Nano cellulose rubber reinforcing material

By adding antibacterial powder and adhesive plastic to nanocellulose, the problem of corrosion of nanocellulose rubber reinforcement materials in water and loss of antibacterial materials is solved, achieving good antibacterial performance and sustained effects.

CN118745266APending Publication Date: 2024-10-08HANGSHI TECH DEV (HANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411123621.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing nanocellulose rubber reinforcing materials lack antibacterial capabilities and are easily corroded by bacteria in water. When antibacterial materials are added, they are easily lost or cannot be evenly dispersed, resulting in a decline in rubber performance.

Method used

A combination of nanocellulose, antibacterial powder, dispersant and adhesive plastic is used. Through homogenization, heating and mixing followed by distillation treatment, the antibacterial powder is evenly dispersed in the nanocellulose by combining the adhesive plastic to enhance the antibacterial ability and reduce loss.

Benefits of technology

It effectively reduces the rate at which nanocellulose is corroded by bacteria, enhances the antibacterial ability of rubber, avoids the loss of antibacterial materials, and ensures the duration of the antibacterial effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745266A_ABST
    Figure CN118745266A_ABST
Patent Text Reader

Abstract

The invention discloses a nano-cellulose rubber reinforcing material, and relates to the technical field of nano-cellulose, and the nano-cellulose rubber reinforcing material is prepared by mixing nano-cellulose, antibacterial powder, a dispersant and adhesive plastic. According to the invention, the antibacterial powder is added into the nano-cellulose, so that the rate of corrosion of the nano-cellulose by bacteria can be effectively reduced, and the situation that the nano-cellulose in the rubber is degraded and the performance of the rubber is rapidly reduced when the nano-cellulose is added into the rubber can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanocellulose, in particular to a nanocellulose rubber reinforcement material. Background Art

[0002] Nanocellulose can be used as rubber reinforcement material. The traditional rubber reinforcement material is carbon black. Nanocellulose can be used as rubber reinforcement material to greatly reduce the use of carbon black. Nanocellulose is abundant in source and low in cost, so it can reduce the production cost of rubber.

[0003] The defects of existing nanocellulose are: 1. Prior art KR101550656B1 discloses a method for preparing nanocellulose. The nanocellulose does not have antibacterial ability. When nanocellulose is used as a reinforcing material for tire rubber, the rubber is easily corroded by bacteria in the water, thereby reducing the overall performance of the rubber. Therefore, a nanocellulose rubber reinforcing material with antibacterial ability is needed to solve this problem.

[0004] 2. The prior art KR101702576B1 discloses a method for preparing nanocellulose, which does not have antibacterial ability. When antibacterial materials are added to nanocellulose, the antibacterial materials are not connected to the nanocellulose, so the antibacterial materials are easily lost when the nanocellulose meets water. Therefore, a nanocellulose rubber reinforcement material that can reduce the loss of antibacterial materials is needed to solve this problem.

[0005] 3. Prior art CN105899455B discloses nanocellulose. The nanocellulose in this technology does not have antibacterial ability. When antibacterial material is added to the nanocellulose, if glue is used to bond the antibacterial material to the nanocellulose, the glue cannot be used in large quantities, so the antibacterial powder cannot be evenly dispersed and bonded in the nanocellulose material. Therefore, a method that can evenly disperse and bond the antibacterial material in the nanocellulose by glue is needed to solve this problem. Summary of the invention

[0006] One purpose of the present application is to provide a nanocellulose rubber reinforcement material that can solve the technical problems raised in the prior art.

[0007] To achieve the above object, the present invention provides the following technical solution: a nano-cellulose rubber reinforcing material, wherein the nano-cellulose rubber reinforcing material is a mixture of nano-cellulose, antibacterial powder, a dispersant and an adhesive plastic.

[0008] Preferably, the antibacterial powder is silver powder.

[0009] Preferably, the dispersant is one or more of triethylhexyl phosphate, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, and fatty acid polyethylene glycol esters.

[0010] Preferably, the weight ratio of the nanocellulose, antibacterial powder, dispersant and adhesive plastic is 100:(6-10):(1-5):(1-3).

[0011] Preferably, the preparation method of the nanocellulose is as follows: The wood pulp cellulose is homogenized by a homogenizer at a working pressure of 200 MPa for 20 to 30 times.

[0012] Preferably, the adhesive plastic is polyethylene or polypropylene.

[0013] Preferably, the preparation method of the nanocellulose rubber reinforcement material is as follows: S1, antibacterial powder, dispersant and adhesive plastic are placed in a mixing device with a heating structure, and then an organic solvent is added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 120-170° C., and the heating and stirring time is 20-40 minutes; S2, then adding the nanocellulose into the mixing device in step S1, and mixing the nanocellulose and the organic solvent in the mixing device for 20-40 minutes; S3. Then, the mixed solution obtained in step S2 is placed in a distillation device for distillation at a distillation temperature of 190-230° C., and the organic solvent in the mixed solution is distilled out to obtain a nano-cellulose rubber reinforcement material.

[0014] Preferably, the step S3 further includes the following steps: S31, cooling the nano-cellulose rubber reinforcement material in air, and after cooling to room temperature, grinding it into powder in a grinder.

[0015] Preferably, the organic solvent is one of ethanol, toluene, amyl acetate and trichloroethylene.

[0016] Preferably, the weight ratio of the nanocellulose to the organic solvent in step S1 and step S2 is 1:(1-2).

[0017] Compared with the prior art, the present invention has the following beneficial effects: The present invention can effectively reduce the rate at which nanocellulose is corroded by bacteria by adding antibacterial powder to nanocellulose, so that when the nanocellulose is added to rubber, the nanocellulose in the rubber can be prevented from being degraded and causing the rubber performance to drop rapidly, so that the nanocellulose rubber reinforcement material has antibacterial ability, and the nanocellulose in the rubber can be prevented from being degraded and causing the rubber performance to drop rapidly.

[0018] The present invention uses adhesive plastic to bond the antibacterial powder to the nanocellulose. By controlling the amount of the adhesive plastic, the antibacterial powder and the nanocellulose can be repeatedly bonded, while the antibacterial powder will not be covered by the adhesive plastic. Thus, the nanocellulose reinforcement material has antibacterial properties and the antibacterial powder is not easy to lose, and the antibacterial effect lasts for a long time.

[0019] The invention mixes the nano-cellulose material, antibacterial powder and adhesive plastic in an organic solvent, so that the antibacterial powder can be evenly dispersed in the nano-cellulose material, thereby preventing the adhesive plastic from being unable to be effectively dispersed in a large amount of nano-cellulose material due to its small amount. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a flow chart of the preparation method of the present invention. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] See also Figure 1 , a nanocellulose rubber reinforcement material, the nanocellulose rubber reinforcement material is a mixture of nanocellulose, antibacterial powder, dispersant and adhesive plastic.

[0023] The antibacterial powder is silver powder; The dispersant is one or more of triethylhexyl phosphate, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, and fatty acid polyethylene glycol esters; The weight ratio of nanocellulose, antibacterial powder, dispersant and adhesive plastic is 100: (6-10): (1-5): (1-3).

[0024] The preparation method of nanocellulose is as follows: The wood pulp cellulose is homogenized by a homogenizer at a working pressure of 200 MPa for 20 to 30 times.

[0025] The bonding plastic is polyethylene or polypropylene.

[0026] The preparation method of the nanocellulose rubber reinforcement material is as follows: S1, antibacterial powder, dispersant and adhesive plastic are placed in a mixing device with a heating structure, and then an organic solvent is added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 120-170° C., and the heating and stirring time is 20-40 minutes; S2, then adding the nanocellulose into the mixing device in step S1, and mixing the nanocellulose and the organic solvent in the mixing device for 20-40 minutes; S3. Then, the mixed solution obtained in step S2 is placed in a distillation device for distillation at a distillation temperature of 190-230° C., and the organic solvent in the mixed solution is distilled out to obtain a nano-cellulose rubber reinforcement material.

[0027] S3 also includes the following steps: S31, cooling the nano-cellulose rubber reinforcement material in air, and after cooling to room temperature, grinding it into powder in a grinder.

[0028] The organic solvent is one of ethanol, toluene, amyl acetate and trichloroethylene.

[0029] The weight ratio of nanocellulose to organic solvent in step S1 and step S2 is 1:(1-2). Example

[0030] 1. 6 parts of silver powder, 3 parts of methyl amyl alcohol and 2 parts of polyethylene are placed in a mixing device with a heating structure, and then 150 parts of ethanol are added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 140°C, and the heating and stirring time is 30 minutes; 2. Then, 100 parts of nanocellulose are added into the mixing device in step 1, and the mixing device mixes the nanocellulose and ethanol for 30 minutes; 3. Then, the mixed solution obtained in step 2 is placed in a distillation device for distillation at a distillation temperature of 190° C., and the ethanol in the mixed solution is distilled out to obtain a nanocellulose rubber reinforcement material.

[0031] Fourth, the nano-cellulose rubber reinforcement material is cooled in the air, and after cooling to room temperature, it is put into a grinder and ground into powder. Example

[0032] 1. 7 parts of silver powder, 3 parts of methyl amyl alcohol and 2 parts of polyethylene are placed in a mixing device with a heating structure, and then 150 parts of ethanol are added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 140°C, and the heating and stirring time is 30 minutes; 2. Then, 100 parts of nanocellulose are added into the mixing device in step 1, and the mixing device mixes the nanocellulose and ethanol for 30 minutes; 3. Then, the mixed solution obtained in step 2 is placed in a distillation device for distillation at a distillation temperature of 190° C., and the ethanol in the mixed solution is distilled out to obtain a nanocellulose rubber reinforcement material.

[0033] Fourth, the nano-cellulose rubber reinforcement material is cooled in the air, and after cooling to room temperature, it is put into a grinder and ground into powder. Example

[0034] 1. 8 parts of silver powder, 3 parts of methyl amyl alcohol and 2 parts of polyethylene are placed in a mixing device with a heating structure, and then 150 parts of ethanol are added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 140°C, and the heating and stirring time is 30 minutes; 2. Then, 100 parts of nanocellulose are added into the mixing device in step 1, and the mixing device mixes the nanocellulose and ethanol for 30 minutes; 3. Then, the mixed solution obtained in step 2 is placed in a distillation device for distillation at a distillation temperature of 190° C., and the ethanol in the mixed solution is distilled out to obtain a nanocellulose rubber reinforcement material.

[0035] Fourth, the nano-cellulose rubber reinforcement material is cooled in the air, and after cooling to room temperature, it is put into a grinder and ground into powder. Example

[0036] 1. 9 parts of silver powder, 3 parts of methyl amyl alcohol and 2 parts of polyethylene are placed in a mixing device with a heating structure, and then 150 parts of ethanol are added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 140°C, and the heating and stirring time is 30 minutes; 2. Then, 100 parts of nanocellulose are added into the mixing device in step 1, and the mixing device mixes the nanocellulose and ethanol for 30 minutes; 3. Then, the mixed solution obtained in step 2 is placed in a distillation device for distillation at a distillation temperature of 190° C., and the ethanol in the mixed solution is distilled out to obtain a nanocellulose rubber reinforcement material.

[0037] Fourth, the nano-cellulose rubber reinforcement material is cooled in the air, and after cooling to room temperature, it is put into a grinder and ground into powder. Example

[0038] 1. 10 parts of silver powder, 3 parts of methyl amyl alcohol and 2 parts of polyethylene are placed in a mixing device with a heating structure, and then 150 parts of ethanol are added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 140°C, and the heating and stirring time is 30 minutes; 2. Then, 100 parts of nanocellulose are added into the mixing device in step 1, and the mixing device mixes the nanocellulose and ethanol for 30 minutes; 3. Then, the mixed solution obtained in step 2 is placed in a distillation device for distillation at a distillation temperature of 190° C., and the ethanol in the mixed solution is distilled out to obtain a nanocellulose rubber reinforcement material.

[0039] Fourth, the nano-cellulose rubber reinforcement material is cooled in the air, and after cooling to room temperature, it is put into a grinder and ground into powder.

[0040] Performance Test: Antibacterial ability test: 500g of the product of each embodiment was taken and wrapped in cloth bags respectively, and then multiple cloth bags were placed in the same sewage at the same time. Then, after 10 hours, the multiple cloth bags were taken out at the same time and placed in different 1L clean water for 10 minutes, and then the multiple cloth bags were taken out at the same time again for drying, and then the weight of the multiple cloth bags was measured respectively. The comparative example was nanocellulose without adding antibacterial powder; Silver ion loss detection: add 0.2L of 68% nitric acid to the clean water in the antibacterial performance test, and then observe whether there is a white precipitate.

[0041] Test data of each embodiment under the same test conditions

[0042] It can be seen from the experimental data that the nanocellulose rubber reinforcement material produced by the present invention has good antibacterial properties, and because the antibacterial powder is bonded to the nanocellulose by bonding plastic polyethylene, etc., the antibacterial powder is lost slowly in water, which effectively prolongs the antibacterial duration of the nanocellulose reinforcement material.

[0043] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, from any point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention, and any reference signs in the claims should not be regarded as limiting the rights involved.

Claims

1. A nanocellulose rubber reinforcement material, characterized in that: The nano-cellulose rubber reinforcing material is prepared by mixing nano-cellulose, antibacterial powder, a dispersant and adhesive plastic.

2. The nanocellulose rubber reinforcing material according to claim 1, characterized in that: The antibacterial powder is silver powder.

3. The nanocellulose rubber reinforcing material according to claim 1, characterized in that: The dispersant is one or more of triethylhexyl phosphate, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, and fatty acid polyethylene glycol ester.

4. The nanocellulose rubber reinforcing material according to claim 1, characterized in that: The weight ratio of the nanocellulose, antibacterial powder, dispersant and adhesive plastic is 100:(6-10):(1-5):(1-3).

5. The nanocellulose rubber reinforcing material according to claim 1, characterized in that: The preparation method of the nanocellulose is as follows: The wood pulp cellulose is homogenized by a homogenizer at a working pressure of 200 MPa for 20 to 30 times.

6. The nanocellulose rubber reinforcing material according to claim 1, characterized in that: The adhesive plastic is polyethylene or polypropylene.

7. A method for preparing a nanocellulose rubber reinforcement material according to any one of claims 1 to 6, characterized in that: The preparation method of the nano-cellulose rubber reinforcement material is as follows: S1, antibacterial powder, dispersant and adhesive plastic are placed in a mixing device with a heating structure, and then an organic solvent is added into the mixing device, and then the mixing device is closed, and then the solution in the mixing device is heated to 120-170° C., and the heating and stirring time is 20-40 minutes; S2, then adding the nanocellulose into the mixing device in step S1, and mixing the nanocellulose and the organic solvent in the mixing device for 20-40 minutes; S3. Then, the mixed solution obtained in step S2 is placed in a distillation device for distillation at a distillation temperature of 190-230° C., and the organic solvent in the mixed solution is distilled out to obtain a nano-cellulose rubber reinforcement material.

8. The method for preparing a nanocellulose rubber reinforcement material according to claim 7, characterized in that: The S3 also includes the following steps: S31, cooling the nano-cellulose rubber reinforcement material in air, and after cooling to room temperature, grinding it into powder in a grinder.

9. The method for preparing a nanocellulose rubber reinforcement material according to claim 7, characterized in that: The organic solvent is one of ethanol, toluene, amyl acetate and trichloroethylene.

10. The method for preparing a nanocellulose rubber reinforcement material according to claim 7, characterized in that: The weight ratio of the nanocellulose to the organic solvent in step S1 and step S2 is 1:(1-2).