Method for preparing aluminoferrite cement based on red mud and aluminoferrite cement
By adding fluxes and controlling the calcination conditions in the process of preparing ferroaluminate cement from red mud, the problems of hardening and insufficient performance in the preparation of red mud are solved, and the performance of the material and the proportion of red mud used are improved.
Patent Information
- Application Number
- CN202410769306.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-14
AI Technical Summary
At present, the performance of red mud in preparing ferroaluminate cement is insufficient. This is mainly due to problems with sintering temperature and red mud content, resulting in hardening, which limits the use ratio and material properties of red mud.
By mixing, drying, grinding, screening, preheating and flux mixing the red mud raw materials, extrusion molding and then calcination are used to control the mass ratio of flux to pretreatment mixture ≥ 0.03, reduce the calcination temperature, and increase the glass phase content to improve meltability and adhesion.
The amount of red mud raw material added and the performance of ferroaluminate cement are increased, the calcination temperature requirement is reduced, hardening is avoided, the glass phase content is increased, and the impermeability and crack resistance of the material are improved.
Smart Images

Figure CN118745087A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of recycling solid waste from the aluminum industry, and in particular to a method for preparing aluminoferrocement based on red mud and the aluminoferrocement. Background Art
[0002] Red mud is an industrial solid waste produced in the process of refining alumina. At present, every ton of alumina produced produces an average of 1.0 to 2.0 tons of red mud. In addition, the comprehensive utilization rate of red mud is only 7.5% at present, which leads to a large amount of red mud storage. The large amount of red mud storage not only occupies land storage space and wastes land resources, but also easily causes environmental pollution and ecological safety hazards. In addition to rich iron and aluminum elements, red mud also contains silicon oxide, aluminum oxide, iron oxide and other components. At present, ferroaluminate cement mainly includes anhydrous calcium sulfoaluminate, iron phase and dicalcium silicate. If red mud can be used as the main raw material to replace some raw materials for the preparation of ferroaluminate cement, the unique component advantages of red mud can be fully utilized.
[0003] At present, the most critical issues to be solved in the preparation of ferroaluminate cement using red mud are the proportion of ingredients, sintering system and the amount of red mud added. Since the preparation of ferroaluminate cement from red mud requires a sintering process to promote the molding of the red mud, and the general sintering process requires a temperature of about 1250°C, but too much red mud under this sintering temperature condition will cause the ferroaluminate cement material to become compacted, which leads to the fact that the amount of red mud added in the preparation process of ferroaluminate cement is generally not high, resulting in insufficient performance of the ferroaluminate cement material finally prepared.
[0004] At present, the technology for preparing ferroaluminate cement using red mud includes: (1) using high-alkali red mud as raw material, mixing various conventional raw materials to first form round cakes, then calcining at 1125°C to 1275°C, and then air cooling to prepare cement clinker. These cement clinkers include sulfoaluminate cement clinker, silicate cement clinker or ferroaluminate cement clinker. In addition, calcium sulfate can be added before calcination to adjust the pH value to solve the problem of excessive alkali content; (2) firstly subjecting red mud, steel slag, slag, desulfurized gypsum, silica fume, aluminum ash and other raw materials to raw material grinding, homogenization, sintering at 1250°C to 1300°C, clinkering, grinding and other preparation stages to finally obtain ferroaluminate cement based on industrial solid waste, and then mixing the ferroaluminate cement based on industrial solid waste with recycled materials, water, foaming agent, aggregate, air entraining agent, and reinforcing material to foam to form a lightweight thermal insulation wall material. Summary of the invention
[0005] The present application provides a method for preparing alumino-ferrocement based on red mud and alumino-ferrocement to solve the following technical problem: how to improve the performance of alumino-ferrocement prepared based on red mud.
[0006] In a first aspect, the present application provides a method for preparing ferroaluminate cement based on red mud, the method comprising:
[0007] The red mud raw material is stirred and then dried to obtain a dried material with a preset moisture content;
[0008] Grinding the dried material and then sieving it to obtain a mixed material with a preset particle size;
[0009] Preheating the mixed material and then cooling it to obtain a pretreated mixed material;
[0010] Mixing the flux with the pretreated mixed material, and then extruding to obtain a calcined raw material;
[0011] calcining the calcined raw material to obtain ferroaluminate cement;
[0012] Wherein, the mass ratio of the flux to the pretreated mixture is ≥0.03.
[0013] Optionally, the mass ratio of the flux to the pretreated mixed material is 0.1 to 0.03:1.
[0014] Optionally, the flux includes at least one of the following:
[0015] Calcium phosphate, calcium aluminum phosphate, borax, sodium borate, lithium salts and lithium silicates.
[0016] Optionally, the preset moisture content is ≤0.5%.
[0017] Optionally, the preset particle size is ≤48 μm.
[0018] Optionally, the temperature of the preheating treatment is 140° C. to 200° C., and the time of the preheating treatment is ≥ 3 hours.
[0019] Optionally, the calcination includes a heating section, and the terminal temperature of the heating section is 1070°C to 1240°C.
[0020] Optionally, the calcination further includes a heat preservation section, the temperature of the heat preservation section is the end temperature of the heating section, and the time of the heat preservation section is 30 minutes to 60 minutes.
[0021] Optionally, the mass ratio of red mud in the red mud raw material to the red mud raw material is 0.5 to 0.7.
[0022] In the second aspect, the present application provides an alumina ferrocement, which is prepared by the method described in the first aspect. The raw materials of the alumina ferrocement include, in parts by weight: red mud: 39 to 73 parts, desulfurized gypsum: 3 to 17 parts, high alumina material: 2 to 8 parts, quicklime: 10 to 20 parts, fly ash: 5 to 10 parts, flux: 3 to 8 parts, carbon slag: 2 to 6 parts and overhaul slag: 1 to 3 parts.
[0023] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0024] The embodiment of the present application provides a method for preparing ferroaluminate cement based on red mud, the method comprising: stirring the red mud raw material, and then drying it to obtain a dried material with a preset moisture content; grinding the dried material, and then screening it to obtain a mixed material with a preset particle size; preheating the mixed material, and then cooling it to obtain a pretreated mixed material; mixing a flux with the pretreated mixed material, and then extruding it to obtain a calcined raw material; calcining the calcined raw material to obtain ferroaluminate cement; wherein the mass ratio of the flux to the pretreated mixed material is ≥0.03. The mass ratio of flux to pretreated mixture can be ≥0.03, which can ensure that the pretreated mixture has sufficient flux. Sufficient flux can effectively improve the composition and structure of the pretreated mixture to improve the solubility of the pretreated mixture. The pretreated mixture with improved thermal solubility can reduce the heat demand in the calcination stage, thereby reducing the temperature in the calcination stage to avoid the compaction of ferroaluminate cement caused by the addition of a large amount of red mud, thereby increasing the amount of red mud raw material added. In addition, sufficient flux can promote the melting reaction of red mud and other components in the pretreated mixture to increase the content of glass phase in ferroaluminate cement. Sufficient glass phase can improve the adhesion and fluidity of ferroaluminate cement to accommodate more red mud raw materials, thereby improving the performance of the prepared ferroaluminate cement. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0026] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0027] Figure 1A schematic flow chart of a method for preparing ferroaluminate cement based on red mud provided in an embodiment of the present application;
[0028] Figure 2 A product diagram of alumina-ferrocement provided in an embodiment of the present application. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0030] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0031] In this document, the terms including "comprising" and the like mean "including but not limited to". "At least one" means one or more, "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in this application can be purchased on the market or prepared by existing methods.
[0032] It should be noted that alumina-ferrocement has excellent impermeability. Under the condition that the calcium sulfoaluminate hydration products of alumina-ferrocement are restricted by the hydration space, the internal structure of alumina-ferrocement will extend into the gaps, which will cut off the structural channels of alumina-ferrocement. In addition, the hydration products of iron glue and aluminum glue in alumina-ferrocement will continuously fill the gaps. The superposition of this dual effect will minimize the void ratio of concrete. Therefore, the internal mechanism of the impermeability of alumina-ferrocement during its own expansion is different from that of silicate cement, and the hydration products in alumina-ferrocement squeeze each other to obtain a mutually interlinked and interconnected structure, thereby promoting alumina-ferrocement to have higher crack resistance and impermeability.
[0033] Therefore, if the amount of red mud raw material added can be increased, the performance of ferroaluminate cement will be further improved.
[0034] Figure 1 A schematic flow chart of a method for preparing ferroaluminate cement based on red mud provided in an embodiment of the present application is shown by way of example;
[0035] like Figure 1 As shown, the embodiment of the present application provides a method for preparing ferroaluminate cement based on red mud, the method comprising:
[0036] S1. stirring the red mud raw material and then drying it to obtain a dried material having a preset moisture content;
[0037] S2. The dried material is ground and then sieved to obtain a mixed material having a preset particle size;
[0038] S3. Preheating the mixture and then cooling it to obtain a pretreated mixture;
[0039] S4. The flux is mixed with the pretreated mixed material, and then extruded to obtain a calcined raw material;
[0040] S5. calcining the calcined raw material to obtain ferroaluminate cement;
[0041] Wherein, the mass ratio of the flux to the pretreated mixture is ≥0.03.
[0042] It should be noted that the red mud raw materials can be bulk solid wastes related to the aluminum industry. These bulk solid wastes can be sintered red mud, desulfurized gypsum, high-alumina materials (aluminum corrective materials), quicklime, fly ash, carbon slag, and overhaul slag.
[0043] It should be noted that the extrusion molding can be extruded into a cylindrical shape.
[0044] In some optional embodiments, the mass ratio of the flux to the pretreated mixed material is 0.1 to 0.03:1;
[0045] In these embodiments, the mass ratio of flux to pretreated mixed material can be 0.1 to 0.03:1, which can enable the pretreated mixed material to have a sufficient amount of flux. A sufficient amount of flux can effectively improve the solubility of the pretreated mixed material to reduce the temperature in the calcination stage, thereby avoiding the compaction of ferroaluminate cement caused by the addition of a large amount of red mud, thereby increasing the amount of red mud raw material added. In addition, a sufficient amount of flux can increase the content of glass phase in ferroaluminate cement, and a sufficient amount of glass phase can improve the adhesion and fluidity of ferroaluminate cement to accommodate more red mud raw materials, thereby improving the performance of the prepared ferroaluminate cement.
[0046] The mass ratio of the flux to the pretreated mixed material can be 0.1:1, 0.09:1, 0.08:1, 0.07:1, 0.06:1, 0.05:1, 0.04:1 or 0.03:1.
[0047] In some optional embodiments, the flux includes at least one of the following:
[0048] calcium phosphate, calcium aluminum phosphate, borax, sodium borate, lithium salts, and lithium silicates;
[0049] In these embodiments, the flux may include: at least one of calcium phosphate, calcium aluminum phosphate, borax, sodium borate, lithium salts and lithium silicates, which can enable the flux to effectively reduce the temperature of the calcination stage, thereby avoiding the hardening of ferroaluminate cement caused by the large amount of red mud added, and then increase the amount of red mud raw material added to improve the performance of the prepared ferroaluminate cement.
[0050] It should be noted that the flux changes the component distribution of silicate, aluminate, ferrite and calcium salt in ferroaluminate cement and promotes the melting reaction of these ferroaluminate cement components, thereby improving the sintering performance of ferroaluminate cement. In addition, the flux can improve the structural distribution of ferroaluminate cement to further improve the melting performance of ferroaluminate cement.
[0051] It should be noted that the flux can promote the melting reaction of silicates and aluminates to affect the formation and change of mineral phases in ferroaluminate cement, and can increase the amount of glass phase generated in ferroaluminate cement. A sufficient amount of glass phase can increase the adhesion and fluidity of ferroaluminate cement to improve the performance of the prepared ferroaluminate cement.
[0052] In some optional embodiments, the preset moisture content is ≤0.5%;
[0053] In these embodiments, the preset moisture content can be ≤0.5%, which can facilitate subsequent grinding and screening to obtain a mixed material with a preset particle size; in addition, the preset moisture content below 0.5% can avoid the need for additional heat to evaporate water during the calcination stage, thereby effectively reducing the temperature of the calcination stage to avoid the large amount of red mud added causing the ferroaluminate cement to become compacted, and then the amount of red mud raw material added can be increased to improve the performance of the prepared ferroaluminate cement.
[0054] In some optional embodiments, the preset particle size is ≤48 μm.
[0055] In these embodiments, the preset particle size can be ≤48 μm, which can make the mixed materials fine enough, and the fine enough mixed materials can be fully and evenly mixed to promote sufficient calcination, thereby promoting the full formation of various phases in the ferroaluminate cement to avoid excessive differences in the final ferroaluminate cement composition.
[0056] In some optional embodiments, the temperature of the preheat treatment is 140° C. to 200° C., and the time of the preheat treatment is ≥ 3 hours.
[0057] In these embodiments, the preheating temperature can be 140°C to 200°C, and the preheating time can be ≥3h, which can promote the initial reaction of the high-aluminum material of the red mud raw material to convert the aluminum hydroxide component in the red mud raw material into alumina, thereby completing the supplementation of the aluminum corrector of the ferroaluminate cement to promote the full formation of the various phase components of the ferroaluminate cement. In addition, the preheating treatment can increase the heat of the carbon-containing matter in the red mud raw material to effectively reduce the calcination temperature in the subsequent calcination stage, so as to avoid the calcination of the ferroaluminate cement caused by the large amount of red mud added, and then the amount of red mud raw material added can be increased to improve the performance of the prepared ferroaluminate cement.
[0058] The temperature of the preheat treatment may be 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C.
[0059] In some optional embodiments, the calcination includes a heating section, and the terminal temperature of the heating section is 1070°C to 1240°C.
[0060] In these embodiments, calcination may include a heating stage, and the terminal temperature of the heating stage may be 1070°C to 1240°C. Heating may be used to meet the heat requirement of calcination to prompt the pretreated mixed material to quickly reach the phase change temperature, thereby prompting the calcined raw material to be converted into alumina-ferrocement product.
[0061] The terminal temperature of the heating section can be 1070°C, 1080°C, 1090°C, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C or 1240°C.
[0062] In some optional embodiments, the calcination further includes a heat preservation section, the temperature of the heat preservation section is the end temperature of the heating section, and the time of the heat preservation section is 30 minutes to 60 minutes.
[0063] In these embodiments, calcination may also include a holding section, and the temperature of the holding section is the end temperature of the heating section, and the holding period may be 30 minutes to 60 minutes, which can promote complete phase change in the ferroaluminate cement to obtain a ferroaluminate cement product with uniform component distribution and stable structure; in addition, while the ferroaluminate cement is being generated, the energy consumption of calcination can be reduced to save the energy consumption cost of calcination.
[0064] The insulation period can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min.
[0065] In some optional embodiments, the mass ratio of the red mud in the red mud raw material to the red mud raw material is 0.5 to 0.7.
[0066] In these embodiments, the mass ratio of red mud in the red mud raw material to the red mud raw material can be 0.5-0.7, which can ensure that the red mud raw material has a sufficient amount of red mud, and the sufficient amount of red mud has a sufficient amount of aluminum phase and iron phase, and after calcination, an ferroaluminate cement product with uniform composition and stable structure can be formed; this means that the amount of red mud doped in the ferroaluminate cement can account for more than half of the red mud raw material.
[0067] The mass ratio of red mud to red mud raw material in the red mud raw material can be 0.5, 0.6 or 0.7.
[0068] Figure 2 A schematic diagram of a product of ferroaluminate cement provided in an embodiment of the present application is shown exemplarily;
[0069] Based on a general inventive concept, such as Figure 2 As shown, an embodiment of the present application provides an alumina ferrocement, which is prepared by the method. The raw materials of the alumina ferrocement include, by weight: red mud: 39 to 73 parts, desulfurized gypsum: 3 to 17 parts, high alumina material: 2 to 8 parts, quicklime: 10 to 20 parts, fly ash: 5 to 10 parts, flux: 3 to 8 parts, carbon slag: 2 to 6 parts and overhaul slag: 1 to 3 parts.
[0070] The ferroaluminate cement is realized based on the above method. The specific steps of the method can refer to the above embodiment. Since the ferroaluminate cement adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.
[0071] It should be noted that in the composition of the ferroaluminate cement, the weight proportion of red mud can be 39 parts to 73 parts, and a sufficient amount of red mud can provide a sufficient amount of aluminum, iron and other elements for the ferroaluminate cement; the weight proportion of desulfurized gypsum can be 3 parts to 17 parts, and a sufficient amount of desulfurized gypsum can adjust the pH value of the ferroaluminate cement; the weight proportion of high-aluminum material can be 2 parts to 8 parts, and a sufficient amount of high-aluminum material can be used as an aluminum correcting material for the ferroaluminate cement; the weight proportion of quicklime can be 10 parts to 20 parts, and a sufficient amount of quicklime can absorb the carbon dioxide generated during the calcination process to avoid the generation of a large amount of carbon dioxide during the calcination process and affecting the product quality of the ferroaluminate cement; the weight proportion of fly ash can be 5 parts to 10 parts, and a sufficient amount of fly ash can supplement silicon elements for the ferroaluminate cement. The weight proportion of the flux can be 3 to 8 parts, which can provide sufficient flux for the ferroaluminate cement to fully reduce the calcination temperature, thereby increasing the amount of red mud raw materials added; the weight proportion of the carbon slag can be 2 to 6 parts, and sufficient carbon slag can be used as a fuel supplement to supplement the heat loss in the calcination stage; the weight proportion of the overhaul slag can be 1 to 3 parts, and sufficient overhaul slag contains sufficient cryolite and calcium fluoride, which can reduce the melting point of the calcined raw materials to reduce the temperature requirement for calcination. In addition, the overhaul slag can be used as a foaming agent during the calcination process to generate nitrogen and a small amount of carbon dioxide during the calcination process, thereby avoiding the poisoning effect of carbon dioxide on the ferroaluminate cement.
[0072] The weight proportions of the red mud may be 39 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts or 73 parts.
[0073] The weight proportions of the desulfurized gypsum can be 3 parts, 5 parts, 10 parts, 15 parts or 17 parts.
[0074] The weight proportion of the high aluminum material can be 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts or 8 parts.
[0075] The weight parts of the quicklime can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts.
[0076] The weight proportions of the fly ash can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts.
[0077] The weight proportion of the flux can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts or 8 parts.
[0078] The weight proportion of the carbon residue can be 2 parts, 3 parts, 4 parts, 5 parts or 6 parts.
[0079] The weight proportion of the overhaul slag can be 1 part, 2 parts or 3 parts.
[0080] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.
[0081] Example 1
[0082] like Figure 1 As shown, a method for preparing ferroaluminate cement based on red mud comprises:
[0083] S1. stirring the red mud raw material and then drying it to obtain a dried material having a preset moisture content;
[0084] S2. Grinding the dried material and then sieving it to obtain a mixed material having a preset particle size;
[0085] S3. Preheating the mixture and then cooling it to obtain a pretreated mixture;
[0086] S4. The flux is mixed with the pretreated mixed material, and then extruded to obtain a calcined raw material;
[0087] S5. calcining the calcined raw materials to obtain ferroaluminate cement.
[0088] The mass ratio of flux to pre-treated mixed material is 0.03:1.
[0089] The flux is lithium salt.
[0090] The preset moisture content is 0.41%.
[0091] The preset particle size is ≤48μm.
[0092] The preheating temperature is 200°C and the preheating time is 3h.
[0093] The calcination includes a heating section, the terminal temperature of the heating section is 1070°C, and the heating rate is 5°C / min.
[0094] The calcination also includes a heat preservation section, the temperature of the heat preservation section is the end temperature of the heating section, and the time of the heat preservation section is 60 minutes.
[0095] A kind of ferroaluminate cement is prepared by a method. The raw materials of the ferroaluminate cement include, by weight: 39 parts of red mud, 17 parts of desulfurized gypsum, 8 parts of high-alumina material, 19 parts of quicklime, 10 parts of fly ash, 3 parts of flux, 4 parts of carbon slag and 3 parts of overhaul slag.
[0096] Example 2
[0097] Based on the contents disclosed in Example 1, the following modifications are further made:
[0098] The mass ratio of flux to pre-treated mixed material is 0.05:1.
[0099] The flux is calcium phosphate.
[0100] The preset moisture content is 0.43%.
[0101] The preheating temperature is 180°C and the preheating time is 3 hours.
[0102] The terminal temperature of the heating section was 1130°C, and the heating rate was 5°C / min.
[0103] The insulation time is 50 minutes.
[0104] In terms of weight, the raw materials of ferroaluminate cement include: red mud: 51 parts, desulfurized gypsum: 13 parts, high-alumina material: 7 parts, quicklime: 15 parts, fly ash: 9 parts, flux: 5 parts, carbon slag: 3 parts and overhaul slag: 2 parts.
[0105] Example 3
[0106] Based on the contents disclosed in Example 1, the following modifications are further made:
[0107] The mass ratio of flux to pre-treated mixed material is 0.08:1.
[0108] The flux is borax.
[0109] The preset moisture content is 0.46%.
[0110] The preheating temperature is 160°C and the preheating time is 3 hours.
[0111] The terminal temperature of the heating section was 1190°C, and the heating rate was 5°C / min.
[0112] The insulation time is 40 minutes.
[0113] In terms of weight, the raw materials of ferroaluminate cement include: red mud: 62 parts, desulfurized gypsum: 10 parts, high-alumina material: 5 parts, quicklime: 13 parts, flux: 8 parts, fly ash: 7 parts, carbon slag: 2 parts and overhaul slag: 1 part.
[0114] Example 4
[0115] Based on the contents disclosed in Example 1, the following modifications are further made:
[0116] The mass ratio of flux to pre-treated mixed material is 0.08:1.
[0117] The flux is lithium silicate.
[0118] The preset moisture content is 0.48%.
[0119] The preheating temperature is 140°C and the preheating time is 3 hours.
[0120] The terminal temperature of the heating section was 1240°C, and the heating rate was 5°C / min.
[0121] The temperature of the insulation section is the end temperature of the heating section, and the time of the insulation section is 30 minutes.
[0122] Calculated by weight, the raw materials of ferroaluminate cement include: red mud: 73 parts, desulfurized gypsum: 7 parts, high-alumina material: 32 parts, quicklime: 10 parts, fly ash: 5 parts, carbon slag: 2 parts and overhaul slag: 1 part.
[0123] Comparative Example 1
[0124] Based on the contents disclosed in Example 4, the following modifications are further made:
[0125] The weight proportion of red mud is 80 parts.
[0126] Comparative Example 2
[0127] Based on the contents disclosed in Example 4, the following modifications are further made:
[0128] The weight proportion of red mud is 30 parts.
[0129] Comparative Example 3
[0130] Based on the contents disclosed in Example 4, the following modifications are further made:
[0131] The weight portion of the co-solvent is 1 part.
[0132] Comparative Example 4
[0133] Based on the contents disclosed in Example 4, the following modifications are further made:
[0134] The weight percentage of the cosolvent is 10 parts
[0135] Comparative Example 5
[0136] Based on the contents disclosed in Example 4, the following modifications are further made:
[0137] The temperature of the preheat treatment is 100°C.
[0138] Comparative Example 6
[0139] Based on the contents disclosed in Example 4, the following modifications are further made:
[0140] The temperature of the preheat treatment is 300°C.
[0141] Comparative Example 7
[0142] Based on the contents disclosed in Example 4, the following modifications are further made:
[0143] The final temperature of the heating section is 1000°C.
[0144] The insulation time is 80 minutes.
[0145] Comparative Example 8
[0146] Based on the contents disclosed in Example 4, the following modifications are further made:
[0147] The final temperature of the heating section is 1300°C.
[0148] The insulation period is 20 minutes.
[0149] Related experiments and effect data:
[0150] The cement products obtained in each embodiment and comparative example were respectively subjected to the "Standard Cement Mortar Strength Test"
[0151] The experiment was conducted according to the standard of GB / T17671-1999, and the compressive strength of each cement product was calculated on the third, seventh and twenty-eighth days of the experiment. The results are shown in Table 1.
[0152] Table 1 Compressive strength data of cement products of various embodiments and comparative examples
[0153]
[0154]
[0155] As can be seen from Table 1, according to the data of Comparative Example 1, Comparative Example 2 and Example 4, excessive or insufficient addition of red mud will result in insufficient strength of the final ferroaluminate cement product or even the inability to further increase the strength.
[0156] In addition, the data from Comparative Example 3, Comparative Example 4 and Example 4 show that if the amount of flux added is insufficient, a small amount of flux will lead to the calcination process cannot be fully carried out, the reaction between the calcined raw materials is insufficient, and the final content of effective phase in the ferroaluminate cement is insufficient, affecting the performance of the ferroaluminate cement. In addition, if the amount of flux added is too much, too much flux will remain in the final ferroaluminate cement, which will also lead to insufficient content of effective phase in the ferroaluminate cement, affecting the performance of the ferroaluminate cement.
[0157] In addition, according to the data of Comparative Example 5, Comparative Example 6 and Example 4, if the preheating temperature is too low or too high, it will lead to insufficient preheating or overheating in the preheating stage, which will eventually affect the heat replenishment in the calcination stage, causing the calcination to be unable to proceed fully, thereby reducing the content of the effective phase in the final ferroaluminate cement and affecting the performance of the ferroaluminate cement.
[0158] In addition, according to the data of Comparative Example 7, Comparative Example 8 and Example 4, if the calcination temperature is too high or too low, and the insulation time is too long or too short, it will affect the heat in the calcination stage, causing the calcination to be unable to proceed fully, thereby reducing the content of the effective phase in the final ferroaluminate cement and affecting the performance of the ferroaluminate cement.
[0159] In summary, the method for preparing ferroaluminate cement based on red mud provided in the embodiment of the present application can effectively improve the composition and structure of the pretreated mixture by adding a flux before calcining the red mud raw material, so as to improve the solubility of the pretreated mixture, and then increase the amount of red mud raw material added. In addition, a sufficient amount of flux can increase the content of the glass phase in the ferroaluminate cement to accommodate more red mud raw material, thereby improving the compressive strength of the prepared ferroaluminate cement.
[0160] In addition, the embodiment of the present application provides a method for preparing ferroaluminate cement based on red mud, which uses a flux to reduce the calcination temperature, can effectively reduce the energy consumption of the entire preparation method, save energy in the preparation stage, and realize the large-scale application of red mud.
[0161] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.
Claims
1. A method for preparing ferroaluminate cement based on red mud, characterized in that: The method comprises: The red mud raw material is stirred and then dried to obtain a dried material with a preset moisture content; Grinding the dried material and then sieving it to obtain a mixed material with a preset particle size; Preheating the mixed material and then cooling it to obtain a pretreated mixed material; Mixing the flux with the pretreated mixed material, and then extruding to obtain a calcined raw material; calcining the calcined raw material to obtain ferroaluminate cement; Wherein, the mass ratio of the flux to the pretreated mixture is ≥0.
03.
2. The method according to claim 1, characterized in that The mass ratio of the flux to the pretreated mixed material is 0.1 to 0.03:
1.
3. The method according to claim 1 or 2, characterized in that: The flux comprises at least one of the following: Calcium phosphate, calcium aluminum phosphate, borax, sodium borate, lithium salts and lithium silicates.
4. The method according to claim 1, characterized in that: The preset moisture content is ≤0.5%.
5. The method according to claim 1, characterized in that The preset particle size is ≤48 μm.
6. The method according to claim 1, characterized in that The temperature of the preheating treatment is 140° C. to 200° C., and the time of the preheating treatment is ≥ 3 hours.
7. The method according to claim 1, characterized in that The calcination comprises a heating section, and the terminal temperature of the heating section is 1070°C to 1240°C.
8. The method according to claim 7, characterized in that The calcination further comprises a heat preservation section, the temperature of the heat preservation section is the end temperature of the heating section, and the time of the heat preservation section is 30 minutes to 60 minutes.
9. The method according to claim 1, characterized in that: The mass ratio of the red mud in the red mud raw material to the red mud raw material is 0.5 to 0.
7.
10. A ferroaluminate cement, characterized in that: The ferroaluminate cement is prepared by the method described in any one of claims 1 to 9. The raw materials of the ferroaluminate cement include, by weight: 39 to 73 parts of red mud, 3 to 17 parts of desulfurized gypsum, 2 to 8 parts of high-alumina material, 10 to 20 parts of quicklime, 5 to 10 parts of fly ash, 3 to 8 parts of flux, 2 to 6 parts of carbon slag and 1 to 3 parts of overhaul slag.
Citation Information
Patent Citations
Method for preparing high-iron cement by utilizing red mud
CN103833245A
Method for preparing microcrystal calcium aluminoferrite by using red mud
CN106746801A
Method for preparing aluminoferriate cement by using red mud cooperating with other solid waste
CN108328950A
Method for preparing aluminoferrite cement clinker from Bayer red mud
CN111533473A
Iron aluminate cement clinker, solid-waste-based high-strength iron aluminate cement and preparation methods of iron aluminate cement clinker and solid-waste-based high-strength iron aluminate cement
CN117486512A