Preparation method of green cementing material based on metallurgical slag
By adding modification treatment and plant fiber to metallurgical slag, a green cementitious material with high strength and low slump is prepared, which solves the problem of insufficient mechanical properties and efflorescence of metallurgical slag in cementitious materials, and achieves Effective use of resources and environmental protection effects.
Patent Information
- Application Number
- CN202410750978.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
AI Technical Summary
The existing metallurgical slag used as a filling material for cementitious materials has poor mechanical properties and low strength, and is difficult to meet the problem of efflorescence on building walls. It fails to effectively utilize metallurgical slag resources, leading to environmental pollution and resource waste.
By adding modified slag, alkali activator and plant fiber to the cement mixer for mixing and maintenance, a green cementitious material based on metallurgical slag is prepared. The modified slag undergoes surface modification treatment and introduces -COO- and The benzene ring structure retards setting, protects slump, inhibits the generation of efflorescence, and improves material strength.
It realizes the effective utilization of metallurgical slag, improves the strength and alkali resistance of cementitious materials, suppresses the generation of efflorescence, saves the amount of alkali activator, has the characteristics of high strength, low slump and environmental protection, and has important application value.
Smart Images

Figure BDA0004887916890000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cementitious materials, and in particular, relates to a method for preparing a green cementitious material based on metallurgical slag. Background Art
[0002] In recent years, with the rapid development of national industry, the metallurgical industry has also grown rapidly. The melt generated in the pyrometallurgical process and floating on the surface of liquid substances such as metals is mainly composed of oxides (silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide), and often contains sulfides and a small amount of metal. This type of waste material is called slag or slag. The stacking and treatment of this type of slag may cause environmental pollution, such as dust, leakage of harmful substances, occupation of land, pollution of groundwater, etc. Therefore, the effective utilization of slag waste is of great significance to environmental protection.
[0003] Since the main components of slag are silicon dioxide and metal oxides, it is often used as a filler for cementitious materials and can also be used as an admixture for cement-based materials. Cementitious materials, also known as binders. Under physical and chemical effects, it can be transformed from a slurry into a solid stone-like body, and can bind other materials to make a composite solid substance with a certain mechanical strength. Cementitious materials can be divided into two categories: inorganic and organic. Lime, gypsum, cement and other building materials commonly known as "ash" on construction sites belong to inorganic cementitious materials; while asphalt, natural or synthetic resins, etc. belong to organic cementitious materials. However, the cementitious materials obtained by adding only slag as a filler have poor mechanical properties and low strength; in addition, cement, as the most commonly used cementitious material, is difficult to solve the problem of alkali efflorescence on building walls with slag as a filler. Therefore, the above problems need to be solved to meet the higher use requirements of metallurgical slag in the field of cementitious material technology. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a green cementitious material based on metallurgical slag.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing a green cementitious material based on metallurgical slag comprises the following steps:
[0007] Add modified slag into a cement mixer, stir at 40-60 rpm / min for 5 minutes, add alkali activator, plant fiber and water and stir at 40-60 rpm / min for 5 minutes, then stir at 120-150 rpm / min for 10 minutes until the mixture is evenly mixed, take out and pour into the corresponding mold, and cure for 5-8 days to obtain a green cementitious material based on metallurgical slag.
[0008] Furthermore, the raw materials are calculated in parts by weight as follows: 50-60 parts of modified slag, 6-10 parts of alkali activator, 10-15 parts of plant fiber, and 90-110 parts of water.
[0009] Furthermore, the alkali activator is sodium silicate with a modulus of 2.5-3.1.
[0010] Furthermore, the plant fiber is one or more of bamboo fiber, flax fiber, ramie fiber and jute fiber.
[0011] Furthermore, the curing is carried out in a constant temperature and humidity curing box with a temperature of 25° C. and a relative humidity greater than 90%.
[0012] Furthermore, the modified slag is prepared by the following steps:
[0013] S1. Dry the slag in an oven at 100°C, add it to a vertical ball mill and grind it into powder, mix it with N,N-dimethylformamide (DMF), add it to a magnetic stirring device, put in a magnet, start stirring for 30 minutes, so that the slag powder is evenly dispersed in N,N-dimethylformamide, evacuate the device, pass N2 gas, add γ-aminopropyltriethoxysilane (silane coupling agent KH-550), set the reaction temperature to 55°C, react for 6 hours, and after the reaction is completed, filter, wash with ethanol, and then dry it in a vacuum drying oven for 2 hours to obtain pre-modified slag; the ratio of slag, N,N-dimethylformamide, and γ-aminopropyltriethoxysilane is 10.0g:100mL:7.5g;
[0014] The chemical composition of the slag is silicon dioxide and metal oxides. The surfaces of these oxides contain a lot of hydroxyl groups, which can be introduced into amino groups by reacting with KH-550 to obtain pre-modified slag.
[0015] S2. In a three-necked flask equipped with a stirring device, the pre-modified slag and N,N-dimethylformamide were mixed and stirred evenly, a magnet was added, and magnetic stirring was carried out for 1 hour, and then terephthalic acid and dicyclohexylcarbodiimide (DCC, a dehydrating agent) were added. The reaction was carried out in a 50°C water bath for 45 minutes. After the reaction was completed, sodium hydroxide solution was added dropwise, and the temperature was maintained at 50°C and stirred for 45 minutes. Then, the solution was filtered, the solvent was removed by rotary evaporation, and vacuum dried to obtain modified slag. The ratio of the amount of pre-modified slag, N,N-dimethylformamide, phthalic acid, dicyclohexylcarbodiimide, and sodium hydroxide solution was 10.0 g: 100 mL: 18.4 g: 22.6 g: 75 mL.
[0016] The amino groups on the pre-modified slag react with the carboxyl groups on the terephthalic acid to undergo an amidation reaction. Under the action of a dehydrating agent, the reaction can be carried out under relatively mild conditions to obtain modified slag.
[0017] By surface modification of the modified slag, -COO is introduced into the molecule - It can slow down the setting and prevent collapse, and can also delay and inhibit the setting time of cement and the hydration of C3A mineral and C3S mineral components to inhibit the production of efflorescence, and can achieve high efficiency in water reduction; in addition, benzene rings are introduced into the molecule, which has a rigid structure and can improve the strength of the matrix.
[0018] Beneficial effects of the present invention:
[0019] 1. The cementitious material prepared by the present invention realizes the effective utilization of resources by utilizing the waste metallurgical slag as the filling material;
[0020] 2. By adding plant fiber, it can not only serve as a reinforcing material to enhance the strength of the cementitious material, but also provide some alkalinity, reducing the amount of alkali activator used and saving costs;
[0021] 3. The modified slag obtained by surface modification of the slag can improve the strength of the material and inhibit the generation of efflorescence;
[0022] Therefore, the cementitious material prepared by the present invention has high strength, is collapse-resistant, can inhibit the generation of efflorescence, and realizes the effective utilization of waste resources. It has good homogeneity without unnecessary additives, is green and environmentally friendly, and has important application value in the technical field of cementitious materials. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1
[0025] Preparation of modified slag:
[0026] S1. Dry 10.0 g of slag in an oven at 100 °C, add it to a vertical ball mill and grind it into powder, mix it with 100 mL of DMF, add it to a magnetic stirring device, put in a magnet, start stirring for 30 minutes, so that the slag powder is evenly dispersed in N,N-dimethylformamide, evacuate the device, pass N2 gas, add 7.5 g of silane coupling agent KH-550, set the reaction temperature to 55 °C, react for 6 hours, filter it after the reaction is completed, wash it with ethanol, and then dry it in a vacuum drying oven for 2 hours to obtain pre-modified slag;
[0027] S2. In a three-necked flask equipped with a stirring device, 10.0 g of pre-modified slag and 100 mL of N,N-dimethylformamide were mixed and stirred evenly, and a magnet was put in. After magnetic stirring for 1 hour, 18.4 g of terephthalic acid and 22.6 g of DCC were added. The mixture was reacted for 45 minutes in a 50°C water bath. After the reaction was completed, 75 mL of sodium hydroxide solution (concentration 0.1 mol / L) was added dropwise. The temperature was maintained at 50°C and stirred for 45 minutes. Then, the mixture was filtered, the solvent was removed by rotary evaporation, and vacuum dried to obtain modified slag.
[0028] Example 2
[0029] Preparation of modified slag:
[0030] S1. Dry 20.0 g of slag in an oven at 100 °C, add it to a vertical ball mill and grind it into powder, mix it with 200 mL of DMF, add it to a magnetic stirring device, put in a magnet, start stirring for 30 minutes, so that the slag powder is evenly dispersed in N, N-dimethylformamide, evacuate the device, pass N2 gas, add 15 g of silane coupling agent KH-550, set the reaction temperature to 55 °C, react for 6 hours, filter it after the reaction is completed, wash it with ethanol, and then dry it in a vacuum drying oven for 2 hours to obtain pre-modified slag;
[0031] S2. In a three-necked flask equipped with a stirring device, mix 20.0 g of pre-modified slag and 200 mL of N,N-dimethylformamide and stir evenly, put in a magnet, stir magnetically for 1 hour, then add 36.8 g of terephthalic acid and 45.2 g of DCC, and react for 45 minutes in a 50°C water bath. After the reaction, add 150 mL of sodium hydroxide solution (concentration 0.1 mol / L) dropwise, maintain the temperature at 50°C and stir for 45 minutes, filter, remove the solvent by rotary evaporation, and dry in vacuo to obtain modified slag.
[0032] Example 3
[0033] Add 50 g of the modified slag prepared in Example 1 into a cement mixer, stir at 40 rpm / min for 5 min, and after stirring evenly, add 6 g of sodium silicate (modulus 2.5), 10 g of bamboo fiber and 90 g of water and stir at 40 rpm / min for 5 min, and then stir at 120 rpm / min for 10 minutes until the mixture is evenly mixed to obtain a green cementitious material based on metallurgical slag.
[0034] Example 4
[0035] 55 g of the modified slag prepared in Example 2 was added to a cement mixer and stirred at 50 rpm / min for 5 min. After stirring evenly, 8 g of sodium silicate (modulus 2.7), 12.5 g of flax fiber and 100 g of water were added and stirred at 50 rpm / min for 5 min. Then, the mixture was stirred at 135 rpm / min for 10 minutes until evenly mixed to obtain a green cementitious material based on metallurgical slag.
[0036] Example 5
[0037] 60 g of the modified slag prepared in Example 2 was added to a cement mixer and stirred at 60 rpm / min for 5 min. After stirring evenly, 10 g of sodium silicate (modulus 3.1), 15 g of jute fiber and 110 g of water were added and stirred at 60 rpm / min for 5 min, and then stirred at 150 rpm / min for 10 minutes until the mixture was evenly mixed to obtain a green cementitious material based on metallurgical slag.
[0038] Comparative Example 1
[0039] Ordinary slag of equal mass is used to replace the modified slag in Example 5, and the remaining steps are the same as in Example 5.
[0040] Comparative Example 2
[0041] Commercially available cementitious materials produced by Chongqing Kunchen Building Materials Co., Ltd. were used.
[0042] Examples 3-5 and comparative examples 1-2 were made into corresponding shapes to be tested according to different test standards, and the following performance tests were performed:
[0043] The degree of efflorescence is determined by the "spray-dry" cycle method specified in JC / T 1024-2007 "Wall Finishing Mortar";
[0044] The national standard GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)" is used to measure the compressive and flexural strength after 28 days of curing according to the standard curing method;
[0045] The slump was measured using CECS203:2006 "Technical Specifications for Application of Self-compacting Concrete"; the results are shown in the following table:
[0046]
[0047] It can be seen from the above table that the strength, collapse retention and efflorescence inhibition ability of the cementitious material prepared in the embodiment of the present invention are higher than those of the control example, and as the amount of modified slag is continuously increased, various properties are improved, which has important application value in the field of cementitious material technology.
[0048] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0049] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing green cementitious materials based on metallurgical slag, It is characterized in that The following steps are involved: Add modified slag into a cement mixer, stir at 40-60 rpm / min for 5 minutes, add alkali activator, plant fiber and water and stir at 40-60 rpm / min for 5 minutes, then stir at 120-150 rpm / min for 10 minutes until the mixture is evenly mixed, take out and pour into the corresponding mold, and cure for 5-8 days to obtain a green cementitious material based on metallurgical slag.
2. A method for preparing a green cementitious material based on metallurgical slag according to claim 1, It is characterized in that The modified slag is prepared by the following steps: S1. Dry the slag in an oven at 100°C, add it to a vertical ball mill and grind it into powder, mix it with N,N-dimethylformamide, stir it magnetically for 30 minutes, evacuate the device, and pass N 2 gas, add γ-aminopropyltriethoxysilane, set the reaction temperature to 55°C, react for 6 hours, and when the reaction is complete, filter, wash, and vacuum dry to obtain pre-modified slag; S2. Mix the pre-modified slag and N,N-dimethylformamide and stir them evenly. After magnetic stirring for 1 hour, add terephthalic acid and dicyclohexylcarbodiimide. React for 45 minutes in a water bath at 50°C. After the reaction is completed, add sodium hydroxide solution dropwise. Maintain the temperature at 50°C and stir for 45 minutes. Then filter, rotary evaporate and vacuum dry to obtain modified slag.
3. A method for preparing a green cementitious material based on metallurgical slag according to claim 2, It is characterized in that In step S1, the ratio of the amount of slag, N,N-dimethylformamide, and γ-aminopropyltriethoxysilane is 10.0 g:100 mL:7.5 g.
4. A method for preparing a green cementitious material based on metallurgical slag according to claim 2, It is characterized in that In step S2, the ratio of the amount of pre-modified slag, N,N-dimethylformamide, phthalic acid, dicyclohexylcarbodiimide, and sodium hydroxide solution is 10.0 g: 100 mL: 18.4 g: 22.6 g: 75 mL.
5. A method for preparing a green cementitious material based on metallurgical slag according to claim 1, It is characterized in that The raw materials are calculated in parts by weight as follows: 50-60 parts of modified slag, 6-10 parts of alkali activator, 10-15 parts of plant fiber, and 90-110 parts of water.
6. A method for preparing a green cementitious material based on metallurgical slag according to claim 1, It is characterized in that The alkali activator is sodium silicate with a modulus of 2.5-3.
1.
7. A method for preparing a green cementitious material based on metallurgical slag according to claim 1, It is characterized in that The plant fiber is one or more of bamboo fiber, flax fiber, ramie fiber and jute fiber.
8. A method for preparing a green cementitious material based on metallurgical slag according to claim 1, It is characterized in that The curing is carried out in a constant temperature and humidity curing box, with a temperature of 25° C. and a relative humidity greater than 90%.