Lithium tungstate and preparation method thereof
The preparation of lithium tungstate by the sol-gel method solves the problems of complex traditional methods and uneven particle size, achieving high purity, fine particle size and uniform distribution of lithium tungstate, improving its electrochemical performance in high-performance applications and catalytic performance.
Patent Information
- Application Number
- CN202410971003.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-08
AI Technical Summary
The traditional preparation method of lithium tungstate is complex and the product particle size is large and unevenly distributed, which limits its application in high-performance fields.
The sol-gel method is used to prepare high purity, fine particle size and uniformly distributed tungstic acid by mixing ammonium tungstate and lithium hydroxide solutions, adding polyvinyl alcohol, heating and dissolving, drying and calcining, and controlling the molar ratio and heating conditions. lithium.
The preparation process is simplified, the electrochemical performance and catalytic efficiency of lithium tungstate are improved, and its performance consistency and stability in lithium-ion batteries, photocatalysis and electrochromic devices are enhanced.
Smart Images

Figure CN118745003A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tungstates, and in particular relates to lithium tungstate and a preparation method thereof. Background Art
[0002] As an important inorganic material, lithium tungstate plays a key role in the development of contemporary science and technology. It is not only widely used in lithium-ion batteries, photocatalysis, electrochromic devices and other fields, but also shows great potential in other high-tech fields. These applications of lithium tungstate benefit from its unique physical and chemical properties, such as high stability, good electrochemical performance and excellent optical properties.
[0003] In the field of lithium-ion batteries, lithium tungstate, as a high-performance cathode material, is valued for its high energy density, good cycle stability and excellent safety performance. Especially in the field of electric vehicles and portable electronic devices, the requirements for battery performance are getting higher and higher. The emergence of lithium tungstate provides new possibilities for the advancement of battery technology.
[0004] In the field of photocatalysis, lithium tungstate is widely used as a highly efficient catalyst for environmental purification and energy conversion. For example, it can be used to decompose water to produce hydrogen, and it can also be used to degrade organic pollutants, thus providing new ideas for solving energy and environmental problems.
[0005] In the field of electrochromic devices, lithium tungstate is used in smart windows, information display and other fields due to its excellent electrochromic performance. Such devices can change their color according to the change of external voltage, and have the advantages of energy saving and environmental protection.
[0006] However, there are some problems with the traditional lithium tungstate preparation methods, such as high-temperature solid phase method and liquid phase method. These methods usually require complex process flows, and the resulting product has a large particle size and uneven particle size distribution. These problems limit the application of lithium tungstate in certain high-performance fields. Summary of the invention
[0007] The purpose of the present invention is to solve the above-mentioned shortcomings and provide a lithium tungstate and a preparation method thereof.
[0008] In the first aspect, a method for preparing lithium tungstate adopts the following technical scheme:
[0009] A method for preparing lithium tungstate, characterized in that it comprises the following steps:
[0010] The ammonium tungstate solution and the lithium hydroxide solution are mixed evenly, polyvinyl alcohol is added, and heated to dissolve to obtain a gel;
[0011] The gel is dried, calcined in an air atmosphere, and cooled to obtain lithium tungstate.
[0012] This method simplifies the preparation process of lithium tungstate by using the sol-gel method, reduces the number of operation steps, and makes the preparation process more efficient and convenient. The sol-gel method can produce high-purity lithium tungstate powder, which is crucial to improving the performance of the final application product, especially in high-tech fields such as lithium-ion batteries. This method can produce lithium tungstate particles with fine particle size and uniform distribution. The fine particle size and uniform particle size distribution help to increase the surface area of the material, thereby enhancing its electrochemical performance and catalytic efficiency. Due to the uniform particle size distribution, the lithium tungstate prepared using this method shows higher consistency in electrochemical performance and catalytic efficiency, which is particularly important for large-scale industrial production.
[0013] Furthermore, the molar ratio of ammonium tungstate to lithium hydroxide is 1:1.5 to 1:2.5.
[0014] By setting a specific molar ratio range, the ratio of reactants can be more finely controlled, the chemical reaction process can be optimized, and the performance of the product, such as electrochemical performance and catalytic efficiency, can be improved. The appropriate molar ratio helps to form a more ideal chemical structure, thereby improving the physical and chemical properties of lithium tungstate, such as improving its stability and cycle performance. The precise molar ratio helps to optimize the electrochemical properties of the material, especially in lithium-ion battery applications, which can improve the energy density, charge and discharge efficiency and cycle life of the battery. In photocatalytic applications, the appropriate molar ratio can enhance the catalytic activity of lithium tungstate and improve its efficiency in decomposing water to produce hydrogen or degrading organic pollutants. The appropriate molar ratio helps to form a uniform nucleus in the sol-gel process and promotes uniform growth of particles, thereby obtaining a more uniform particle size distribution. A fixed molar ratio helps to reduce batch-to-batch differences and improve the consistency and repeatability of the production process.
[0015] Furthermore, the added amount of the polyvinyl alcohol is 1.5wt% to 2.5wt% of the mixed solution of lithium tungstate and lithium hydroxide.
[0016] By precisely controlling the amount of polyvinyl alcohol added, the gel formation process can be optimized, thereby affecting the microstructure and performance of the final product. The appropriate amount of polyvinyl alcohol added helps to form a more uniform gel structure, thereby promoting the uniform growth of lithium tungstate particles and obtaining a more uniform particle size distribution. The right amount of polyvinyl alcohol can serve as an effective gelling agent to help remove impurities and improve the purity of the final product. The appropriate amount of polyvinyl alcohol added helps to improve the structural stability of the product, especially during high temperature treatment, reducing cracking and agglomeration of the product. Uniform particle size distribution and high purity help to improve the electrochemical properties of lithium tungstate, such as improving the energy density and cycle stability of the battery.
[0017] Furthermore, the heating and dissolving temperature is 50°C to 70°C.
[0018] Furthermore, the drying temperature is 50° C. to 80° C., and the drying time is 24 h to 30 h.
[0019] Furthermore, the calcination temperature is 550° C. to 650° C., and the calcination time is 3.5 h to 4.5 h.
[0020] Furthermore, the calcination heating rate is 75°C / h to 85°C / h.
[0021] In the second aspect, a lithium tungstate adopts the following technical solution:
[0022] A lithium tungstate is prepared by any of the above-mentioned methods for preparing lithium tungstate.
[0023] Furthermore, the lithium tungstate has a purity of >99.9wt% and a particle size of 100nm to 150nm.
[0024] Lithium tungstate with a purity greater than 99.9wt% has fewer impurities, which is critical for improving its performance in high-performance applications, such as lithium-ion batteries, photocatalysis, and electrochromic devices. Lithium tungstate particles with a particle size range of 100nm to 150nm have a large specific surface area, which helps to increase its contact area with the reactants and enhance its catalytic activity and electrochemical performance. In lithium-ion battery applications, fine and uniform particles can provide higher energy density, better charge and discharge performance, and longer cycle life. In photocatalytic applications, smaller particle size and larger specific surface area help improve catalytic efficiency and accelerate photocatalytic reactions, such as water hydrogen production or organic pollutant degradation. Fine particle size helps to improve the dispersibility of lithium tungstate in solvents or matrices, thereby enhancing its stability and performance consistency in the final product. Uniform particle size distribution helps to reduce performance differences between batches and improve the overall performance consistency of the product. Lithium tungstate with high purity and fine and uniform particle size is more suitable for high-performance and precision applications, such as high-end electronic devices and efficient energy conversion systems.
[0025] Beneficial effects of the present invention:
[0026] The present invention provides a method for preparing lithium tungstate. Compared with the traditional method for preparing lithium tungstate (such as high-temperature solid phase method and liquid phase method), the sol-gel method simplifies the preparation process, reduces the operation steps, and makes the entire preparation process more efficient and convenient; high-purity lithium tungstate powder and lithium tungstate particles with fine particle size and uniform distribution can be prepared by the sol-gel method. The fine particle size and uniform particle size distribution help to increase the surface area of the material, thereby enhancing its electrochemical performance and catalytic efficiency. Due to the uniform particle size distribution, the lithium tungstate prepared by this method shows higher consistency in electrochemical performance and catalytic efficiency, can provide higher energy density and better cycle stability in lithium-ion batteries, and can also show better performance in photocatalytic and electrochromic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a photo of the lithium tungstate morphology provided in Example 2. DETAILED DESCRIPTION
[0028] The following is a further specific description of a lithium tungstate and a preparation method thereof described in the present invention in conjunction with the examples. For the sake of simplicity of description, this document cannot list all the alternative technical features and implementation schemes contained in the present invention. Therefore, those skilled in the art should know that any technical features and implementation schemes in this embodiment do not limit the scope of protection of the present invention, which includes any alternative technical features and implementation schemes adopted by all those skilled in the art without creative labor. Specifically, the implementation schemes obtained by replacing any technical feature in the present invention or combining any two or more technical features provided by the present invention should be within the scope of protection of the present invention.
[0029] If no specific techniques and conditions are specified in the examples, the procedures are carried out according to the techniques and conditions described in the literature in the art or according to the product instructions. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0030] Example
[0031] Example 1
[0032] Embodiment 1 provides a method for preparing lithium tungstate, comprising the following steps:
[0033] The ammonium tungstate solution and the lithium hydroxide solution were mixed evenly at a molar ratio of 1:1.5, 1.5 wt% of polyvinyl alcohol was added, and the mixture was heated to 50° C. to dissolve to obtain a gel;
[0034] The gel was dried at 50° C. for 24 h, calcined in air atmosphere at a calcination temperature of 550° C. for 4.5 h, at a heating rate of 75° C. / h, and cooled to obtain lithium tungstate.
[0035] Example 2
[0036] Embodiment 2 provides a method for preparing lithium tungstate, comprising the following steps:
[0037] The ammonium tungstate solution and the lithium hydroxide solution were mixed evenly in a molar ratio of 1:2, 2 wt % of polyvinyl alcohol was added, and the mixture was heated to 60° C. to dissolve to obtain a gel;
[0038] The gel was dried at 70° C. for 28 h, calcined in air atmosphere at a calcination temperature of 600° C. for 4 h at a heating rate of 80° C. / h, and cooled to obtain lithium tungstate.
[0039] A morphology photo of lithium tungstate provided in Example 2 is shown in Figure 1 .
[0040] Example 3
[0041] Embodiment 3 provides a method for preparing lithium tungstate, comprising the following steps:
[0042] The ammonium tungstate solution and the lithium hydroxide solution were mixed evenly in a molar ratio of 1:2.5, 2.5 wt% of polyvinyl alcohol was added, and the mixture was heated to 70° C. to dissolve to obtain a gel;
[0043] The gel was dried at 80° C. for 24 h, calcined in air at a temperature of 650° C. for 3.5 h, at a heating rate of 85° C. / h, and cooled to obtain lithium tungstate.
[0044] Comparative Example
[0045] Comparative Example 1
[0046] Comparative Example 1 provides a method for preparing lithium tungstate, which differs from Example 2 in that the molar ratio of ammonium tungstate to lithium hydroxide is 1:3.
[0047] Comparative Example 2
[0048] Comparative Example 2 provides a method for preparing lithium tungstate, which differs from Example 2 in that the molar ratio of ammonium tungstate to lithium hydroxide is 1:1.
[0049] Comparative Example 3
[0050] Comparative Example 3 provides a method for preparing lithium tungstate, which differs from Example 2 in that the amount of polyvinyl alcohol added is 1 wt %.
[0051] Comparative Example 4
[0052] Comparative Example 4 provides a method for preparing lithium tungstate, which differs from Example 2 in that the amount of polyvinyl alcohol added is 3 wt %.
[0053] Comparative Example 5
[0054] Comparative Example 5 provides a method for preparing lithium tungstate, which differs from Example 2 in that the drying time is 20 hours.
[0055] Comparative Example 6
[0056] Comparative Example 6 provides a method for preparing lithium tungstate, which differs from Example 2 in that the calcination temperature is 500°C.
[0057] Comparative Example 7
[0058] Comparative Example 7 provides a method for preparing lithium tungstate, which differs from Example 2 in that the heating rate is 70°C / h.
[0059] Comparative Example 8
[0060] Comparative Example 8 provides a method for preparing lithium tungstate, which differs from Example 2 in that the heating rate is 90°C / h.
[0061] Indicator testing
[0062] The lithium tungstate prepared by the lithium tungstate preparation methods provided in Examples 1-3 and Comparative Examples 1-8 were tested for purity, particle size and bulk ratio, and the results are shown in Table 1.
[0063] Table 1
[0064]
[0065] It can be seen from Table 1 that (1) changing the molar ratio of ammonium tungstate and lithium hydroxide will lead to a decrease in the purity of the product lithium tungstate; (2) increasing or decreasing the amount of polyvinyl alcohol and insufficient calcination temperature will lead to a decrease in the purity of the product lithium tungstate and a larger particle size, and a lower bulk ratio; (3) insufficient drying time and a heating rate that is too slow or too fast will lead to a larger particle size of the lithium tungstate and a lower bulk ratio.
[0066] For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived from them are still within the scope of protection of the claims of the invention.
Claims
1. A method for preparing lithium tungstate, characterized in that: The following steps are involved: The ammonium tungstate solution and the lithium hydroxide solution are mixed evenly, polyvinyl alcohol is added, and heated to dissolve to obtain a gel; The gel is dried, calcined in an air atmosphere, and cooled to obtain lithium tungstate.
2. The method for preparing lithium tungstate according to claim 1, characterized in that: The molar ratio of ammonium tungstate to lithium hydroxide is 1:1.5 to 1:2.
5.
3. The method for preparing lithium tungstate according to claim 1, characterized in that: The amount of polyvinyl alcohol added is 1.5wt% to 2.5wt% of the mixed solution of lithium tungstate and lithium hydroxide.
4. The method for preparing lithium tungstate according to claim 1, characterized in that: The heating and dissolving temperature is 50℃~70℃.
5. The method for preparing lithium tungstate according to claim 1, characterized in that: The drying temperature is 50℃~80℃, and the drying time is 24h~30h.
6. The method for preparing lithium tungstate according to claim 1, characterized in that: The calcination temperature is 550°C to 650°C, and the calcination time is 3.5h to 4.5h.
7. The method for preparing lithium tungstate according to claim 1, characterized in that: The calcination heating rate is 75°C / h to 85°C / h.
8. A lithium tungstate, characterized in that: The lithium tungstate is prepared by the preparation method of the lithium tungstate according to any one of claims 1 to 7.
9. The lithium tungstate according to claim 8, characterized in that: The lithium tungstate has a purity of >99.9wt% and a particle size of 100nm to 150nm.