Preparation method and application of special magnesium oxide
Through silicon carbide radiant panel flame heating and zoned temperature control technology, the problem of unstable magnesium oxide quality has been solved, and the preparation of high purity and low specific surface area magnesium oxide has been achieved. It is suitable for cover glass and LED thermal conductive materials, improving product quality. quality and production efficiency.
Patent Information
- Application Number
- CN202410750695.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
AI Technical Summary
The research and application of magnesium oxide in China are out of touch, and the production equipment is single, resulting in uneven quality of magnesium oxide, which cannot meet the needs of high purity and low specific surface area, affecting its application in cover glass and LED thermal conductive materials.
Silicon carbide radiant plate flame heating and zoned temperature control heating technology are used to ensure the high purity and low specific surface area of magnesium oxide. Through zoned temperature control heating, more uniform heating and precise temperature control are achieved, reducing energy consumption and production costs.
Achieved the preparation of high purity (more than 99%), low specific surface area (less than 10m2/g) magnesium oxide, improved the clarity and quality performance of glass, reduced production costs and technical thresholds, and is suitable for cover glass and LED thermal conductivity Material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical product preparation technology, and in particular relates to a preparation method of special magnesium oxide and application thereof. Background Art
[0002] Entering the 21st century, electronic products and e-commerce occupy a major share in production, and our daily life is inseparable from electronic products. Among these electronic products, the touch screen, which we commonly refer to as cover glass, has been widely valued and studied as part of emerging electronic products. Our mobile phones, computers, navigation devices, various electronic touch screens, etc. are undergoing changes again and again as people study cover glass. As the most important raw material for cover glass, magnesium oxide is also moving forward step by step to adapt to the challenges of this new field.
[0003] At present, the research on magnesium oxide in China is still in its infancy, and there is still a big gap between the current technology and that of Japan and Israel. The main reasons for this situation are: people's research and application of magnesium oxide are out of touch, the equipment for producing magnesium oxide is single and limited, and there is no unified standard for the application of magnesium oxide; the above three reasons have resulted in the uneven production of magnesium oxide, and the good and the bad are mixed. This situation puts customers who use magnesium oxide in a dilemma and unable to make a decision.
[0004] Therefore, how to provide a method for preparing magnesium oxide for cover glass with simple process, small specific surface area and high purity is a problem that needs to be solved urgently by R&D technicians in this field. Summary of the invention
[0005] Based on the above problems, the present invention proposes a method for preparing special magnesium oxide. The specific technical scheme is as follows:
[0006] A method for preparing special magnesium oxide specifically comprises the following steps: calcining raw materials at 700-800°C for at least 90 minutes to obtain special magnesium oxide.
[0007] Furthermore, the raw material is high-purity magnesium hydroxide or magnesium carbonate.
[0008] Furthermore, the heating for calcination adopts a silicon carbide radiation plate.
[0009] Furthermore, the calcination is heated by zoned temperature control.
[0010] Furthermore, the zoned temperature-controlled heating includes 8 heating zones, and the temperatures of each zone are: 200-250°C in zone 1, 250-300°C in zone 2, 300-400°C in zone 3, 400-500°C in zone 4, 500-600°C in zone 5, 600-700°C in zone 6, 700-750°C in zone 7, and 750-800°C in zone 8.
[0011] Furthermore, the residence times of the eight heating zones are: 10 minutes in zone 1, 10 minutes in zone 2, 15 minutes in zone 3, 15 minutes in zone 4, 15 minutes in zone 5, 15 minutes in zone 6, 45 minutes in zone 7, and 45 minutes in zone 8.
[0012] On the other hand, the present invention discloses magnesium oxide obtained by the method for preparing the special magnesium oxide.
[0013] Furthermore, the purity of the magnesium oxide is above 99%, and the bulk density is greater than 1g / cm 3 , whiteness greater than 98, specific surface area of 10m 2 / g or less.
[0014] Furthermore, the present invention discloses the use of the magnesium oxide in preparing cover glass and LED thermal conductive materials.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0016] The present invention adopts the silicon carbide radiation plate for flame insulation heating and calcination to avoid direct flame contact with raw materials, reduce local overheating or underheating, make heating more uniform, and ensure more stable quality of magnesium oxide products. Due to the efficient heat transfer performance of the silicon carbide radiation plate, lower energy consumption can be achieved under the same heating conditions, thereby reducing production costs.
[0017] The present invention adopts a zoned temperature control heating method, which can reduce energy waste, improve energy utilization, reduce energy consumption and production costs in the production process, make the production process more stable and controllable, shorten the production cycle, improve production efficiency, and increase output. By accurately controlling the temperature and residence time of each heating zone, the specific surface area of magnesium oxide can be regulated, thereby reducing its activity value, which is of great significance for producing high-quality magnesium oxide suitable for the glass industry. Magnesium oxide with low specific surface area and low activity value can provide higher clarity and better quality performance in glass production.
[0018] Compared with the traditional method, the preparation method adopted in the present invention is simple and intuitive, does not require complicated operation steps and equipment, and reduces the production cost and technical threshold. DETAILED DESCRIPTION
[0019] The following will clearly and completely describe the technology of the present invention in combination with the embodiments; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments; based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work should belong to the protection scope of the present invention. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0020] Embodiment 1:
[0021] This embodiment describes in detail a method for preparing special magnesium oxide using magnesium hydroxide as a raw material, and the specific steps are as follows:
[0022] Raw materials: Choose high-purity magnesium hydroxide (Mg(OH)2) as the raw material, and ensure that the purity of the raw material is above 99%. Evenly put 500 grams of magnesium hydroxide raw material into a ceramic crucible. The ceramic crucible can maintain stability under high temperature conditions and prevent the raw material from reacting with other substances.
[0023] Calcination equipment: In this embodiment, a push plate kiln is used as the calcination equipment. The zoned heating of the push plate kiln can ensure that the temperature distribution during the calcination process is more uniform and controllable by independently regulating the temperature of each zone. By setting different temperature gradients in different zones, gradual heating and cooling can be achieved. Through precise temperature control, magnesium oxide with low activity value can be produced, which is suitable for use in glass kilns. Low activity value magnesium oxide is more stable in glass manufacturing and is not prone to chemical reactions, thereby improving the clarity of the glass.
[0024] Install silicon carbide radiation panels in the pusher kiln for flame insulation heating to ensure heat transfer efficiency and temperature uniformity. Silicon carbide radiation panels have excellent thermal conductivity and high temperature resistance.
[0025] Zoned temperature-controlled calcination: Push the ceramic crucible containing the magnesium hydroxide raw material into the push-plate kiln for calcination. The push-plate kiln is divided into 8 temperature zones. Each temperature zone is independently controlled to achieve gradual heating and cooling, which are:
[0026] Preheating area:
[0027] Zone 1: Raise the temperature to 200°C at a rate of 5°C per minute and hold for 10 minutes.
[0028] Zone 2: Raise the temperature to 300°C at a rate of 5°C per minute and hold for 10 minutes.
[0029] The purpose of the preheating zone is to slowly increase the temperature to remove moisture from the magnesium hydroxide and avoid damage to the material due to drastic temperature changes.
[0030] Decomposition area:
[0031] Zone 3: Heat up to 400°C at a rate of 7°C per minute and stay for 15 minutes.
[0032] Zone 4: Raise the temperature to 500°C at a rate of 7°C per minute and hold for 15 minutes.
[0033] Zone 5: Heat up to 600°C at a rate of 7°C per minute and stay for 15 minutes.
[0034] The purpose of the decomposition zone is to gradually increase the temperature so that the magnesium hydroxide decomposes and releases water and hydroxide.
[0035] The temperature for calcining and decomposing magnesium hydroxide (Mg(OH)2) is approximately between 350°C and 550°C. Specifically, magnesium hydroxide decomposes when heated to produce magnesium oxide (MgO) and water vapor (H2O), and the reaction is as follows:
[0036] Mg(OH)2→MgO+H2O
[0037] This step is usually carried out in a relatively low temperature range, but in order to ensure complete decomposition and obtain high-quality magnesium oxide, a higher temperature range (close to or exceeding 500°C) is often selected in actual industrial operations.
[0038] Pre-calcination area:
[0039] Zone 6: Heat up to 700°C at a rate of 10°C per minute and stay for 15 minutes.
[0040] The purpose of the pre-calcination zone is to further increase the temperature in preparation for entering the high temperature calcination stage.
[0041] Calcination area:
[0042] Zone 7: Heat up to 750°C at a rate of 15°C per minute and stay for 45 minutes.
[0043] Zone 8: Raise the temperature to 800°C at a rate of 15°C per minute and hold for 45 minutes.
[0044] The purpose of the calcining zone is to fully sinter the magnesium oxide crystals under high temperature conditions to form an ideal crystal structure and reduce the specific surface area and activity value. The role of the silicon carbide radiation plate in this area is particularly important to ensure uniform temperature distribution and stable control.
[0045] Cooling and Collection:
[0046] After calcination, take the ceramic crucible out of the push plate kiln and let the magnesium oxide cool naturally to room temperature. Avoid rapid cooling during the cooling process to prevent the magnesium oxide crystal structure from being destroyed.
[0047] Screening and crushing:
[0048] The cooled magnesium oxide is processed through screening and crushing equipment to ensure particle uniformity and appropriate particle size. The goal is to obtain a specific surface area of 10m 2 / g or less magnesium oxide powder to ensure low activity value.
[0049] Product Inspection:
[0050] The purity, bulk density, whiteness and specific surface area of the prepared magnesium oxide were tested.
[0051] The test results show that the purity of the obtained magnesium oxide is 99.5% and the bulk density is 1.1g / cm 3 , whiteness is 99, specific surface area is 9.5m 2 / g, fully meets the requirements of magnesium oxide for cover glass.
[0052] application:
[0053] The magnesium oxide product can be widely used in the production process of cover glass, which can significantly improve the clarity of the glass, reduce bubbles and twill, and improve the quality and performance of glass products.
[0054] Embodiment 2:
[0055] This embodiment describes in detail a method for preparing special magnesium oxide using magnesium carbonate as a raw material, and the specific steps are as follows:
[0056] Raw material preparation: Choose high-purity magnesium carbonate (MgCO3) as the raw material, and ensure that the purity of the raw material is above 99%. Evenly put 500 grams of magnesium carbonate raw material into a ceramic crucible.
[0057] Zoned temperature-controlled calcination: Push the ceramic crucible containing the magnesium hydroxide raw material into the push-plate kiln for calcination, and enter the following zones respectively:
[0058] Preheating area:
[0059] Zone 1: Raise the temperature to 200°C at a rate of 5°C per minute and hold for 10 minutes.
[0060] Zone 2: Raise the temperature to 300°C at a rate of 5°C per minute and hold for 10 minutes.
[0061] Decomposition area:
[0062] Zone 3: Heat up to 400°C at a rate of 7°C per minute and stay for 15 minutes.
[0063] Zone 4: Raise the temperature to 500°C at a rate of 7°C per minute and hold for 15 minutes.
[0064] Zone 5: Heat up to 600°C at a rate of 7°C per minute and stay for 15 minutes.
[0065] The temperature for calcining and decomposing magnesium carbonate (MgCO3) is approximately between 350°C and 600°C. When magnesium carbonate is heated, it decomposes to produce magnesium oxide (MgO) and carbon dioxide (CO2). The reaction is as follows:
[0066] MgCO3→MgO+CO2
[0067] At around 350°C, magnesium carbonate begins to decompose, but in order to ensure complete decomposition and obtain high-quality magnesium oxide, a high temperature of 500-600°C helps ensure that the reaction proceeds fully and avoids residual undecomposed magnesium carbonate.
[0068] Pre-calcination area:
[0069] Zone 6: Heat up to 700°C at a rate of 10°C per minute and stay for 15 minutes.
[0070] Calcination area:
[0071] Zone 7: Heat up to 750°C at a rate of 15°C per minute and stay for 45 minutes.
[0072] Zone 8: Raise the temperature to 800°C at a rate of 15°C per minute and hold for 45 minutes.
[0073] Cooling and collection: After calcination, take the ceramic crucible out of the push plate kiln and let the magnesium oxide cool naturally to room temperature. Avoid rapid cooling during the cooling process to prevent the crystal structure of magnesium oxide from being destroyed.
[0074] Screening and crushing: The cooled magnesium oxide is processed through screening and crushing equipment to ensure particle uniformity and appropriate particle size. The goal is to obtain a specific surface area of 10m 2 / g or less magnesium oxide powder to ensure low activity value.
[0075] Product inspection: The purity, bulk density, whiteness and specific surface area of the produced magnesium oxide are tested.
[0076] The test results show that the purity of the obtained magnesium oxide is 99.3% and the bulk density is 1.1g / cm 3 , whiteness is 98.5, specific surface area is 9m 2 / g, fully meets the requirements of magnesium oxide for cover glass.
[0077] Application: This magnesium oxide product can be widely used in the production process of cover glass, which can significantly improve the clarity of glass, reduce bubbles and twill, and improve the quality and performance of glass products.
Claims
1. A method for preparing special magnesium oxide, characterized in that: The method specifically comprises the following steps: calcining the raw materials at 700-800° C. for at least 90 minutes to obtain a special magnesium oxide.
2. The method for preparing a special magnesium oxide according to claim 1, characterized in that: The raw material is magnesium hydroxide or magnesium carbonate.
3. The method for preparing a special magnesium oxide according to claim 1, characterized in that: The calcination is heated by using a silicon carbide radiation plate.
4. The method for preparing a special magnesium oxide according to claim 1, characterized in that: The calcination is heated by zoned temperature control.
5. The method for preparing a special magnesium oxide according to claim 4, characterized in that: The zoned temperature-controlled heating includes 8 heating zones, and the temperatures of each zone are: 200-250°C in zone 1, 250-300°C in zone 2, 300-400°C in zone 3, 400-500°C in zone 4, 500-600°C in zone 5, 600-700°C in zone 6, 700-750°C in zone 7, and 750-800°C in zone 8.
6. The method for preparing a special magnesium oxide according to claim 5, characterized in that: The residence times of the eight heating zones are: 10 minutes in zone 1, 10 minutes in zone 2, 15 minutes in zone 3, 15 minutes in zone 4, 15 minutes in zone 5, 15 minutes in zone 6, 45 minutes in zone 7, and 45 minutes in zone 8.
7. The magnesium oxide obtained by the method for preparing a special magnesium oxide according to any one of claims 1 to 6.
8. The magnesium oxide according to claim 7, characterized in that The purity of the magnesium oxide is above 99%, and the bulk density is greater than 1g / cm 3 , whiteness greater than 98, specific surface area of 10m 2 / g or less.