Preparation method of high-defect titanium dioxide material for forming sub-monolayer passivation layer to protect Ti < 3 + > through shallow surface doping

The method of forming a sub-monolayer passivation layer through shallow surface doping stabilizes highly defective titanium dioxide materials under low temperature conditions, solves the problems of material stability and high cost in traditional methods, and achieves efficient light absorption and electrochemical activity improvement. Suitable for many application areas.

CN118745000APending Publication Date: 2024-10-08NORTHEASTERN UNIV CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410744915.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When introducing high-defect titanium dioxide materials, the existing technology faces problems such as high-temperature heat treatment leading to a decrease in the structural stability of the material, high preparation costs, difficulty in accurately controlling defect type and distribution through ion implantation, and possible environmental risks.

Method used

A shallow surface doping method is used to form a sub-monolayer passivation layer under low temperature conditions, and the highly defective titanium dioxide material is stabilized through a specific alkaline electrolyte and annealing process to ensure the structural stability of the material and precise control of defect types.

Benefits of technology

It achieves the effective introduction of high-defective titanium dioxide materials under low temperature conditions, reduces preparation costs, improves the stability and light absorption capacity of the material, broadens the light absorption range, and enhances electrochemical activity. It is suitable for photocatalysis, photovoltaic cells and gas transmission. Sensory and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745000A_ABST
    Figure CN118745000A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nano material preparation, and discloses a preparation method of a high-defect titanium dioxide material for protecting Ti < 3 + > by forming a sub-monolayer passivation layer through shallow surface doping. A sub-monolayer passivation layer is formed through shallow surface doping, so that Ti < 3 + > in the high-defect titanium dioxide material is protected; the high-defect titanium dioxide material is an amorphous titanium dioxide material, the amorphous titanium dioxide material is subjected to shallow surface doping treatment in a specific electrolyte and then is stabilized through an annealing process, so that the high-defect titanium dioxide material which is dark in color and contains a large number of oxygen defects is generated, and a sub-monolayer passivation layer is formed on the surface to protect Ti < 3 + >. According to the shallow surface doping method disclosed by the invention, the high-defect titanium dioxide material is successfully prepared under a low-temperature condition, and many challenges encountered in a traditional method are overcome. By means of the innovative method, rich oxygen defects can be effectively introduced into various forms of amorphous titanium dioxide, and meanwhile the structural stability of the material is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nano material preparation, and in particular to a method for protecting Ti by forming a sub-monolayer passivation layer through shallow surface doping. 3+ A method for preparing high-defect titanium dioxide materials. Background Art

[0002] Titanium dioxide (TiO2) is a semiconductor material with great value in many scientific and technological fields. It is widely used in photocatalysis, photovoltaic cells, electrolysis and gas sensors. This material is favored by researchers because of its good chemical stability, low toxicity, high dielectric constant and abundant resources. The performance and effect of TiO2 largely depend on its crystal structure, morphology and defect state. In particular, in some applications, TiO2 with high defect state shows higher activity.

[0003] Current research shows that the introduction of defects can significantly change the light absorption, electrical conductivity and catalytic activity of TiO2. Drawing on these new insights, we find that this new type of highly defective titanium dioxide material has broad application prospects in multiple fields. In the field of photocatalysis, this material is expected to achieve important breakthroughs in solar-driven water decomposition or organic decomposition due to its enhanced light absorption ability. In addition, it also shows potential advantages in other applications such as photovoltaic cells, electrolysis and gas sensing.

[0004] However, traditional methods of introducing defects in titanium dioxide, such as high-temperature heat treatment, ion implantation, or doping with other elements, face multiple challenges. High-temperature heat treatment may not only lead to a decrease in the stability of the material structure and undesirable concurrent reactions, but also increase the preparation cost. Although ion implantation can introduce defects, it may cause undesirable material damage, and it is difficult to accurately control the type and distribution of defects. In addition, doping with other elements may require the use of chemicals with environmental risks. In summary, although the existing technology can achieve the purpose of introducing defects, it may also lead to a decrease in the stability of the material structure, increase the preparation cost, and be easy to degrade or lose activity in practical applications. Therefore, it is particularly important to develop a new method to effectively introduce and stabilize high-defect TiO2 under low temperature conditions.

[0005] In summary, the development of this method of stabilizing high-defect titanium dioxide through shallow surface doping and its preparation technology is an urgent problem to be solved in the current scientific and technological field. Summary of the invention

[0006] The present invention aims to provide a method for protecting Ti by forming a sub-monolayer passivation layer through shallow surface doping. 3+ A method for preparing a high-defect titanium dioxide material by shallow surface doping to form a sub-monolayer passivation layer to protect Ti 3+To stabilize high-defect titanium dioxide materials. The method can effectively produce and stabilize high-defect TiO2 at low temperature and in a short time, maintain good material stability, and provide greater flexibility for different practical applications. In general, the purpose of the present invention is to improve the properties and performance of titanium dioxide materials through this innovative method, reduce preparation costs and environmental impact, and provide a high-defect titanium dioxide material with superior performance for the fields of photocatalysis, photovoltaic cells, electrolysis and gas sensing.

[0007] The technical solution of the present invention is as follows: a method for forming a sub-monolayer passivation layer to protect Ti by shallow surface doping 3+ A method for preparing a high-defect titanium dioxide material, wherein a sub-monolayer passivation layer is formed by shallow surface doping to protect Ti in the high-defect titanium dioxide material 3+ The high-defect titanium dioxide material is an amorphous titanium dioxide material. The amorphous titanium dioxide material is treated by shallow surface doping in a specific electrolyte and then stabilized by an annealing process, thereby producing a high-defect titanium dioxide material with a dark color and a large number of oxygen defects. A sub-monolayer passivation layer is formed on the surface of Ti 3+ For protection.

[0008] The specific electrolyte is an alkaline electrolyte.

[0009] The alkaline electrolyte contains 0.1M phosphate components, including phosphoric acid H3PO4 and phosphate electrolyte; the phosphate electrolyte is one or more of sodium dihydrogen phosphate NaH2PO4 and disodium hydrogen phosphate Na2HPO4; the mixed solution is adjusted to alkalinity by an alkaline solution, and the alkaline solution is KOH or NaOH.

[0010] Furthermore, the pH value of the electrolyte was adjusted to 7.2 to optimize the doping process and the formation of the passivation layer.

[0011] The amorphous titanium dioxide material includes amorphous titanium dioxide nanoparticles, nanotubes, nanowires, nanobelts, and nanosheets, collectively referred to as a-TiO2.

[0012] The shallow surface doping treatment is carried out in a three-electrode system, wherein a-TiO2 is used as a working electrode, a Pt sheet is used as a counter electrode, and Ag / AgCl is used as a reference electrode; at a constant current of 0.01-0.02Acm -2 Shallow surface doping is performed at a constant potential between -2.5V and -1.5V for 90-270 seconds.

[0013] The a-TiO2 is used as a working electrode as follows; when powdered a-TiO2 is selected, it is mixed with an ethanol-water solution to form a uniform slurry, and the electrode surface is thoroughly cleaned; after the slurry is applied, it is naturally dried at room temperature or subjected to temperature-controlled heat treatment; when flake a-TiO2 is selected, the flake a-TiO2 is sandwiched between platinum electrodes.

[0014] Furthermore, the volume ratio of the ethanol-water solution is water:ethanol=1:1.

[0015] The annealing conditions are as follows: the annealing is carried out in a high-purity nitrogen atmosphere, the annealing temperature reaches 420-470° C., the starting temperature is room temperature, the heating rate is 10° C. per minute, and the holding time is 1 hour.

[0016] Furthermore, the annealing conditions are: carrying out the annealing in a high-purity nitrogen atmosphere, the temperature reaching 450° C., the heating rate being 10° C. per minute, and the holding time being 1 hour.

[0017] The present invention proposes a new technology to stabilize high-defect titanium dioxide materials by forming a sub-monolayer passivation layer through shallow surface doping under low temperature conditions. Compared with traditional methods such as high-temperature heat treatment, ion implantation or element doping, this method can not only effectively introduce abundant oxygen defects, but also has lower preparation cost and higher material stability. The core of the present invention is to use specific phosphoric acid or phosphate electrolyte to shallowly surface dope amorphous titanium dioxide nanoparticles, nanotubes, nanowires, nanobelts and nanosheets and other materials in various forms, and then further stabilize the material structure through a precisely controlled annealing process. This high-defect titanium dioxide material is expected to exhibit superior performance in the fields of photocatalysis, photovoltaic cells, electrolysis and gas sensing.

[0018] The present invention adopts a shallow surface doping method, through low temperature and short time processing, combined with the formation of a sub-monolayer passivation layer, to achieve precise control of TiO2 defects and excellent material stability. Compared with traditional methods, this new method is not only lower in cost, but also shows greater flexibility in different practical applications.

[0019] Beneficial effects of the present invention: The shallow surface doping method of the present invention successfully realizes the preparation of high-defect titanium dioxide materials under low temperature conditions, overcoming many challenges encountered in traditional methods. Through this innovative method, rich oxygen defects can be effectively introduced into various forms of amorphous titanium dioxide while maintaining the structural stability of the material. This technology not only reduces the preparation cost, but also improves the environmental friendliness of material preparation, avoiding environmental pollution and material damage that may occur during high-temperature heat treatment or chemical doping. The careful selection of the electrolyte and the precise control of the annealing process further ensure the high quality and good performance of the material. In addition, the high-defect titanium dioxide material obtained in the present invention is expected to show significant performance advantages in multiple application fields. In particular, in the fields of photocatalysis, photovoltaic cells, electrolysis and gas sensing, this material is expected to achieve major breakthroughs due to its enhanced light absorption capacity and improved electrochemical activity. The development of this material not only provides a new type of high-efficiency material for related scientific and technological fields, but also brings new possibilities for future environmental protection and energy conversion technologies. In general, the present invention provides an efficient and environmentally friendly way to prepare and apply high-defect titanium dioxide materials, providing important support for research and development in related fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Highly defective TiO2 nanotubes stabilized by shallow surface doping to form a sub-monolayer passivation layer (left); ordinary TiO2 nanotubes annealed in air (right).

[0021] Figure 2 This is an EPR comparison chart of titanium dioxide that has been shallowly surface doped with phosphate (KH2PO4) to form a sub-monolayer passivation layer and has not been shallowly surface doped.

[0022] Figure 3 Solid UV comparison of TiO2 with a sub-monolayer passivation layer formed by shallow surface doping in an electrolyte containing phosphate and without shallow surface doping. DETAILED DESCRIPTION

[0023] Example 1

[0024] A method for protecting Ti by forming a sub-monolayer passivation layer through shallow surface doping 3+ The method for preparing a high-defect titanium dioxide material comprises the following specific steps:

[0025] Step 1: Material preparation:

[0026] Step 1.1: Select a-TiO2 amorphous titanium dioxide nanoparticles as the base material.

[0027] Step 2: Electrolyte preparation:

[0028] Step 2.1: Prepare a phosphoric acid electrolyte (H3PO4) containing 0.1 M phosphate component;

[0029] Step 2.2: Use 5 ml of 1 mol / L KOH to adjust the solution to alkalinity.

[0030] Step 3: Electrode preparation:

[0031] Step 3.1: Mixing powdered a-TiO2 nanoparticles with ethanol-water solution (ethanol: water = 1:1) to prepare a uniform slurry;

[0032] Step 3.2: Thoroughly clean the surface of the glassy carbon electrode to remove surface contaminants, clean it with ethanol or ionized water, and restore its smoothness by mechanical polishing;

[0033] Step 3.3: Apply the prepared slurry evenly on the surface of the glassy carbon electrode. After application, dry it naturally at room temperature or use temperature-controlled heat treatment.

[0034] Step 4: Shallow surface doping process:

[0035] Step 4.1: Perform shallow surface doping in a three-electrode system, setting a-TiO2 as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl as the reference electrode;

[0036] Step 4.2: Select a constant current of 0.017Acm -2 Doping was performed for 90 seconds.

[0037] Step 5: Annealing treatment:

[0038] Step 5.1: performing annealing treatment in a high-purity nitrogen atmosphere;

[0039] Step 5.2: Set the temperature to rise to 450°C at 10°C per minute and maintain for 1 hour.

[0040] The light absorption capacity and electrochemical activity of the high-defect titanium dioxide material prepared by the above steps are significantly improved. Specifically, solid UV image analysis shows that the sub-monolayer passivation layer formed by shallow surface doping can effectively protect the Ti 3+ The site causes the light absorption edge of the material to redshift to the visible light region, thereby significantly broadening the light absorption range and enhancing the light absorption capacity of the material. In addition, the resistance of the material surface is reduced and the photocurrent is significantly increased, further verifying the enhancement of electrochemical activity. These characteristics make the material have broad prospects in the field of optoelectronic applications.

[0041] Example 2

[0042] A method for protecting Ti by forming a sub-monolayer passivation layer through shallow surface doping 3+The method for preparing a high-defect titanium dioxide material comprises the following specific steps:

[0043] Step 1: Material preparation:

[0044] Step 1.1: Select a-TiO2 amorphous titanium dioxide nanotubes as the base material.

[0045] Step 2: Electrolyte preparation:

[0046] Step 2.1: Prepare a sodium dihydrogen phosphate (NaH2PO4) electrolyte containing 0.1 M phosphate component;

[0047] Step 2.2: Use 5 ml of 1 mol / L KOH to adjust the solution to alkalinity.

[0048] Step 3: Electrode preparation:

[0049] Step 3.1: Sandwich the sheet-like a-TiO2 nanotubes on a platinum clip as the working electrode.

[0050] Step 4: Shallow surface doping process:

[0051] Step 4.1: Perform shallow surface doping in a three-electrode system, setting a-TiO2 as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl as the reference electrode;

[0052] Step 4.2: Select a constant current of 0.017A cm -2 Doping was performed for 270 seconds;

[0053] Step 5: Annealing treatment:

[0054] Step 5.1: performing annealing treatment in a high-purity nitrogen atmosphere;

[0055] Step 5.2: Set the temperature to rise to 450°C at 10°C per minute and maintain for 1 hour.

[0056] The light absorption capacity and electrochemical activity of the high-defect titanium dioxide material prepared by the above steps are significantly improved. Specifically, solid UV image analysis shows that the sub-monolayer passivation layer formed by shallow surface doping can effectively protect the Ti 3+ The site causes the light absorption edge of the material to redshift to the visible light region, thereby significantly broadening the light absorption range and enhancing the light absorption capacity of the material. In addition, the resistance of the material surface is reduced and the photocurrent is significantly increased, further verifying the enhancement of electrochemical activity. These characteristics make the material have broad prospects in the field of optoelectronic applications.

[0057] Example 3

[0058] A method for protecting Ti by forming a sub-monolayer passivation layer through shallow surface doping3+ A method for preparing a high-defect titanium dioxide material, the specific steps comprising:

[0059] Step 1: Material preparation:

[0060] Step 1.1: Select a-TiO2 amorphous titanium dioxide nanowires as the base material.

[0061] Step 2: Electrolyte preparation:

[0062] Step 2.1: Prepare disodium hydrogen phosphate (Na2HPO4) containing 0.1 M phosphate component;

[0063] Step 2.2: Use 8 ml of 1 mol / L NaOH to adjust the solution to alkalinity.

[0064] Step 3: Electrode preparation:

[0065] Step 3.1: Mix the powdered a-TiO2 nanowires with an ethanol-water solution (ethanol: water = 1:1) to prepare a uniform slurry;

[0066] Step 3.2: Thoroughly clean the surface of the glassy carbon electrode to remove surface contaminants, clean it with ethanol or ionized water, and restore its smoothness by mechanical polishing;

[0067] Step 3.3: Apply the prepared slurry evenly on the surface of the glassy carbon electrode. After application, dry it naturally at room temperature or use temperature-controlled heat treatment.

[0068] Step 4: Shallow surface doping process:

[0069] Step 4.1: Perform shallow surface doping in a three-electrode system, setting a-TiO2 as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl as the reference electrode;

[0070] Step 4.2: Select a constant potential of -2.5 V for doping and a time of 270 seconds.

[0071] Step 5: Annealing treatment:

[0072] Step 5.1: performing annealing treatment in a high-purity nitrogen atmosphere;

[0073] Step 5.2: Set the temperature to rise to 450°C at 10°C per minute and maintain for 1 hour.

[0074] The light absorption capacity and electrochemical activity of the high-defect titanium dioxide material prepared by the above steps are significantly improved. Specifically, solid UV image analysis shows that the sub-monolayer passivation layer formed by shallow surface doping can effectively protect the Ti 3+The site causes the light absorption edge of the material to redshift to the visible light region, thereby significantly broadening the light absorption range and enhancing the light absorption capacity of the material. In addition, the resistance of the material surface is reduced and the photocurrent is significantly increased, further verifying the enhancement of electrochemical activity. These characteristics make the material have broad prospects in the field of optoelectronic applications.

[0075] Example 4

[0076] A method for protecting Ti by forming a sub-monolayer passivation layer through shallow surface doping 3+ A method for preparing a high-defect titanium dioxide material, the specific steps comprising:

[0077] Step 1: Material preparation:

[0078] Step 1.1: Select a-TiO2 amorphous titanium dioxide nanoribbons as the base material.

[0079] Step 2: Electrolyte preparation:

[0080] Step 2.1: Prepare disodium hydrogen phosphate (K2HPO4) containing 0.1 M phosphate component;

[0081] Step 2.2: Use 7 ml of 1 mol / L KOH to adjust the solution to alkalinity.

[0082] Step 3: Electrode preparation:

[0083] Step 3.1: Mix the powdered a-TiO2 nanobelts with an ethanol-water solution (ethanol: water = 1:1) to prepare a uniform slurry;

[0084] Step 3.2: Thoroughly clean the surface of the glassy carbon electrode to remove surface contaminants, clean it with ethanol or ionized water, and restore its smoothness by mechanical polishing;

[0085] Step 3.3: Apply the prepared slurry evenly on the surface of the glassy carbon electrode. After application, dry it naturally at room temperature or use temperature-controlled heat treatment.

[0086] Step 4: Shallow surface doping process:

[0087] Step 4.1: Perform shallow surface doping in a three-electrode system, setting a-TiO2 as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl as the reference electrode;

[0088] Step 4.2: Select a constant potential of -1.5 V for doping and the time is 270 seconds.

[0089] Step 5: Annealing treatment:

[0090] Step 5.1: performing annealing treatment in a high-purity nitrogen atmosphere;

[0091] Step 5.2: Set the temperature to rise to 450°C at 10°C per minute and maintain for 1 hour.

[0092] The light absorption capacity and electrochemical activity of the high-defect titanium dioxide material prepared by the above steps are significantly improved. Specifically, solid UV image analysis shows that the sub-monolayer passivation layer formed by shallow surface doping can effectively protect the Ti 3+ The site causes the light absorption edge of the material to redshift to the visible light region, thereby significantly broadening the light absorption range and enhancing the light absorption capacity of the material. In addition, the resistance of the material surface is reduced and the photocurrent is significantly increased, further verifying the enhancement of electrochemical activity. These characteristics make the material have broad prospects in the field of optoelectronic applications.

[0093] Comparative Example 1

[0094] Based on Example 1, the phosphoric acid electrolyte (H3PO4) in step 2.1 was replaced with a nitric acid electrolyte (HNO3), and the remaining steps were consistent with Example 1. Finally, it was found that amorphous titanium dioxide nanoparticles were easier to restore the original color, and the dark color did not last long.

[0095] The ordinary titanium dioxide nanomaterial prepared by the above steps does not form a sub-monolayer passivation layer, so its light absorption capacity and electrochemical activity are relatively weak. Specifically, through solid ultraviolet image analysis, it can be seen that the light absorption edge of the undoped ordinary titanium dioxide material has not been significantly red-shifted, the light absorption range has not been significantly widened, and the light absorption capacity has not been significantly enhanced. At the same time, the resistance of the material surface is high, the photocurrent is low, and the electrochemical activity is not significantly enhanced. These results show that the performance of titanium dioxide materials that have not formed a sub-monolayer passivation layer in optoelectronic applications is relatively limited.

[0096] Comparative Example 2

[0097] Based on Example 2, in step 2.2, the solution was not adjusted to alkalinity, and the remaining steps were consistent with Example 2. Finally, it was found that amorphous titanium dioxide nanotubes were easier to restore the original color, and the dark color did not last long.

[0098] The ordinary titanium dioxide nanomaterial prepared by the above steps does not form a sub-monolayer passivation layer, so its light absorption capacity and electrochemical activity are relatively weak. Specifically, through solid ultraviolet image analysis, it can be seen that the light absorption edge of the undoped ordinary titanium dioxide material has not been significantly red-shifted, the light absorption range has not been significantly widened, and the light absorption capacity has not been significantly enhanced. At the same time, the resistance of the material surface is high, the photocurrent is low, and the electrochemical activity is not significantly enhanced. These results show that the performance of titanium dioxide materials that have not formed a sub-monolayer passivation layer in optoelectronic applications is relatively limited.

[0099] Comparative Example 3

[0100] Based on Example 3, in step 5.1, the sample was not annealed in a high-purity nitrogen atmosphere, and the remaining steps were consistent with Example 3. Finally, it was found that amorphous titanium dioxide nanowires were easier to restore their original color, and the dark color did not last long.

[0101] The ordinary titanium dioxide nanomaterial prepared by the above steps does not form a sub-monolayer passivation layer, so its light absorption capacity and electrochemical activity are relatively weak. Specifically, through solid ultraviolet image analysis, it can be seen that the light absorption edge of the undoped ordinary titanium dioxide material has not been significantly red-shifted, the light absorption range has not been significantly widened, and the light absorption capacity has not been significantly enhanced. At the same time, the resistance of the material surface is high, the photocurrent is low, and the electrochemical activity is not significantly enhanced. These results show that the performance of titanium dioxide materials that have not formed a sub-monolayer passivation layer in optoelectronic applications is relatively limited.

Claims

1. A method of forming a sub-monolayer passivation layer to protect Ti by shallow surface doping 3+ A method for preparing a high-defect titanium dioxide material, characterized in that: Sub-monolayer passivation layer formed by shallow surface doping to protect Ti in high-defect titanium dioxide materials 3 + ; The high-defect titanium dioxide material is an amorphous titanium dioxide material. The amorphous titanium dioxide material is treated by shallow surface doping in a specific electrolyte and then stabilized by an annealing process, thereby producing a high-defect titanium dioxide material with a dark color and a large number of oxygen defects. A sub-monolayer passivation layer is formed on the surface to resist Ti 3+ For protection.

2. The preparation method according to claim 1, characterized in that: The specific electrolyte is an alkaline electrolyte.

3. The preparation method according to claim 2, characterized in that: The alkaline electrolyte contains 0.1M phosphate component, including phosphoric acid H3PO4 and phosphate electrolyte; the phosphate electrolyte is sodium dihydrogen phosphate NaH2PO4 and / or disodium hydrogen phosphate Na2HPO4; The mixed solution is adjusted to be alkaline by using an alkaline solution, wherein the alkaline solution is KOH or NaOH.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The amorphous titanium dioxide material includes amorphous titanium dioxide nanoparticles, nanotubes, nanowires, nanobelts, and nanosheets, collectively referred to as a-TiO2.

5. The preparation method according to claim 4, characterized in that: The shallow surface doping treatment is carried out in a three-electrode system, wherein a-TiO2 is used as a working electrode, a Pt sheet is used as a counter electrode, and Ag / AgCl is used as a reference electrode; at a constant current of 0.01-0.02A cm -2 Shallow surface doping is performed at a constant potential between -2.5V and -1.5V for 90-270 seconds.

6. The preparation method according to claim 5, characterized in that: The a-TiO2 is used as a working electrode as follows; when powdered a-TiO2 is selected, it is mixed with an ethanol-water solution to form a uniform slurry, and the electrode surface is thoroughly cleaned; the volume ratio of ethanol to water in the ethanol-water solution is 1:1; after the slurry is applied, it is naturally dried at room temperature or subjected to temperature-controlled heat treatment; when flake a-TiO2 is selected, the flake a-TiO2 is sandwiched between platinum electrodes.

7. The preparation method according to any one of claims 1, 2, 3, 5 or 6, characterized in that: The annealing conditions are as follows: the annealing is carried out in a high-purity nitrogen atmosphere, the annealing temperature reaches 420-470° C., the starting temperature is room temperature, the heating rate is 10° C. per minute, and the holding time is 1 hour.

8. The preparation method according to claim 4, characterized in that: The annealing conditions are as follows: the annealing is carried out in a high-purity nitrogen atmosphere, the annealing temperature reaches 420-470° C., the starting temperature is room temperature, the heating rate is 10° C. per minute, and the holding time is 1 hour.