High-rate hard carbon negative electrode material and preparation method thereof

Through the high-temperature carbonization preparation method of phenolic resin and organic copper compounds, the problem of poor conductivity and rate performance of traditional graphite anode materials in sodium-ion batteries has been solved, and efficient hard carbon anode material preparation has been achieved, which is suitable for the field of electric vehicles.

CN118744978APending Publication Date: 2024-10-08TAIAN FARADAY ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410750984.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional graphite anode materials are difficult to meet the needs of commercial applications in sodium-ion batteries due to poor conductivity and rate performance, especially in the field of electric vehicles.

Method used

Phenolic resin and organic copper compounds (such as copper gluconate, copper porphyrin, copper octoate, etc.) are used as carbon sources and catalysts to prepare hard carbon negative electrode materials through high-temperature carbonization. The organic copper compounds are converted into Cu nanoparticles during the carbonization process. Improve graphitization degree and electrical conductivity.

Benefits of technology

It significantly improves the conductivity and rate capacity of hard carbon materials, simplifies the synthesis process, reduces industrialization costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744978A_ABST
    Figure CN118744978A_ABST
Patent Text Reader

Abstract

The invention discloses a high-rate hard carbon negative electrode material and a preparation method thereof.The high-rate hard carbon negative electrode material is prepared through high-temperature carbonization with phenolic resin as a carbon source precursor and an organic copper compound as a catalyst. And preparing the hard carbon negative electrode material through high-temperature carbonization. Graphite carbon with a high graphitization degree is prepared at a low temperature by adding an organic copper compound, meanwhile, the conductivity of the hard carbon material is greatly improved, and the hard carbon material is applied as a sodium-ion battery negative electrode material and shows high rate capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery materials, and in particular to a high-rate hard carbon negative electrode material and a preparation method thereof. Background Art

[0002] With the rapid expansion of power generation from renewable energy sources such as solar energy and wind energy, research on new materials for energy storage batteries is also deepening. my country is rich in sodium resources, and sodium-ion batteries are considered to be the most suitable new type of batteries for large-scale energy storage, and are expected to alleviate problems such as the limited development of energy storage caused by the shortage and uneven distribution of lithium resources. However, the ionic radius of sodium ions (0.102nm) is much larger than the ionic radius of lithium ions (0.076nm), which seriously hinders the application of traditional graphite negative electrode materials from a kinetic point of view. Therefore, it is necessary to find suitable negative electrode materials to meet the application needs of commercial sodium-ion batteries.

[0003] Hard carbon has become an extremely excellent negative electrode material for sodium-ion batteries due to its excellent performance and low cost. Hard carbon can be divided into biomass-based hard carbon and synthetic polymer-based hard carbon. The former is obtained by heat treatment of biomass, and the synthetic organic polymer is obtained by artificial synthesis. Synthetic polymer-based hard carbon materials represented by phenolic resin have high specific capacity, controllable raw materials, and good product consistency, but poor conductivity and rate performance, which do not meet the requirements of sodium-ion batteries in the field of electric vehicles. Summary of the invention

[0004] Aiming at the problem that the conductivity and rate performance of hard carbon materials prepared by phenolic resin are poor, the present invention proposes a feasible method for preparing hard carbon negative electrode materials and has the feasibility of large-scale production.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A high-rate hard carbon negative electrode material comprises a phenolic resin and an organic copper compound.

[0007] A method for preparing a high-rate hard carbon negative electrode material, wherein phenolic resin is used as a carbon source precursor, an organic copper compound is used as a catalyst, and the hard carbon negative electrode material is prepared by high-temperature carbonization.

[0008] As a further embodiment of the present invention, the organic copper compound is any one of copper gluconate, copper porphyrin, copper octanoate, copper-based trimesic acid (Cu-BTC), cuprous cyanamide, copper cyanide, copper citrate, copper malate, copper acetate, sodium copper ethylenediaminetetraacetate, copper oxalate and copper benzoate.

[0009] As a further solution of the present invention: the ratio of the phenolic resin to the organic copper compound is 100:1-25.

[0010] As a further solution of the present invention: the carbonization temperature is 1350-1550°C.

[0011] As a further solution of the present invention: the heating rate during the carbonization process is 1-20°C / min.

[0012] As a further solution of the present invention: the atmosphere of the carbonization process is a protective gas, specifically any one or more of N2, Ar, He, H2, NH3, and CO2.

[0013] A sodium ion battery comprising the high-rate hard carbon negative electrode material according to claim 1.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] The above invention method can provide a hard carbon negative electrode material and a preparation method thereof and a sodium ion battery, and the synthesis method can obtain an optimized negative electrode material. The beneficial details are as follows:

[0016] 1. The organic copper compound is converted into Cu nanoparticles in situ during the carbonization process, which catalyzes the surrounding carbon to generate graphite carbon with a high degree of graphitization at low temperature. At the same time, the generation of Cu metal can greatly improve the conductivity of the hard carbon material, thereby improving the hard carbon rate capacity.

[0017] 2. Nitrogen-containing catalysts (cuprous cyanamide, copper cyanide, copper porphyrin) can introduce nitrogen elements into hard carbon, and can also improve the electrical conductivity of hard carbon materials and change the interlayer spacing.

[0018] The synthesis process is simple, and the Cu metal does not need to be removed by pickling, so it has industrial prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a TEM image of the hard carbon negative electrode material obtained in Example 1 after acid washing to remove copper. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1:

[0022] A hard carbon negative electrode material and a preparation method thereof and a sodium ion battery, the specific implementation scheme of which is as follows:

[0023] Mix 10g of copper citrate and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 2.5℃ per minute and keep them warm for 3 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0024] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 285.6 mAh g -1 .

[0025] Embodiment 2:

[0026] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0027] Mix 20g of copper citrate and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 2.5℃ per minute and keep them warm for 3 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0028] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 285.6 mAh g -1 .

[0029] Embodiment 3:

[0030] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0031] Mix 30g of copper citrate and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 2.5℃ per minute and keep them warm for 3 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0032] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 288.4 mAh g-1 .

[0033] Embodiment 4:

[0034] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0035] Mix 40g of copper citrate and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 2.5℃ per minute and keep them warm for 3 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0036] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 282.8 mAh g -1 .

[0037] Embodiment 5:

[0038] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0039] Mix 50g of copper citrate and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 2.5℃ per minute and keep them warm for 3 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0040] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 280.5 mAh g -1 .

[0041] Embodiment 6:

[0042] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0043] Mix 30g of copper gluconate and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 1.5℃ per minute and keep them warm for 2 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0044] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 288.2 mAh g -1 .

[0045] Embodiment 7:

[0046] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0047] Mix 30g of cuprous cyanamide and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 1.5℃ per minute and keep them warm for 2 hours, then heat them to 1450℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0048] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 289.8 mAh g -1 .

[0049] Embodiment 8:

[0050] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0051] Mix 30g of copper cyanide and 1kg of phenolic resin evenly, put them into a tubular furnace in He atmosphere, heat up to 650℃ at 1.5℃ per minute and keep it for 2 hours, heat up to 1350℃ at 5℃ per minute and keep it for 3 hours, and after cooling, you can get a hard carbon negative electrode material.

[0052] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 290.3 mAh g -1 .

[0053] Embodiment 9:

[0054] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0055] Mix 30g of copper porphyrin and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 550℃ at 1℃ per minute and keep them warm for 2 hours, then heat them to 1500℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0056] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 287.3 mAh g -1 .

[0057] Embodiment 10:

[0058] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0059] Mix 30g of copper octylate and 1kg of phenolic resin evenly, put them into a tubular furnace in Ar atmosphere, heat them to 600℃ at 2℃ per minute and keep them warm for 2 hours, then heat them to 1400℃ at 2.5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0060] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 286.6 mAh g -1 .

[0061] Embodiment 11:

[0062] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0063] Mix 30g Cu-BTC and 1kg phenolic resin evenly, put them into a tubular furnace in Ar atmosphere, heat them to 600℃ at 3℃ per minute and keep them warm for 2 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, the hard carbon negative electrode material can be obtained.

[0064] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1The first discharge capacity at current density is 287.4 mAh g -1 .

[0065] Embodiment 12:

[0066] Preferably, the above-mentioned feature item is a hard carbon negative electrode material, a preparation method thereof, and a sodium ion battery, and its specific implementation scheme is as follows:

[0067] Mix 30g of copper malate and 1kg of phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them at 2.5℃ per minute to 600℃ and keep them warm for 2 hours, then heat them at 5℃ per minute to 1400℃ and keep them warm for 5 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0068] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 287.4 mAh g -1 .

[0069] Comparative Example 1:

[0070] Mix 1 kg of phenolic resin evenly, put it into a tubular furnace in a N2 atmosphere, heat it to 600°C at 1.5°C per minute and keep it for 2 hours, then heat it to 1400°C at 5°C per minute and keep it for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0071] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1 The first discharge capacity at current density is 175.2 mAh g -1 .

[0072] Comparative Example 2:

[0073] Mix 30g zinc gluconate and 1kg phenolic resin evenly, put them into a tubular furnace in a N2 atmosphere, heat them to 600℃ at 1.5℃ per minute and keep them warm for 2 hours, then heat them to 1400℃ at 5℃ per minute and keep them warm for 3 hours. After cooling, a hard carbon negative electrode material can be obtained.

[0074] The sodium ion battery uses hard carbon negative electrode material as the negative electrode material, sodium metal sheet as the positive electrode, the electrolyte is 1MNaFP6 dissolved in EC:DMC (1:1), and the separator is Celgard 2400 to carry out electrochemical testing. -1The first discharge capacity at current density is 188.2 mAh g -1 .

[0075] The above is a specific implementation method formed by combining some of the characteristic methods provided in the present invention. It should be pointed out that for ordinary technicians in this technical field, several implementation methods can be formed without departing from the principles of the present invention. These implementation methods formed based on the present invention should also be regarded as the protection scope of the present invention.

[0076] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0077] In addition, it should be understood that although the present specification is described in terms of implementation modes, not every implementation mode contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment have also been appropriately combined to form other implementation modes that those skilled in the art can understand.

Claims

1. A high rate hard carbon negative electrode material, characterized in that: Includes phenolic resins and organic copper compounds.

2. A method for preparing a high-rate hard carbon negative electrode material, characterized in that: The hard carbon negative electrode material is prepared by high-temperature carbonization using phenolic resin as a carbon source precursor and an organic copper compound as a catalyst.

3. The method for preparing a high-rate hard carbon negative electrode material according to claim 2, characterized in that: The organic copper compound is any one of copper gluconate, copper porphyrin, copper octanoate, copper-based trimesic acid (Cu-BTC), cuprous cyanamide, copper cyanide, copper citrate, copper malate, copper acetate, sodium copper ethylenediaminetetraacetate, copper oxalate and copper benzoate.

4. The method for preparing a high-rate hard carbon negative electrode material according to claim 2, characterized in that: The ratio of the phenolic resin to the organic copper compound is 100:1-25.

5. The method for preparing a high-rate hard carbon negative electrode material according to claim 2, characterized in that: The carbonization temperature is 1350-1550°C.

6. The method for preparing a high-rate hard carbon negative electrode material according to claim 2, characterized in that: The heating rate during the carbonization process is 1-20°C / min.

7. The method for preparing a high-rate hard carbon negative electrode material according to claim 2, characterized in that: The atmosphere of the carbonization process is a protective gas, specifically any one or more of N2, Ar, He, H2, NH3, and CO2.

8. A sodium ion battery, characterized in that: Including the high-rate hard carbon negative electrode material as described in claim 1.