High-temperature sintered high-silicon micro-expansion aluminoferrite solid waste-based cementing material and preparation method thereof

Through high-temperature sintering process and raw material combination, high silicon micro-expansion ferroaluminate solid waste-based cementitious material is formed, which solves the problems of poor corrosion resistance and high cost of ferroaluminate cement in marine engineering, and realizes the material's The rapid setting, rapid hardening and late strength increase steadily, meeting the durability requirements of marine engineering and realizing the reuse of resources.

CN118745086APending Publication Date: 2024-10-08OCEAN UNIV OF CHINA

Patent Information

Application Number
CN202410166155.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing ferroaluminate cement has poor corrosion resistance in marine engineering, high raw material quality and cost, improper control of temperature and oxygen content during the firing process, and unreasonable particle size selection, resulting in early concentration of hydration heat and poor mechanical properties in the later stage. Stablize.

Method used

It uses high-temperature sintered high-silicon micro-expanded ferroaluminate solid waste-based cementitious materials, and combines phosphogypsum, diatomaceous earth, iron tailings, red mud, bauxite and other raw materials through three heating, heat preservation, and oxygen control processes. Control the particle size distribution and chemical composition to form more C2S and C4AF minerals to achieve rapid setting, rapid hardening, high early strength and stable growth in later strength.

Benefits of technology

It improves the corrosion resistance and later strength stability of the material, reduces energy consumption, meets the durability requirements of marine engineering, and realizes the reuse of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745086A_ABST
    Figure CN118745086A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature sintered high-silicon micro-expansion aluminoferrite solid waste-based cementing material and a preparation method thereof. The raw materials comprise 40-44 parts of phosphogypsum, 10-13 parts of diatomite, 10-14 parts of iron tailings, 3-6 parts of red mud, 2-8 parts of bauxite, 14-18 parts of aluminum ore waste rock, 8-10 parts of fly ash I, 2-4 parts of fly ash II, 6-8 parts of gypsum, 4-6 parts of carbonized steel slag, and 4-6 parts of basalt fiber. The particle size range of the material is as follows: 20-30 [mu] m of phosphogypsum, 10-20 [mu] m of diatomite, 60-80 [mu] m of iron tailings, 30-40 [mu] m of red mud, 20-30 [mu] m of bauxite, 50-55 [mu] m of aluminum ore waste rock I, 0-8 [mu] m of fly ash I, 12-18 [mu] m of fly ash I, 6-12 [mu] m of gypsum and 0-3 [mu] m of carbonized steel slag. The high-temperature sintering process comprises three times of heating, heat preservation and oxygen control, the temperature is increased to 480-500 DEG C, 760-820 DEG C and 1300-1330 DEG C respectively, heat preservation is conducted for 20 min, 10 min and 50 min respectively, the oxygen content is controlled to be 21-23%, 28-30% and 24-26% respectively, and C2S is controlled to be larger than or equal to 40% when the materials are sintered. The prepared high-silicon micro-expansion aluminoferrite solid waste-based cementing material has the advantages of quick setting, quick hardening, high early strength, micro-expansion, continuously increased later strength, corrosion resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention of this article relates to the field of special solid waste-based cementitious materials, in particular to a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material and a preparation method thereof. Background Art

[0002] The hydration products of traditional silicate cement are mainly tricalcium silicate, dicalcium silicate, tricalcium aluminate and tetracalcium aluminoferrite, which are easily corroded and damaged by seawater, and it is difficult to ensure the durability of marine engineering. Although the addition of modifiers can improve the durability of traditional silicate cement, the effect is not obvious and the cost is relatively high.

[0003] Ferroaluminate cement is a new type of cement independently invented by my country based on the five-element system of CaO-SiO2-Al2O3-Fe2O3-SO3. It is a recognized typical cement series after silicate cement and aluminate cement. At present, the main product of the ferroaluminate cement industry is ferroaluminate cement. Ferroaluminate cement has the characteristics of fast hardening, high strength, high frost resistance, and low negative temperature construction. It is widely used in marine engineering, construction engineering, bridge construction and other fields, and has very good development prospects. However, ordinary ferroaluminate cement has high requirements on raw material performance and high cost, and it is difficult to meet the use needs of general marine engineering.

[0004] As the scale and difficulty of marine engineering construction continue to increase, whether it is possible to develop marine cementitious materials with good durability has become a restricting factor for the large-scale construction of marine engineering in my country. The cementitious materials used in marine engineering mainly improve their erosion resistance by fine aggregate effect or reducing calcium content, which fails to fundamentally solve the problem of poor erosion resistance of materials.

[0005] Problems in existing patented technologies for ferroaluminate cement-based materials:

[0006] 1. In the current existing patent technologies, high-quality clay is usually used to burn ferroaluminate cement, which has high requirements on material quality and type, is difficult to source, has high requirements on raw materials for production, and restricts the scope of use of raw materials. These problems have not yet been solved.

[0007] 2. In the existing patented technology, compared with sulphoaluminate cement, the C4AF content in ferroaluminate cement increases very little, and the other components are basically the same. Therefore, there are risks such as early hydration heat concentration, lack of development of mechanical properties in the later stage, or even shrinkage.

[0008] 3. In the current existing patent technology, for firing high-silicon ferroaluminate cement clinker, it is not possible to find a suitable condition such as temperature and oxygen content during the firing process.

[0009] 4. In the current patents for sintered ferroaluminate solid waste-based cementitious materials, there is little attention paid to the selection of particle size. There are rarely any specific particle size ranges for the selection of raw materials, which cannot fully exert their activity. Summary of the invention

[0010] In response to the problems caused by the above situation, the present application provides a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material and a preparation method. The components include by weight: ① 30-34 parts of phosphogypsum; ② 10-13 parts of diatomaceous earth; ③ 10-14 parts of iron tailings; ④ 3-6 parts of red mud; ⑤ 6-8 parts of bauxite; ⑥ 14-18 parts of aluminum ore waste rock; ⑦ 8-10 parts of fly ash I and 2-4 parts of fly ash II; ⑧ 6-8 parts of gypsum; ⑨ 4-6 parts of carbonized steel slag; ⑩ 4-6 parts of basalt fiber; some of the raw materials are dried. , crushing, grinding and screening steps, the particle size distribution range of each material is: phosphogypsum 20-30μm, diatomaceous earth 10-20μm, iron tailings 60-80μm, red mud 30-40μm, bauxite 20-30μm, aluminum ore waste 50-55μm, fly ash I 0-8μm, fly ash I 12-18μm, gypsum 6-12μm, carbonized steel slag 0-3μm. In this application, the sintering process is improved, and three heating, heat preservation and oxygen control are adopted to obtain the high-silicon micro-expansion ferroaluminate solid waste-based cementitious material with the advantages of fast setting, fast hardening, high early strength, micro-expansion, continuous and stable growth of late strength, corrosion resistance, etc.

[0011] To achieve the above object, the technical solution adopted in the present invention is as follows:

[0012] (1) washing phosphogypsum, iron tailings, diatomaceous earth, bauxite, and aluminum ore waste rock to remove surface impurities;

[0013] (2) placing the washed product and red mud in an oven and drying them at 80-100° C. until the weight remains constant;

[0014] (3) crushing phosphogypsum, diatomaceous earth, iron tailings, bauxite, aluminum ore waste rock, and red mud respectively, and then ball-milling them to a maximum particle size of less than 120 μm, weighing the required number of portions according to the ratio, mixing them, and setting aside;

[0015] (4) ultrafine grinding the product of (3) and other raw materials, phosphogypsum 20-30 μm, diatomaceous earth 10-20 μm, iron tailings 60-80 μm, red mud 30-40 μm, bauxite 20-30 μm, aluminum ore waste rock 50-55 μm, fly ash I 0-8 μm, fly ash I 12-18 μm, gypsum 6-12 μm, carbonized steel slag 0-3 μm;

[0016] (5) preheating phosphogypsum, diatomaceous earth, iron tailings, red mud, bauxite, and aluminum ore waste rock to maintain the internal temperature at 480-500° C. and control the internal oxygen content at 21-23% for 20 minutes;

[0017] (6) oxygenating the interior of the calcining furnace, controlling the internal oxygen content at 28-30%, heating the temperature to 780-820° C. at 10° C. / min, and keeping the temperature for 10 min to carry out oxidation reaction;

[0018] (7) controlling the oxygen content in the calcining furnace to 21-23%, raising the temperature to 1300-1330° C. at a rate of 5° C. / min, and calcining for 50 min;

[0019] (8) After calcination, the mixture is naturally cooled and ultrafine ground to obtain a clinker particle size of 0-8 μm and 10-18 μm, with a mass ratio of 1.2:1;

[0020] (9) Mix cement clinker, fly ash I, fly ash II, gypsum, and carbonized steel slag, put them into a mixer, and stir them at a speed of 200-240 r / min for 15 min;

[0021] (10) Basalt fiber is added and stirred at a speed of 100-120 r / min for 10 min to obtain a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material.

[0022] This patent is mainly divided into three stages in the high temperature sintering process:

[0023] (1) First, heat to 480-500°C, control the internal oxygen content at 21-23%, and continue for 20 minutes to remove the crystal water in the raw material.

[0024] (2) Continue heating to 760-820°C, control the internal oxygen content at 28-30%, and keep warm for 10 minutes to promote the oxidation reaction of the raw material and prepare for the subsequent solid phase reaction.

[0025] (3) Finally, the temperature is heated to 1300-1330°C, and the internal oxygen content is controlled at 21-23% for 50 minutes to promote solid phase reaction, which can combine the raw materials to generate more C2S and C4AF minerals.

[0026] When preparing high-temperature sintered high-silicon slightly expanded ferroaluminate solid waste-based materials, all raw materials are uniformly ground to pass through a 170-mesh sieve to ensure that the raw materials are small and uniform in fineness.

[0027] Preferably, the phosphogypsum described herein refers to the solid waste residue generated when phosphate ore is treated with sulfuric acid during the phosphoric acid production process, and its main component is dihydrate gypsum, which can replace natural gypsum as a raw material for preparing ferroaluminate cement.

[0028] Preferably, diatomite is a siliceous rock, a biogenic siliceous sedimentary rock, which is mainly composed of the remains of ancient diatoms. Its chemical composition is mainly SiO2, which can be expressed as SiO2·nH2O, and contains a small amount of Al2O3, Fe2O3, CaO, MgO, etc. and organic matter.

[0029] Preferably, the iron tailings refer to the waste residue discharged after the useful target components are extracted in the gold ore selection operation, which mainly contains oxides of calcium, iron, aluminum, magnesium, silicon and a small amount of precious metals and heavy metals. The components include 14-17%wt Al2O3, 48-63%wt SiO2, 12-17%wt Fe2O3 and a small amount of CaO.

[0030] Preferably, the red mud is sintered red mud, which refers to the solid waste generated when producing alumina by the sintering process, and the particle size powder is obtained after preliminary grinding, drying and screening.

[0031] Furthermore, the red mud powder used has a high content of Fe2O3, which makes the relative content of Fe in the raw material higher, and can replace part of Al with Fe to generate tetracalcium aluminoferrate, which is used to replace part of anhydrous calcium sulphoaluminate, and can also make the cement have early strength and high strength properties.

[0032] Preferably, bauxite is also called bauxite or bauxite, the main component of which is aluminum oxide, which is hydrated aluminum oxide containing impurities and is a soil-like mineral. It is a general term for a variety of hydrated aluminum oxide ores with very different geological sources.

[0033] Preferably, the main minerals in the aluminum ore waste are quartz, hematite and kaolinite, wherein the Fe2O3 content is >20%.

[0034] Preferably, fly ash is fine ash collected from the flue gas after coal combustion, and is the main solid waste discharged from coal-fired power plants. The main oxide components are: SiO2, Al2O3, FeO, Fe2O3, CaO, TiO2, etc.

[0035] Preferably, gypsum is a monoclinic mineral, which is a hydrate whose main chemical component is calcium sulfate (CaSO4), and the theoretical composition is CaO 32.6%, SO3 46.5%, and H2O 20.9%.

[0036] Preferably, the carbonized steel slag refers to solid waste slag produced during the smelting of pig iron and cured in a carbonized environment.

[0037] Preferably, the basalt fiber is a continuous fiber drawn from natural basalt, which is a continuous fiber drawn at high speed through a platinum-rhodium alloy drawing plate after the basalt material is melted at 1450-1500°C.

[0038] Furthermore, basalt fiber is a new type of inorganic environmentally friendly green high-performance fiber material, which is composed of oxides such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, iron oxide and titanium dioxide.

[0039] In an embodiment of the present invention, the clinker chemical composition of the high-temperature sintered high-silicon slightly expansive ferroaluminate cement includes: 42-48 parts of CaO, 14-20 parts of SiO2, 16-24 parts of Al2O3, 5-13 parts of Fe2O3, and 3-7 parts of SO3.

[0040] In an embodiment of the present invention, the high silicon micro-expansive ferroaluminate cement clinker comprises 20-35 parts, C2S40-55 parts, C4AF15-35 parts.

[0041] In some embodiments of the present invention, the particle size of each raw material is small, the specific surface area is large, the preparation process is rapid, and the energy consumption can be greatly reduced.

[0042] The beneficial effects of the present invention are:

[0043] 1. The traditional ferroaluminate cement clinker minerals are mainly C4A3S, C4AF and C2S. The iron phase and silicate phase in the clinker are controlled at a relatively low level, and the C2S content is only less than 30%. Therefore, there are problems such as concentrated hydration heat in the early stage, poor development of mechanical properties in the later stage, and even shrinkage. In this patent, raw materials with low Al content and high Fe content are selected. During the high-temperature sintering process, CaO, Fe2O3, Al2O3, CaSO4, etc. in the raw materials are decomposed and combined after dehydration to form new and more cementitious minerals C2S and C4AF. While ensuring that the clinker has the characteristics of early strength, rapid strength, corrosion resistance, etc., it also has a higher and steadily increasing later strength.

[0044] 2. Traditionally, a large amount of limestone, clay, and iron ore are needed to burn ferroaluminate cement clinker, and high requirements are placed on raw materials. Therefore, the present invention focuses on the use of industrial solid waste when selecting raw materials, and selects phosphogypsum to mainly provide Ca elements, diatomaceous earth to mainly provide Si elements, iron tailings and aluminum ore waste rock to provide the required Fe elements, and red mud and bauxite to provide Al elements. The Si content in the selected solid waste is higher than that in burning ordinary ferroaluminate cement, and more C2S and C4AF cementitious minerals can be produced, ensuring the stable growth of the strength in the later stage, and can well realize resource recycling. In addition, in the preparation of high-silicon micro-expansion ferroaluminate solid waste-based cementitious materials, the ratio of SO3 provided by gypsum to SO3 required for the hydration reaction of ferroaluminate cement clinker to form calcium sulfonate is between 1-2, so that the ferroaluminate solid waste-based cementitious materials have better expansion properties.

[0045] 3. The present invention adopts a high-temperature sintering method to burn. After the raw materials are dried, they are fired into high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious materials. During the firing process, heating, insulation, and oxygen control are performed three times. First, the oxygen content is controlled at 21-23%, and the material is heated to 480-500°C and kept warm for 20 minutes to remove the crystal water and interlayer water in the raw materials. The oxygen content is controlled at 28-30%, and the material is heated to 760-820°C and kept warm for 10 minutes to allow the carbonates in the raw materials to fully react in a high-oxygen environment to generate oxidation products, in preparation for subsequent solid-phase reactions. Finally, the oxygen content is controlled at 24-26%, the temperature is heated to 1300-1330°C, and the temperature is kept warm for 50 minutes. In a high-temperature and high-oxygen environment, it is beneficial to promote the synthesis and conversion of calcium ions, sulfur ions, aluminum ions, etc. in the raw materials into C4AF and C2S, and it can control formation.

[0046] 4. This patent grinds the raw materials ultrafinely before sintering to control the particle size of the raw materials to be small, so that they can react in a short time during the firing process, and can produce more C2S and C4AF cementitious minerals while saving energy. In addition, when configuring high-silicon micro-expanded ferroaluminate solid waste-based cementitious materials, the clinker, fly ash, gypsum, and carbonized steel slag are ground and optimized. The ferroaluminate cement clinker is 0-8μm and 10-18μm, the fly ash is 0-8μm and 12-18μm, the carbonized steel slag is 0-3μm, and the gypsum is 6-12μm. This can ensure that the water demand and hydration rate of the material during the hydration process are relatively moderate, with high 3d and 28d activity indexes and strength, and suitable setting time. In addition, the ferroaluminate cement clinker and fly ash are divided into two groups with different particle sizes and qualities, and matched with gypsum and carbonized steel slag with different particle sizes, which is beneficial to improving the packing density of the slurry, reducing the initial porosity of the cement slurry, and improving the liquid strength of the slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The present invention is a method for preparing a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material DETAILED DESCRIPTION

[0048] The following implementation cases will clearly and completely demonstrate the concept, purpose, technical solution and effects of the present invention. The following embodiments and drawings will help to fully understand the purpose, features and effects of the present invention. Obviously, the implementation cases described are only some examples of the present invention, which are representative and can serve as a certain illustration of the present application.

[0049] Example 1: High-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material used for grouting

[0050] 1. Prepare raw materials: 40 parts of phosphogypsum, 11 parts of diatomaceous earth, 12 parts of iron tailings, 3 parts of red mud, 6 parts of bauxite, 16 parts of aluminum ore waste rock, 12 parts of fly ash, 7 parts of gypsum, 5 parts of carbonized steel slag, 4 parts of basalt fiber, and 80 parts of water.

[0051] 2. Production steps

[0052] (1) Wash phosphogypsum, iron ore tailings, diatomaceous earth, bauxite, and aluminum ore waste rock with water to remove surface impurities.

[0053] (2) The washed product and red mud are placed in an oven and dried at 80-100° C. until the weight remains constant.

[0054] (3) Phosphogypsum, diatomaceous earth, iron tailings, bauxite, aluminum ore waste rock, and red mud are crushed separately, and then ball-milled to a maximum particle size of less than 120 μm. The required number of portions is weighed and mixed according to the ratio for later use.

[0055] (4) The product of (3) and other raw materials are ultra-finely ground, including phosphogypsum 20-30 μm, diatomaceous earth 10-20 μm, iron tailings 60-80 μm, red mud 30-40 μm, bauxite 20-30 μm, aluminum ore waste rock I 50-55 μm, fly ash I 0-8 μm, fly ash I 12-18 μm, gypsum 6-12 μm, and carbonized steel slag 0-3 μm.

[0056] (5) Preheating the phosphogypsum, diatomaceous earth, iron tailings, red mud, bauxite, and aluminum ore waste rock to maintain the internal temperature at 480-500° C. and control the internal oxygen content at 21-23% for 20 minutes.

[0057] (6) The calcining furnace is filled with oxygen to control the internal oxygen content at 28-30%, and the temperature is heated to 780-820° C. at 10° C. / min. The temperature is kept for 10 minutes to carry out an oxidation reaction.

[0058] (7) The oxygen content in the calcining furnace was controlled at 24-26%, the temperature was increased to 1300-1330°C at a rate of 5°C / min, and calcined for 50 minutes.

[0059] (8) After calcination, the mixture is naturally cooled and ultrafine ground to obtain a clinker particle size of 0-8 μm and 10-18 μm, with a mass ratio of 1.2:1.

[0060] (9) Cement clinker, fly ash I, fly ash II, gypsum, and carbonized steel slag are mixed, put into a mixer, water is added, and stirred at a speed of 200-240 r / min for 15 min.

[0061] (10) Basalt fiber is added and stirred at a rotation speed of 100-120 r / min for 10 min to obtain a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based grouting material.

[0062] Example 2: High temperature sintered high silicon micro-expansion ferroaluminate solid waste based cementitious material used for grouting

[0063] 1. Prepare raw materials: 42 parts of phosphogypsum, 12 parts of diatomaceous earth, 12 parts of iron tailings, 4 parts of red mud, 8 parts of bauxite, 15 parts of aluminum ore waste rock, 14 parts of fly ash, 7 parts of gypsum, 6 parts of carbonized steel slag, 5 parts of basalt fiber, and 85 parts of water.

[0064] 2. Production steps

[0065] (1) Wash phosphogypsum, iron ore tailings, diatomaceous earth, bauxite, and aluminum ore waste rock with water to remove surface impurities.

[0066] (2) The washed product and red mud are placed in an oven and dried at 80-100° C. until the weight remains constant.

[0067] (3) Phosphogypsum, diatomaceous earth, iron tailings, bauxite, aluminum ore waste rock, and red mud are crushed separately, and then ball-milled to a maximum particle size of less than 120 μm. The required number of portions is weighed and mixed according to the ratio for later use.

[0068] (4) The product of (3) and other raw materials are ultra-finely ground, including phosphogypsum 20-30 μm, diatomaceous earth 10-20 μm, iron tailings 60-80 μm, red mud 30-40 μm, bauxite 20-30 μm, aluminum ore waste rock I 50-55 μm, fly ash I 0-8 μm, fly ash I 12-18 μm, gypsum 6-12 μm, and carbonized steel slag 0-3 μm.

[0069] (5) Preheating the phosphogypsum, diatomaceous earth, iron tailings, red mud, bauxite, and aluminum ore waste rock to maintain the internal temperature at 480-500° C. and control the internal oxygen content at 21-23% for 20 minutes.

[0070] (6) The calcining furnace is filled with oxygen to control the internal oxygen content at 28-30%, and the temperature is heated to 780-820° C. at 10° C. / min. The temperature is kept for 10 minutes to carry out an oxidation reaction.

[0071] (7) The oxygen content in the calcining furnace was controlled at 24-26%, the temperature was increased to 1300-1330°C at a rate of 5°C / min, and calcined for 50 minutes.

[0072] (8) After calcination, the mixture is naturally cooled and ultrafine ground to obtain a clinker particle size of 0-8 μm and 10-18 μm, with a mass ratio of 1.2:1.

[0073] (9) Cement clinker, fly ash I, fly ash II, gypsum, and carbonized steel slag are mixed, put into a mixer, water is added, and stirred at a speed of 200-240 r / min for 15 min.

[0074] (10) Basalt fiber is added and stirred at a rotation speed of 100-120 r / min for 10 min to obtain a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based grouting material.

[0075] Comparative Example 1: Ordinary Portland Cement-Based Grouting Material

[0076] 1. Raw materials: 70 parts of ordinary Portland cement, 12 parts of fly ash, 7 parts of gypsum, 5 parts of carbonized steel slag, 4 parts of basalt fiber, and 75 parts of water.

[0077] 2. Production steps

[0078] (1) Ordinary silicate cement, fly ash, gypsum, and carbonized steel slag are crushed, ground, and ultra-finely ground to make ordinary silicate cement

[0079] The mud particle sizes are 0-8μm and 10-18μm, with a mass ratio of 1.2:1, fly ash I 0-8μm, fly ash I 12-18μm, gypsum 6-12μm, and carbonized steel slag 0-3μm.

[0080] (2) Ordinary Portland cement, fly ash I, fly ash II, gypsum, and carbonized steel slag are mixed, put into a mixer, water is added, and stirred at a speed of 200-240 r / min for 15 min.

[0081] (3) adding basalt fiber and stirring at a rotation speed of 100-120 r / min for 10 min to obtain an ordinary silicate cement-based grouting material.

[0082] Comparative Example 2: Ordinary ferroaluminate cement-based grouting material

[0083] 1. Raw materials: 70 parts of ordinary Portland cement, 12 parts of fly ash, 7 parts of gypsum, 5 parts of carbonized steel slag, 4 parts of basalt fiber, and 80 parts of water.

[0084] 2. Production steps

[0085] (1) Ordinary silicate cement, fly ash, gypsum, and carbonized steel slag are crushed, ground, and ultra-finely ground to make ordinary silicate cement

[0086] The mud particle sizes are 0-8μm and 10-18μm, with a mass ratio of 1.2:1, fly ash I 0-8μm, fly ash I 12-18μm, gypsum 6-12μm, and carbonized steel slag 0-3μm.

[0087] (2) Ordinary Portland cement, fly ash I, fly ash II, gypsum, and carbonized steel slag are mixed, put into a mixer, water is added, and stirred at a speed of 200-240 r / min for 15 min.

[0088] (3) adding basalt fiber and stirring at a rotation speed of 100-120 r / min for 10 min to obtain an ordinary silicate cement-based grouting material.

[0089] Table 1

[0090]

[0091] It can be seen from the results in Table 1 that the high-temperature sintered high-silicon slightly expansive ferroaluminate solid waste-based cementitious material obtained in each embodiment of the present invention is used to make a grouting slurry. Compared with ordinary Portland cement-based or ordinary ferroaluminate-based grouting slurry, it has the characteristics of fast setting, fast hardening, high early strength, and continuous and stable growth of later strength, and can better meet the needs of construction.

Claims

1. A high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material, characterized in that The invention is made of the following raw materials in parts by weight: ① 30-34 parts of phosphogypsum; ② 10-13 parts of diatomaceous earth; ③ 10-14 parts of iron tailings; ④ 3-6 parts of red mud; ⑤ 6-8 parts of bauxite; ⑥ 14-18 parts of aluminum ore waste rock; ⑦ 8-10 parts of fly ash I and 2-4 parts of fly ash II; ⑧ 6-8 parts of gypsum; ⑨ 4-6 parts of carbonized steel slag; ⑩ 4-6 parts of basalt fiber; some of the raw materials are dried The materials are obtained through drying, crushing, grinding and screening steps, and the particle size distribution range of each material is as follows: phosphogypsum 20-30μm, diatomaceous earth 10-20μm, iron tailings 60-80μm, red mud 30-40μm, bauxite 20-30μm, aluminum ore waste rock 50-55μm, fly ash I 0-8μm, fly ash II 12-18μm, gypsum 6-12μm, and carbonized steel slag 0-3μm. During the high-temperature sintering process, the first stage is heated to 480-500°C, the internal oxygen content is controlled at 21-23%, and the heat is kept for 20 minutes. In the second stage, the temperature is continued to be heated to 760-820°C, the internal oxygen content is controlled at 28-30%, and the heat is kept for 10 minutes to promote the oxidation reaction of the raw material. In the third stage, the temperature is heated to 1300-1330°C, the internal oxygen content is controlled at 24-26%, and it lasts for 50 minutes.

2. According to claim 1, the method for preparing high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material comprises: (1) washing phosphogypsum, iron tailings, diatomaceous earth, bauxite, and aluminum ore waste rock to remove surface impurities; (2) placing the washed product and red mud in an oven and drying them at 80-100° C. until the weight remains constant; (3) crushing phosphogypsum, diatomaceous earth, iron tailings, bauxite, aluminum ore waste rock, and red mud respectively, ball-milling to a maximum particle size of less than 120 μm, weighing the required number of portions according to the ratio, mixing, and setting aside; (4) ultrafine grinding the product of (3) and other raw materials, phosphogypsum 20-30 μm, diatomaceous earth 10-20 μm, iron tailings 60-80 μm, red mud 30-40 μm, bauxite 20-30 μm, aluminum ore waste rock I 50-55 μm, fly ash I 0-8 μm, fly ash I 12-18 μm, gypsum 6-12 μm, carbonized steel slag 0-3 μm; (5) preheating phosphogypsum, diatomaceous earth, iron tailings, red mud, bauxite, and aluminum ore waste rock to maintain the internal temperature at 480-500° C. and control the internal oxygen content at 21-23% for 20 minutes; (6) oxygenating the interior of the calcining furnace, controlling the internal oxygen content at 28-30%, heating the temperature to 780-820° C. at 10° C. / min, and keeping the temperature for 10 min to carry out oxidation reaction; (7) Controlling the oxygen content in the calcining furnace to 24-26%, raising the temperature to 1300-1330° C. at a rate of 5° C. / min, and calcining for 50 min; (8) After calcination, the mixture is naturally cooled and ultrafine ground to obtain a clinker particle size of 0-8 μm and 10-18 μm, with a mass ratio of 1.2:1; (9) Mix cement clinker, fly ash I, fly ash II, gypsum, and carbonized steel slag, put them into a mixer, and stir them at a speed of 200-240 r / min for 15 min; (10) Basalt fiber is added and stirred at a speed of 100-120 r / min for 10 min to obtain a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material.

3. According to claim 1, when sintering high-silicon micro-expanded ferroaluminate solid waste-based cementitious material at high temperature, all raw materials are uniformly ground to a particle size that can pass through a 170-mesh sieve to ensure that the raw material fineness is small and uniform.

4. According to claim 1, the method for preparing high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material is characterized by: The moisture content of phosphogypsum, diatomaceous earth, iron tailings, bauxite, aluminum ore waste rock and red mud after dehydration treatment is less than 1%.

5. According to claim 1, a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material, the clinker chemical composition of which includes: CaO 42-48 parts, SiO2 14-20 parts, Al2O3 16-24 parts, Fe2O3 5-13 parts, SO3 3-7 parts.

6. According to claim 1, a high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material, wherein the clinker minerals include: C2S 40-55 parts, C4AF 15-35 parts.

7. According to claim 1, the high-temperature sintering high-silicon micro-expansion ferroaluminate solid waste-based cementitious material controls the particle size range of the powder to 0-8μm, 6-12μm, 10-18μm, and the specific surface area is uniformly 1440-2000m 2 / kg, making the raw materials more compact and improving the slurry strength, while controlling the particle size of each raw material to the optimal hydration range to maximize activity.

8. According to claim 1, in the high-temperature sintered high-silicon micro-expansion ferroaluminate solid waste-based cementitious material, the ratio of SO3 provided by gypsum to SO3 required for the hydration reaction of ferroaluminate cement clinker to form ettringite is between 1 and 2, so that the ferroaluminate solid waste-based cementitious material has good expansion performance, and the free expansion rate of concrete prepared using the cementitious material in water is 9 to 10.5×10 -4 .

9. According to claim 1, the high-silicon micro-expanded ferroaluminate solid waste-based cementitious material is characterized by: The phosphogypsum I and phosphogypsum II meet the national standard GB / T 23456-2018 before grinding; the diatomite meets the national standard GB14936-2012; the iron tailings I and iron tailings II meet the national standard GB50863-2013 before grinding; the red mud is Bayer red mud, which meets the national standard GB50986-2014; the bauxite meets the national standard GB / T 12215-2019; the aluminum ore waste rock I and aluminum ore waste rock II meet the national standard GB / T24483 before grinding; the fly ash I and fly ash II are Class I fly ashes that meet the national standard GB / T 1596-2017 before grinding; the steel slag meets the national standard YB / T022-2008 before carbonization; the gypsum meets the national standard GB / T 9776; the basalt fiber meets the national standard GB / T 38111-2019 regulations.

10. According to claim 1, the high-temperature sintered high-silicon slightly expansive ferroaluminate solid waste-based cementitious material is based on ferroaluminate clinker, supplemented by fly ash, gypsum, and carbonized steel slag. It has the advantages of wide raw material adaptability, low energy consumption, fast setting, fast hardening, high early strength, continuous and stable growth of later strength, and corrosion resistance. It can be used as cement, mortar, concrete, grouting material, etc., and can be better adapted to various harsh environments.

Citation Information

Patent Citations

  • Marine cement and preparation method and application thereof

    AU2020104285A4

  • Belite-sulphoaluminate-ferrous aluminate cement and preparation method thereof

    CN105060745A

  • High iron aluminate-belite-sulfoaluminate cement clinker and preparation method thereof

    CN107721214A

  • System and method to treat electrolytic aluminum waste residue and co-produce quick-setting quick-hardening cement under cooperation of cement kiln

    CN108585564A

  • Condensing and curing material, hardened body containing condensing and curing material and preparation method of hardened body

    CN113402244A

Cited By

  • Gluing agent for cemented filling of argillaceous tailings and use method of cementing agent

    CN120309281A