High-performance glass fiber component and manufacturing method thereof

By adding a trace amount of Bi2O3 in the manufacturing of high-strength glass fibers, the high-temperature viscosity of the glass is reduced and F is replaced, which solves the pollution problem caused by the volatilization of F, maintains the high-temperature viscosity and avoids harmful gases, and improves the strength and process safety of the glass fiber. .

CN118745079AInactive Publication Date: 2024-10-08HUANGSHI HONGHE ELECTRONIC MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410732396.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the manufacturing process of high-strength glass fiber, the F used will volatilize and pollute the atmosphere, causing harm to workers, and it is difficult to effectively reduce the high-temperature viscosity of glass with existing technology.

Method used

By adding a trace amount of Bi2O3, it forms a [BiO6] network outer body in the glass structure, reducing the high-temperature viscosity of the glass, replacing F, avoiding the generation of harmful gases, and optimizing the composition content and process flow of the glass fiber, including SiO2, Al2O3 , CaO, MgO, ZrO2, CeO2, Bi2O3, etc. proportions and process conditions to ensure the uniformity and drawing performance of the glass liquid.

Benefits of technology

It achieves the high-temperature viscosity of glass while avoiding harmful gas emissions, improves the strength and high-temperature resistance of glass fiber, reduces harmful pollution in the process, and ensures production safety and excellent performance of glass fiber.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-performance glass fiber component and a manufacturing method thereof. The high-performance glass fiber component comprises 55-63 wt% of SiO2; the content of Al2O3 is 23 to 26 weight percent; the content of CaO is 5-12 wt%; the content of MgO is 11.5 to 14.5 weight percent; the content of ZrO2 is 0.5 to 1.5 wt%; the content of Bi2O3 is 0.2 to 1.0 wt%; the content of CeO2 is 0.2-0.5 wt%, a trace amount of Bi2O3 is added and exists in a glass structure in the form of a [BiO6] network outer body, so that the network connection degree of the glass structure is reduced, the high-temperature viscosity of the glass is reduced, and harmful gas is not generated, and therefore, the trace amount of Bi2O3 is used for replacing F in the prior art, and the glass has the advantages of low cost and high efficiency. The high-temperature viscosity of the glass is ensured, and meanwhile, a large amount of harmful gas is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of high-performance glass fibers, and in particular to a high-performance glass fiber component and a method for manufacturing the same. Background Art

[0002] High-strength glass fiber is a glass fiber drawn from glass of the silicon-aluminum-magnesium-calcium system. Compared with alkali-free glass fiber, it has a series of excellent properties such as high tensile strength, high elastic modulus, good impact resistance, fatigue resistance and high temperature resistance.

[0003] In the prior art, in order to ensure the high-temperature viscosity of glass and facilitate molding operations, F is used in the production of high-strength glass fibers. In the actual production process, F volatilizes and pollutes the atmosphere, and at the same time causes harm to the health of workers. Summary of the invention

[0004] The embodiments of the present application provide a high-performance glass fiber component and a method for manufacturing the same, so as to solve the problem that F is required for the manufacture of high-strength glass fibers in the related art.

[0005] In a first aspect, a high-performance glass fiber component and a method for making the same are provided, comprising:

[0006] The SiO2 content is 55-63wt%; the Al2O3 content is 23-26wt%; the CaO content is 5-12wt%; the MgO content is 11.5-14.5wt%; the ZrO2 content is 0.5-1.5wt%; the Bi2O3 content is 0.2-1.0wt%; and the CeO2 content is 0.2-0.5wt%.

[0007] In some embodiments, the content of Al2O3 is 15-22wt%.

[0008] In some embodiments, the content of MgO is 5-10 wt %.

[0009] In some embodiments, the high performance glass fiber composition further contains BaO in an amount of 0.1-0.5 wt %.

[0010] In some embodiments, the high performance glass fiber composition further contains Y2O3 in an amount of 0.05-5 wt%.

[0011] In some embodiments, the high performance glass fiber composition further contains La2O3 in an amount of 0.05-3 wt%.

[0012] In some embodiments, the high performance glass fiber composition further contains Na2O and K2O, and the content of Na2O and K2O is 0-0.5 wt%.

[0013] Mixing: The high-performance glass fiber components are weighed and mixed to obtain a uniform mixture, wherein the mixture includes SiO2, Al2O3, CaO, MgO, ZrO2, Bi2O3, and CeO2;

[0014] Melting: The mixture is fed into the experimental kiln and melted at 1400-1500°C, clarified and homogenized for at least 6 hours to obtain a uniform, bubble-free glass liquid;

[0015] Wire drawing: The glass liquid is drawn through a platinum-rhodium alloy plate to obtain high-strength glass fiber.

[0016] In some embodiments, the mixture further comprises 0-0.5 wt % of Na2O and K2O and 0.1-0.5 wt % of BaO.

[0017] In some embodiments, the mixture further comprises 0.05-5wt% Y2O3 and 0.05-3wt% La2O3.

[0018] The embodiment of the present application provides a high-performance glass fiber component and a method for manufacturing the same. Since the present application adds a trace amount of Bi2O3, so that it exists in the glass structure in the form of a [BiO6] network exosome, the network connection degree of the glass structure is reduced, the high-temperature viscosity of the glass is reduced, and no harmful gases are generated. Therefore, a trace amount of Bi2O3 is used to replace F in the prior art, thereby ensuring the high-temperature viscosity of the glass while avoiding the generation of a large amount of harmful gases. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0020] The embodiments of the present application provide a high-performance glass fiber component and a method for manufacturing the same, which can solve the problem in the related art that F is required for the manufacture of high-strength glass fibers.

[0021] A high-performance glass fiber component and a method for making the same, comprising:

[0022] The SiO2 content is 55-63wt%; the Al2O3 content is 23-26wt%; the CaO content is 5-12wt%; the MgO content is 11.5-14.5wt%; the ZrO2 content is 0.5-1.5wt%; the Bi2O3 content is 0.2-1.0wt%; the CeO2 content is 0.2-0.5wt%;

[0023] SiO2 is the main component of silicate glass and plays the main skeleton role in the glass system; however, if the silica content is increased excessively, at the same melting temperature, the viscosity of the glass liquid will increase, the clarification temperature will increase, and the drawing performance will deteriorate;

[0024] Al2O3 is an intermediate oxide. Adding Al2O3 in the manufacture of silicate glass can improve the crystallization tendency of glass and enhance the chemical stability of glass. If the content of Al2O3 is too high, the liquidus line of glass will rise, the melting temperature of glass will be high, and the wire drawing will be difficult. If the content of Al2O3 is too low, it will be detrimental to the fiber strength and water resistance of glass.

[0025] CaO is a network exosome ion. Adding CaO in the manufacture of silicate glass can adjust the high-temperature viscosity of the glass and improve the water resistance of the silicate glass. However, if the CaO content is too high, the silicate glass material will become shorter, more brittle, and have an increased tendency to crystallize.

[0026] In the manufacture of silicate glass, MgO and CaO have similar functions, both of which can adjust the high-temperature viscosity of silicate glass and improve the water resistance of silicate glass. Replacing part of CaO with MgO can reduce the crystallization ability of silicate glass and adjust the material properties of silicate glass.

[0027] Adding ZrO2 in the manufacture of silicate glass can improve the strength of silicate glass, improve the viscosity, hardness, chemical stability of silicate glass, improve the water resistance, acid and alkali resistance of silicate glass, and reduce the thermal expansion coefficient of silicate glass. If too much ZrO2 is added, it will cause aggregation in the silicate glass, causing crystallization and phase separation of the silicate glass, and excessively increase the viscosity of the silicate glass liquid;

[0028] Adding a small amount of bismuth oxide in the manufacture of silicate glass can greatly reduce the viscosity of silicate glass, and it has a high degree of fluxing ability, which is also beneficial to improve the melting quality of silicate glass and obtain a lower bubble index; but if too much is introduced in the manufacture of silicate glass, the ion radius will become larger, it will be easy to polarize, and the network structure of the silicate glass will be destroyed;

[0029] Adding CeO2 in the manufacture of silicate glass can reduce the high-temperature viscosity of the glass. When the glass is melted at high temperature, O2 is released, which can play a good clarification role. Since CeO2 provides free oxygen under high temperature conditions, adding CeO2 to the glass component can increase the bridging oxygen in the glass network structure, making the connection between silicon-oxygen tetrahedrons tighter, and improving the mechanical properties and acid and alkali resistance of the fiber. However, too high a content will cause bubbles, so the content is controlled at 0.2-0.5wt%;

[0030] After testing, the silicon dioxide content was controlled at 55-62wt%, the Al2O3 content was controlled at 15-22wt%, the MgO content was controlled at 5-12wt%, the ZrO2 content was controlled at 0.5-1.5wt%, the Bi2O3 content was controlled at 0.2-1.0wt%, and the Al2O3 content was 15-22wt%.

[0031] The content of MgO is 5-10wt%;

[0032] If excessive MgO is added during the manufacture of silicate glass, the chemical stability of the silicate glass will be reduced, so its content needs to be controlled within 5-10 wt%.

[0033] The high-performance glass fiber composition further contains BaO, the content of which is 0.1 to 0.5 wt %;

[0034] BaO is a network exosome ion. Adding BaO in the manufacture of silicate glass can play a fluxing role, reduce the viscosity of glass during formation, improve the material properties of glass, make the glass easier to melt, and improve the wire drawing performance. At the same time, due to the corrosiveness of BaO to refractory materials, in the actual manufacture of silicate glass, the BaO content should not be too high and should be controlled at 0.1-0.5wt%.

[0035] The high-performance glass fiber composition further contains Y2O3, the content of which is 0.05-5wt%, and the high-performance glass fiber composition further contains La2O3, the content of which is 0.05-3wt%;

[0036] Rare earth oxides Y2O3 and La2O3 as well as Sm2O3 and Gd2O3 can also be selectively introduced. 3+ and La 3+ The coordination state, ionic radius, ionic field strength and Sm 3+ and Gd 3+ There are some differences. When used in combination with each other, on the one hand, it can provide richer extra-network ion coordination structure, which is beneficial to improve the stability of the glass structure; on the other hand, the hexacoordination structure of yttrium ions combined with the octacoordination structure of other ions can further enhance the integrity of the glass structure and improve the glass performance; on the third hand, when the temperature is lowered, the probability of each ion producing a regular arrangement will also decrease, which is beneficial to reduce the growth rate of the crystal, thereby further improving the glass's anti-crystallization ability.

[0037] The high-performance glass fiber composition further contains Na2O and K2O, wherein the content of Na2O and K2O is 0-0.5wt%;

[0038] Na2O and K2O are fluxing agents. Adding Na2O and K2O in the manufacture of silicate glass can reduce the viscosity of the glass. In order to prevent the increase of free oxygen, the decrease of bridging oxygen ions, the loose structure, the increase of network voids, and the decrease of fiber strength, it is necessary to control the dosage of Na2O and K2O, preferably within 0-0.5wt%.

[0039] Mixing: The high-performance glass fiber components are weighed and mixed to obtain a uniform mixture, wherein the mixture includes SiO2, Al2O3, CaO, MgO, ZrO2, Bi2O3, and CeO2;

[0040] Melting: The mixture is fed into the experimental kiln and melted at 1400-1500°C, clarified and homogenized for at least 6 hours to obtain a uniform, bubble-free glass liquid;

[0041] Wire drawing: The glass liquid is drawn through a platinum-rhodium alloy bushing to obtain high-strength glass fiber;

[0042] The mixture also includes 0-0.5 wt% of Na2O and K2O and 0.1-0.5 wt% of BaO;

[0043] The mixture also includes 0.05-5wt% Y2O3 and 0.05-3wt% La2O3;

[0044] SiO2 is introduced from silica sand, Al2O3 is introduced from kaolin, CaO is mainly introduced from limestone, MgO is introduced from dolomite, Bi2O3 and ZrO2 are introduced from their respective oxides, CeO2 is introduced from its oxide, Na2O is introduced from NaCl, K2O is introduced from potassium carbonate, and BaO is introduced from barium sulfate;

[0045] First, use a ball mill to mix the mixture evenly, take a small part of the mixture and put it into a platinum crucible and keep it at 1500-1520℃ for 5h to obtain a uniform, bubble-free glass liquid; pour the glass liquid into a pre-prepared graphite grinder, anneal it in a high-temperature furnace, grind the prepared glass sheet into a φ6mm*25mm disc, and measure the thermal expansion coefficient. After the thermal expansion coefficient measurement is completed, use a screw feeder to feed the remaining mixture into the experimental kiln for melt drawing; collect glass beads for bubble detection, and record the wire breakage rate and operation efficiency to evaluate the wire drawing performance.

[0046] In the description of the present application, it should be noted that the terms "upper", "lower", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. Unless otherwise expressly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present application can be understood according to the specific circumstances.

[0047] It should be noted that, in this application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0048] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A high performance glass fiber component, characterized in that: The raw materials include the following components: The SiO2 content is 55-63wt%; the Al2O3 content is 23-26wt%; the CaO content is 5-12wt%; the MgO content is 11.5-14.5wt%; the ZrO2 content is 0.5-1.5wt%; the Bi2O3 content is 0.2-1.0wt%; and the CeO2 content is 0.2-0.5wt%.

2. The high performance glass fiber component according to claim 1, characterized in that: The raw materials include the following components: The content of Al2O3 is 15-22wt%.

3. The high performance glass fiber component according to claim 1, characterized in that: The content of MgO is 5-10wt%.

4. The high performance glass fiber component according to claim 1, characterized in that: The high-performance glass fiber composition further contains BaO in an amount of 0.1 to 0.5 wt %.

5. The high performance glass fiber component according to claim 1, characterized in that: The high performance glass fiber composition further contains Y2O3 in an amount of 0.05-5 wt%.

6. The high performance glass fiber component according to claim 1, characterized in that: The high-performance glass fiber composition further contains La2O3 in an amount of 0.05-3 wt%.

7. The high performance glass fiber component according to claim 1, characterized in that: The high-performance glass fiber composition further contains Na2O and K2O, and the contents of the Na2O and K2O are 0-0.5 wt %.

8. A method for producing high-performance glass fiber, characterized in that: include: Used to manufacture the high-performance glass fiber according to any one of claims 1 to 7; Mixing: The high-performance glass fiber components are weighed and mixed to obtain a uniform mixture, wherein the mixture includes SiO2, Al2O3, CaO, MgO, ZrO2, Bi2O3, and CeO2; Melting: The mixture is fed into the experimental kiln and melted at 1400-1500°C, clarified and homogenized for at least 6 hours to obtain a uniform, bubble-free glass liquid; Wire drawing: The glass liquid is drawn through a platinum-rhodium alloy filter plate to obtain high-strength glass fiber.

9. The method for producing high-performance glass fiber according to claim 8, characterized in that: The mixture further comprises 0-0.5 wt % of Na2O and K2O and 0.1-0.5 wt % of BaO.

10. The method for producing high-performance glass fiber according to claim 8, wherein: The mixture also includes 0.05-5 wt % of Y2O3 and 0.05-3 wt % of La2O3.

Citation Information

Cited By

  • Glass fiber with low thermal expansion coefficient and preparation method thereof

    CN122187375A