. The performance indicators of synthetic polymer membranes are relatively high, with excellent waterproofness, weather resistance, elasticity and tensile strength.

[0004] At present, the commonly used waterproofing membranes on the market are basically not breathable, or have very low breathability. When used for roof waterproofing, it is not conducive to ventilation of the internal environment, reducing the comfort of living. In addition, when the waterproofing membrane is exposed to sunlight, it will age under the long-term ultraviolet rays and cracks will appear on the surface. When the waterproofing membrane is used on the roof and wall, a large number of bacteria will breed in a long-term humid environment, which is not good for human health. Summary of the invention

[0005] The object of the present invention is to provide an anti-seepage waterproof breathable coiled material to improve the air permeability and antibacterial properties of the waterproof coiled material.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] The present invention provides an anti-seepage waterproof breathable coiled material, which comprises, from top to bottom, an air-permeable upper layer, a reinforcing fiber layer, a waterproof TPO layer and an air-permeable lower layer in sequence, wherein the air-permeable upper layer and the reinforcing fiber layer are bonded by electrostatic spinning spraying and hot pressing compounding, the air-permeable upper layer in the transverse direction extends to the left and right by the same distance than the reinforcing fiber layer, and the portion extending to the right is bonded and sealed with the right side of the coiled material by hot melting, the reinforcing fiber layer and the waterproof TPO layer are bonded by calendering, the waterproof TPO layer and the air-permeable lower layer are bonded by electrostatic spinning and hot pressing compounding, the air-permeable lower layer in the transverse direction extends to the left and right by the same distance than the waterproof TPO layer, and the portion extending to the left is bonded and sealed with the left side of the coiled material by hot melting;

[0008] The air permeable upper layer and the air permeable lower layer are both ZnO@PU / PVDF nanofiber membranes;

[0009] Furthermore, the reinforcing fiber layer is a glass fiber base cloth;

[0010] The raw materials of the waterproof TPO layer include 20-40 parts of polypropylene resin, 25-35 parts of calcium carbonate powder, 30-40 parts of TPO resin, 15-25 parts of polyethylene resin, 1-5 parts of antioxidant 1010, 1-3 parts of stearic acid, 0.5-2 parts of titanate coupling agent and 0.5-2 parts of titanium dioxide by weight.

[0011] Adding calcium carbonate powder increases the porosity of the waterproof TPO layer and improves the breathability of the membrane.

[0012] Furthermore, the thickness of the anti-seepage, waterproof and breathable coiled material is 2.0 mm;

[0013] Furthermore, the thickness of the ZnO@PU / PVDF nanofiber membrane is 0.1 to 0.3 mm;

[0014] Furthermore, the preparation steps of the anti-seepage waterproof breathable coiled material are as follows:

[0015] (1) the raw materials of the waterproof TPO layer are fully mixed in proportion, put into a twin-screw extruder for heating and then melt extrusion, and a composite material is formed by calendaring and drawing with a glass fiber base cloth, wherein the upper layer of the composite material is a reinforcing fiber layer and the lower layer is a waterproof TPO layer;

[0016] (2) adding polyurethane particles and PVDF powder into a mixed solvent according to a mass ratio, heating and stirring at 80° C. to prepare a mixed solution, adding nano zinc oxide powder into the mixed solution and ultrasonically dispersing the mixed solution to obtain a ZnO@PU / PVDF spinning solution;

[0017] (3) The composite material is used as a receiving substrate, and the ZnO@PU / PVDF spinning solution is electrospun to form a ZnO@PU / PVDF nanofiber membrane on both the upper and lower layers of the composite material, and then hot-pressed at 170°C to obtain an anti-seepage, waterproof and breathable roll material, wherein the upper layer is a breathable upper layer and the lower layer is a breathable lower layer;

[0018] (4) Cut and hot-melt bond the anti-seepage waterproof and breathable membrane.

[0019] Furthermore, the heating temperature of the twin-screw extruder is 230-280°C.

[0020] Furthermore, the mass ratio of the polyurethane particles to the PVDF powder is 2:8 to 8:2. The polyurethane nanofiber membrane has excellent air permeability but has hydrophobic defects. PVDF has good hydrophobicity and toughness, and the blending and modification of the two play a complementary role.

[0021] Furthermore, the mixed solvent is prepared by mixing a polar solvent and acetone;

[0022] The volume ratio of the polar solvent to acetone is 2:8 to 4:6, and the mixing of the polar solvent and acetone is conducive to the dissolution of polyurethane and PVDF;

[0023] The polar solvent is one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

[0024] Furthermore, the mass proportion of the polyurethane particles and the PVDF powder in the mixed solution is 10%-15%;

[0025] The mass proportion of the nano zinc oxide powder in the spinning solution is 1%-5%.

[0026] Furthermore, the voltage of the electrospinning is 25 kV, the receiving distance is 10 cm, the spinning speed is 1 mL / h, and the inner diameter of the syringe needle is 0.5 mm.

[0027] Beneficial effects of the present invention:

[0028] (1) A four-layer structure of anti-seepage waterproof and breathable roll material is formed by compounding a breathable upper layer, a reinforcing fiber layer, a waterproof TPO layer and a breathable lower layer. Compared with the traditional TPO waterproof roll material, the nanofiber membrane is used as the breathable upper layer and the breathable lower layer. The nanofiber membrane structure with small pore size and high porosity effectively improves the waterproof and breathable properties of the roll material. The four-layer structure has a complex pore structure, which reduces the penetration channel and improves the anti-seepage property.

[0029] (2) A nanofiber membrane is prepared by mixing nano zinc oxide, polyurethane and polyvinylidene fluoride. Nano zinc oxide absorbs, reflects and scatters ultraviolet light to improve the anti-ultraviolet performance of the coil. Nano zinc oxide has a photocatalytic effect under light irradiation, producing substances such as hydroxide, oxygen anions and hydrogen peroxide, thereby playing an antibacterial role and giving the coil antibacterial properties. The chelating effect of polyurethane makes it difficult for nano zinc oxide in the nanofiber membrane to fall off, thereby improving the dispersibility.

[0030] (3) Doping with nano zinc oxide can transform polyvinylidene fluoride into β-phase. β-phase is the secondary phase structure of PVDF, which has a lower melting point and higher flexibility. It makes the nanofiber membrane have better adhesion when hot-pressed at a lower temperature and better compatibility with polyurethane.

[0031] (4) Through cutting and hot-melt bonding of the anti-seepage waterproof breathable roll material, an L-shaped structure with an overall seal and the extended part of the breathable layer as the overlap band is formed. By rationally utilizing the hot-melt bonding properties of the ZnO@PU / PVDF nanofiber membrane, the intermediate layer material is saved while the overlap is simple during use and the sealing is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention will be further described below in conjunction with the accompanying drawings.

[0033] Figure 1 It is a schematic structural diagram of an embodiment of the present invention.

[0034] In the figure: 1. Breathable upper layer; 2. Reinforced fiber layer; 3. Waterproof TPO layer; 4. Breathable lower layer. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] See also Figure 1The present invention provides an anti-seepage, waterproof and breathable coiled material, comprising an air-permeable upper layer 1, a reinforcing fiber layer 2, a waterproof TPO layer 3 and a breathable lower layer 4, the air-permeable upper layer 1 and the reinforcing fiber layer 2 are bonded by electrostatic spinning and hot pressing, the air-permeable upper layer 1 extends to the left and right by the same distance than the reinforcing fiber layer 2 in the transverse direction, and the rightward extending portion is bonded and sealed with the right side of the coiled material by hot melting, the reinforcing fiber layer 2 and the waterproof TPO layer 3 are bonded by calendering, the waterproof TPO layer 3 and the air-permeable lower layer 4 are bonded by electrostatic spinning and hot pressing, the air-permeable lower layer 4 extends to the left and right by the same distance than the waterproof TPO layer 3 in the transverse direction, and the leftward extending portion is bonded and sealed with the left side of the coiled material by hot melting, when two pieces of anti-seepage, waterproof and breathable coiled materials need to overlap, the leftward extending portion of the air-permeable upper layer 1 is hot-melt bonded to the upper surface of the anti-seepage, waterproof and breathable coiled material, and the rightward extending portion of the air-permeable lower layer 4 is hot-melt bonded to the lower surface of the anti-seepage, waterproof and breathable coiled material, to achieve an L-shaped overlapping structure of the coiled material.

[0037] Example 1

[0038] Weigh the raw materials according to weight proportions, including 30 parts of polypropylene resin, 30 parts of calcium carbonate powder, 35 parts of TPO resin, 20 parts of polyethylene resin, 10103 parts of antioxidant, 2 parts of stearic acid, 1 part of titanate coupling agent and 1 part of titanium dioxide, stir and mix the raw materials and put them into a twin-screw extruder at a temperature of 250°C for melt extrusion, and introduce the glass fiber base cloth as a reinforcing fiber layer into the drawing roller, and extrude the composite reinforcing fiber layer and the waterproof TPO layer through the upper and lower rollers to form a composite material, wherein the upper layer of the composite material is the reinforcing fiber layer, and the lower layer is the waterproof TPO layer.

[0039] A mixed solvent with a volume ratio of DMF / acetone of 3:7 was prepared, and polyurethane (PU) particles and PVDF powder were added to the mixed solvent in a mass ratio of 5:5. The mixed solution was prepared by heating and stirring at 80°C, in which the sum of the mass of PU and PVDF accounted for 12%. Nano zinc oxide powder was then added to the mixed solution, in which the mass proportion of the nano zinc oxide powder was 3%. Ultrasonic dispersion was performed for 1 hour to obtain a spinning solution, which was then cooled to room temperature.

[0040] The electrospinning voltage was set to 25 kV, the receiving distance was 10 cm, the spinning speed was 1 mL / h, the inner diameter of the syringe needle was 0.5 mm, the composite material was used as the receiving substrate, the spinning solution was sprayed through the syringe, and a ZnO@PU / PVDF nanofiber membrane with a thickness of 0.2 mm was formed on both sides of the composite material. It was further hot-pressed at 170°C to make the ZnO@PU / PVDF nanofiber membrane bonded to the composite material as the breathable upper layer and the breathable lower layer to obtain an anti-seepage, waterproof and breathable roll with a thickness of 2.0 mm.

[0041] The obtained anti-seepage waterproof breathable coiled material is further cut and hot-melt bonded to obtain Figure 1The anti-seepage, waterproof and breathable membrane with the overlapped structure shown.

[0042] Example 2

[0043] The difference from Example 1 is that the mass ratio of polyurethane (PU) particles to PVDF powder is 2:8, and the other steps are the same as Example 1.

[0044] Example 3

[0045] The difference from Example 1 is that the mass ratio of polyurethane (PU) particles to PVDF powder is 8:2, and the other steps are the same as Example 1.

[0046] Example 4

[0047] The difference from Example 1 is that the mass proportion of nano zinc oxide powder is 1%, and the other steps are the same as Example 1.

[0048] Example 5

[0049] The difference from Example 1 is that the mass proportion of nano zinc oxide powder is 5%, and the other steps are the same as Example 1.

[0050] Example 6

[0051] The difference from Example 1 is that the thickness of the ZnO@PU / PVDF nanofiber membrane is 0.1 mm, and the other steps are the same as Example 1.

[0052] Example 7

[0053] The difference from Example 1 is that the thickness of the ZnO@PU / PVDF nanofiber membrane is 0.3 mm, and the other steps are the same as Example 1.

[0054] Example 8

[0055] Weigh the raw materials according to weight proportions, including 20 parts of polypropylene resin, 25 parts of calcium carbonate powder, 30 parts of TPO resin, 15 parts of polyethylene resin, 10101 parts of antioxidant, 1 part of stearic acid, 0.5 parts of titanate coupling agent and 0.5 parts of titanium dioxide, stir and mix the raw materials and put them into a twin-screw extruder at a temperature of 230°C for melt extrusion, and introduce the glass fiber base cloth as a reinforcing fiber layer into the drawing roller, and extrude and draw the composite reinforcing fiber layer and the waterproof TPO layer through the upper and lower rollers to form a composite material, wherein the upper layer of the composite material is the reinforcing fiber layer, and the lower layer is the waterproof TPO layer.

[0056] A mixed solvent with a volume ratio of DMAC / acetone of 2:8 was prepared, polyurethane (PU) particles and PVDF powder were added to the mixed solvent in a mass ratio of 5:5, and the mixed solution was prepared by heating and stirring at 80°C, in which the sum of the mass of PU and PVDF accounted for 10%, and nano zinc oxide powder was added to the mixed solution, in which the mass proportion of the nano zinc oxide powder was 3%, and ultrasonic dispersion was performed for 1 hour to obtain a spinning solution, which was then cooled to room temperature.

[0057] The electrospinning voltage was set to 25 kV, the receiving distance was 10 cm, the spinning speed was 1 mL / h, the inner diameter of the syringe needle was 0.5 mm, the composite material was used as the receiving substrate, the spinning solution was sprayed through the syringe, and a ZnO@PU / PVDF nanofiber membrane with a thickness of 0.2 mm was formed on both sides of the composite material. It was further hot-pressed at 170°C to make the ZnO@PU / PVDF nanofiber membrane bonded to the composite material as the breathable upper layer and the breathable lower layer to obtain an anti-seepage, waterproof and breathable roll with a thickness of 2.0 mm.

[0058] The obtained anti-seepage waterproof breathable coiled material is further cut and hot-melt bonded to obtain Figure 1 The anti-seepage, waterproof and breathable membrane with the overlapped structure shown.

[0059] Example 9

[0060] Weigh the raw materials according to weight proportions, including 40 parts of polypropylene resin, 35 parts of calcium carbonate powder, 40 parts of TPO resin, 25 parts of polyethylene resin, 10105 parts of antioxidant, 3 parts of stearic acid, 2 parts of titanate coupling agent and 2 parts of titanium dioxide, stir and mix the raw materials and put them into a twin-screw extruder at a temperature of 280°C for melt extrusion, and introduce the glass fiber base cloth as a reinforcing fiber layer into the drawing roller, and extrude and draw the composite reinforcing fiber layer and the waterproof TPO layer through the upper and lower rollers to form a composite material, wherein the upper layer of the composite material is the reinforcing fiber layer, and the lower layer is the waterproof TPO layer.

[0061] A mixed solvent with a volume ratio of DMAC / acetone of 2:8 was prepared, polyurethane (PU) particles and PVDF powder were added to the mixed solvent in a mass ratio of 5:5, and a mixed solution was prepared by heating and stirring at 80°C, in which the sum of the mass of PU and PVDF accounted for 15%. Nano zinc oxide powder was then added to the mixed solution, in which the mass proportion of the nano zinc oxide powder was 3%, and ultrasonic dispersion was performed for 1 hour to obtain a spinning solution, which was then cooled to room temperature.

[0062] The electrospinning voltage was set to 25 kV, the receiving distance was 10 cm, the spinning speed was 1 mL / h, the inner diameter of the syringe needle was 0.5 mm, the composite material was used as the receiving substrate, the spinning solution was sprayed through the syringe, and a ZnO@PU / PVDF nanofiber membrane with a thickness of 0.2 mm was formed on both sides of the composite material. It was further hot-pressed at 170°C to make the ZnO@PU / PVDF nanofiber membrane bonded to the composite material as the breathable upper layer and the breathable lower layer to obtain an anti-seepage, waterproof and breathable roll with a thickness of 2.0 mm.

[0063] The obtained anti-seepage waterproof breathable coiled material is further cut and hot-melt bonded to obtain Figure 1 The anti-seepage, waterproof and breathable membrane with the overlapped structure shown.

[0064] Comparative Example 1

[0065] Compared with Example 1, nano titanium dioxide powder is used to replace nano zinc oxide powder, and other steps are the same as Example 1.

[0066] Comparative Example 2

[0067] Compared with Example 1, polyurethane (PU) and nano zinc oxide powder are used to prepare the spinning solution, PVDF powder is removed, and the other steps are the same as Example 1.

[0068] Comparative Example 3

[0069] Compared with Example 1, PVDF powder and nano zinc oxide powder are used to prepare the spinning solution, polyurethane (PU) is removed, and the other steps are the same as Example 1.

[0070] Comparative Example 4

[0071] Compared with Example 1, polyurethane (PU) and PVDF powders are used to prepare the spinning solution, the nano zinc oxide powder is removed, and the other steps are the same as Example 1.

[0072] Comparative Example 5

[0073] Compared with Example 1, the anti-seepage waterproof breathable coiled material has no breathable upper layer and breathable lower layer, and uses the glass fiber base cloth as the middle reinforcing fiber layer, and the upper and lower layers are calendered composite waterproof TPO layers.

[0074] Weigh the raw materials according to weight, including 30 parts of polypropylene resin, 30 parts of calcium carbonate powder, 35 parts of TPO resin, 20 parts of polyethylene resin, 10103 parts of antioxidant, 2 parts of stearic acid, 1 part of titanate coupling agent and 1 part of titanium dioxide, stir and mix the raw materials, and put them into two twin-screw extruders of equal mass at a temperature of 250°C for melt extrusion, and introduce the glass fiber base cloth as the middle reinforcing fiber layer into the drafting roller, and extrude the composite waterproof TPO upper layer, the reinforcing fiber layer and the waterproof TPO lower layer through three-roll extrusion drafting to form a coiled material. The coiled material is as follows: Figure 1As shown in the figure, the upper waterproof TPO layer is similar to the breathable upper layer of the embodiment, and the lower waterproof TPO layer is similar to the breathable lower layer of the embodiment.

[0075] Performance tests were performed on Examples 1 to 9 and Comparative Examples 1 to 5, and the results are shown in Table 1.

[0076] Refer to GB 27789-2011 "Thermoplastic polyolefin (TPO) waterproof membrane" for mechanical properties and water permeability and water absorption performance tests;

[0077] Refer to GB / T 1038.1-2022 "Plastic film and sheet gas permeability test method Part 1: Differential pressure method" for gas permeability test;

[0078] Refer to GB / T 30706-2014 "Test method and evaluation of antibacterial performance of photocatalytic antibacterial materials and products under visible light irradiation" for performance antibacterial performance testing.

[0079] Table 1

[0080]

[0081]

[0082] According to Table 1, in Examples 1-3, the mass ratio of urethane (PU) particles and PVDF powder in the ZnO@PU / PVDF nanofiber membrane is adjusted, the proportion of PU increases, the elongation at break of the coil first increases and then decreases, the water absorption rate increases, the air permeability increases, and the water permeability decreases slightly. Too much PU is not conducive to waterproof performance, and the appropriate proportion is conducive to improving the elongation at break. Compared with Example 1, the proportion of nano zinc oxide in Example 4 and Example 5 is different. The increase in the content of nano zinc oxide is obviously beneficial to the antibacterial and anti-aging properties. In Example 6 and Example 7, the thickness of the ZnO@PU / PVDF nanofiber membrane is different from that in Example 1. The increase in the thickness of the ZnO@PU / PVDF nanofiber membrane is beneficial to the enhancement of mechanical properties and impermeability, but the thickness is too large and the air permeability will be significantly reduced. The coils in Examples 8 and 9 have similar properties to those in Example 1, and all properties are good. In Comparative Example 1, nano titanium dioxide is used to replace nano zinc oxide, but the antibacterial and anti-ultraviolet properties of nano zinc oxide are better than those of nano titanium dioxide. In Comparative Example 2, the water absorption rate of the coiled material prepared without PVDF is improved, the waterproof performance is reduced, and the seam peeling strength is greatly reduced. In Comparative Example 3, the air permeability of the coiled material prepared without polyurethane is poor, and the antibacterial and anti-ultraviolet performance are slightly reduced, mainly due to the obvious agglomeration of nano zinc oxide. In Comparative Example 4, when nano zinc oxide is not added, the antibacterial and anti-aging properties of the coiled material are significantly reduced. Comparative Example 5 uses TPO waterproof coiled material prepared by traditional technology. The adhesion of TPO material is not as good as that of PVDF material, the seam peeling strength at the overlap is poor, and the gas permeability is very low, and the antibacterial and anti-aging properties are significantly weaker.

[0083] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An anti-seepage, waterproof and breathable coiled material, characterized in that: From top to bottom, the breathable upper layer (1), the reinforcing fiber layer (2), the waterproof TPO layer (3) and the breathable lower layer (4) are sequentially bonded by electrostatic spinning and hot pressing. The breathable upper layer (1) extends to the left and right by the same distance than the reinforcing fiber layer (2), and the portion extending to the right is bonded and sealed by hot melting with the right side of the coiled material. The reinforcing fiber layer (2) and the waterproof TPO layer (3) are bonded by calendaring. The waterproof TPO layer (3) and the breathable lower layer (4) are bonded by electrostatic spinning and hot pressing. The breathable lower layer (4) extends to the left and right by the same distance than the waterproof TPO layer (3), and the portion extending to the left is bonded and sealed by hot melting with the left side of the coiled material. The breathable upper layer (1) and the breathable lower layer (4) are both ZnO@PU / PVDF nanofiber membranes.

2. The anti-seepage waterproof breathable coiled material according to claim 1, characterized in that: The reinforcing fiber layer (2) is a glass fiber base cloth; The raw materials of the waterproof TPO layer (3) include, by weight, 20-40 parts of polypropylene resin, 25-35 parts of calcium carbonate powder, 30-40 parts of TPO resin, 15-25 parts of polyethylene resin, 1-5 parts of antioxidant 1010, 1-3 parts of stearic acid, 0.5-2 parts of titanate coupling agent and 0.5-2 parts of titanium dioxide.

3. The anti-seepage waterproof breathable coiled material according to claim 1, characterized in that: The thickness of the anti-seepage, waterproof and breathable coiled material is 2.0 mm.

4. The anti-seepage waterproof breathable coiled material according to claim 1, characterized in that: The thickness of the ZnO@PU / PVDF nanofiber membrane is 0.1-0.3 mm.

5. The anti-seepage waterproof breathable coiled material according to claim 1, characterized in that: Prepared by the following steps: (1) mixing the raw materials of the waterproof TPO layer (3) in proportion, putting them into a twin-screw extruder for heating and then melting and extruding, and forming a composite material with a glass fiber base cloth through calendaring and drawing, wherein the upper layer of the composite material is a reinforcing fiber layer (2) and the lower layer is a waterproof TPO layer (3); (2) polyurethane particles and PVDF powder are added to a mixed solvent according to a mass ratio, heated and stirred at 80° C. to prepare a mixed solution, and nano zinc oxide powder is added to the mixed solution and ultrasonically dispersed for 1 h to obtain a ZnO@PU / PVDF spinning solution; (3) The composite material is used as a receiving substrate, and the ZnO@PU / PVDF spinning solution is electrospun to form a ZnO@PU / PVDF nanofiber membrane on both the upper and lower layers of the composite material, and then hot-pressed at 170° C. to obtain an anti-seepage, waterproof and breathable roll material, wherein the upper layer is a breathable upper layer (1) and the lower layer is a breathable lower layer (4); (4) Cut and hot-melt bond the anti-seepage, waterproof and breathable membrane to form an L-shaped overlap structure.

6. The anti-seepage waterproof breathable coiled material according to claim 5, characterized in that: The heating temperature of the twin-screw extruder is 230-280°C.

7. The anti-seepage waterproof breathable coiled material according to claim 5, characterized in that: The mass ratio of the urethane particles to the PVDF powder is 2:8 to 8:

2.

8. The anti-seepage waterproof breathable coiled material according to claim 5, characterized in that: The mixed solvent is prepared by mixing a polar solvent and acetone; The volume ratio of the polar solvent to acetone is 2:8 to 4:6; The polar solvent is one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

9. The anti-seepage waterproof breathable coiled material according to claim 5, characterized in that: The mass proportion of the polyurethane particles and the PVDF powder in the mixed solution is 10%-15%; The mass proportion of the nano zinc oxide powder in the spinning solution is 1%-5%.

10. The anti-seepage waterproof breathable coiled material according to claim 5, characterized in that: The voltage of the electrospinning is 25 kV, the receiving distance is 10 cm, the spinning speed is 1 mL / h, and the inner diameter of the syringe needle is 0.5 mm.

Citation Information

Patent Citations

  • Thermoplastic polyolefin TPO waterproof coiled material and preparation method thereof

    CN107933034A

  • Preparation method of polyvinylidene fluoride / polyurethane cross-linked modified glass fiber composite veneering material

    CN118024709A

  • ETES high polymer modified asphalt waterproofing membrane

    CN204820509U

  • TPO macromolecular self-adhesive film waterproof roll

    CN209466785U

  • Snow blanket

    US9271335B1

Cited By

  • Permeable plastic composite pervious concrete and preparation method thereof

    CN120718435A