Composite functional master batch based on functional modifier, preparation method of composite functional master batch and application of composite functional master batch in plastic plates

By using micro-nano calcite powder, wollastonite short fibers and chopped glass fibers in functional modifiers in plastic sheets, combined with surface activation and pre-dispersion treatment technology, a high-performance composite functional masterbatch is prepared to solve the current problem. In order to solve the problem of insufficient mechanical properties of plastic sheets in the technology, significant performance improvement and cost reduction have been achieved.

CN118745268APending Publication Date: 2024-10-08JIANGXI HONGYI POLYMERIC MATERIALS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410963866.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

There is no report in the prior art on a method for preparing a high-performance composite functional masterbatch based on a functional modifier that is universally applicable to various plastic sheets, resulting in insufficient mechanical properties of the plastic sheets.

Method used

Provides a composite functional masterbatch based on functional modifiers, including micro-nano calcite powder, wollastonite short fibers and chopped glass fibers. Through surface activation treatment and pre-dispersion treatment, it is combined with a coupling agent and a dispersant to form High-performance composite functional masterbatch, suitable for plastic sheets with different resins.

Benefits of technology

It significantly improves the tensile strength, impact strength and bending performance of plastic sheets, reduces costs, and improves the compatibility and performance of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745268A_ABST
    Figure CN118745268A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional materials, and provides a composite functional master batch based on a functional modifier, a preparation method of the composite functional master batch and application of the composite functional master batch in plastic plates. The composite functional master batch comprises a functional modifier, a flexibilizer, a coupling agent, a dispersant, an antioxidant and a stabilizer in specific parts by mass. The functional modifier comprises micro-nano calcite powder, wollastonite short fibers and chopped glass fibers. The functional modifier is used as a reinforcing material, and the high-performance composite functional master batch with reinforcing and toughening effects is obtained by virtue of a particle toughening mechanism of micro-nano calcite powder in the functional modifier and a toughening mechanism of pulling out, debonding and fiber bridging of wollastonite short fibers and chopped glass fibers. The method is universal for plastic plates made of various resins, the cost of the plastic plates is greatly reduced, and meanwhile, the tensile strength, the impact strength, the bending property and other mechanical properties of the plastic plates can be obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional materials, and in particular to a composite functional masterbatch based on a functional modifier, a preparation method thereof, and application of the composite functional masterbatch in plastic sheets. Background Art

[0002] Plastic sheets are sheets made of plastic. There are many types of plastic sheets, which can be roughly divided into: PE sheets, PP sheets, PS sheets, HIPS sheets, PVC sheets, ABS sheets, PET sheets, PBT sheets, PMMA sheets, PC sheets, PETG sheets, MC sheets, PSU sheets, PEEK sheets, POM sheets, PVDF sheets, PCB sheets, GPPS sheets, APET sheets, composite sheets, carved sheets, PVC foam sheets, plastic rattan sheets, and imitation wood plastic sheets. The production methods of plastic sheets include: extrusion, calendering, lamination, and casting. Extrusion and calendering are continuous production processes, while other methods are intermittent production processes.

[0003] Before plastic sheet molding, in order to meet the requirements of product molding process and performance, it is necessary to select appropriate resins and auxiliary materials such as additives with certain functions, design the formula, and prepare them into molding materials. Common additives include plasticizers, stabilizers, antioxidants, lubricants, fillers, colorants, curing agents, foaming agents, flame retardants, antistatic agents, etc. Additives are usually added for two purposes. One is to improve the molding processability of plastics; the other is to change the performance of plastic products. The specific types and amounts of additives added during the preparation process are determined by the use requirements of the plastics and the molding process.

[0004] The Chinese patent with publication number CN 105365190 introduces a PP raw material sheet processing technology, including: feeding; using a single screw extruder, the extrusion barrel is heated in four zones; evaporating the water contained in the PP raw material and timely removing it through the exhaust holes set on the barrel; forming and shaping into a sheet in the extrusion mold. The Chinese patent with publication number CN 117362832A introduces a high-toughness and high-filling PP sheet preparation process and application. The high-toughness and high-filling PP sheet includes the following components: PP, linear low-density polyethylene, modified heavy calcium carbonate, nano calcium carbonate, polyolefin elastomer, coupling agent, lubricant, antioxidant, glass fiber, light stabilizer, hyperbranched epoxy resin, silicone epoxy modified acrylic resin, etc.; the prepared high-toughness and high-filling PP sheet has many advantages such as non-toxic and tasteless, low water absorption, dimensional stability, heat resistance, friction resistance, corrosion resistance, shrinkage resistance, strong impact resistance, and not easy to deform. The Chinese patent with publication number CN 215722458 U introduces a high-strength PP plate. The high-strength PP plate adopts a PP plate body designed with protrusions and grooves, and the protrusions and grooves are respectively located on both sides of the PP plate body. When the components are inserted, the protrusions and grooves are connected to seal the two adjacent PP plate bodies; the practicality and flexibility of the PP plate body are improved, the difficulty of construction is reduced, the sealing effect can be improved, and the service life of the equipment can be extended.

[0005] At present, there is no report on the preparation method of high-performance composite functional masterbatch based on functional modifier and toughening agent that is applicable to various plastic sheets. Therefore, it is of great significance to study and obtain a composite functional masterbatch based on functional modifier so that it can be applied to various plastic sheets. Summary of the invention

[0006] The object of the present invention is to provide a composite functional masterbatch based on a functional modifier and a preparation method thereof and application in plastic sheets in view of the deficiencies in the prior art.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a composite functional masterbatch based on a functional modifier, wherein the composite functional masterbatch comprises the following raw materials in parts by weight: 45 to 85 parts of a functional modifier, 10 to 50 parts of a toughening agent, 1 to 3.5 parts of a coupling agent, 1.5 to 4.5 parts of a dispersant, 0.001 to 0.005 parts of an antioxidant, and 0.001 to 0.005 parts of a stabilizer;

[0009] The functional modifier comprises micro-nano calcite powder, wollastonite short fibers and chopped glass fibers, and the mass ratio of the micro-nano calcite powder, wollastonite short fibers and chopped glass fibers is 30-50:20-35:8-35.

[0010] Preferably, the toughening agent comprises one or more of ethylene-vinyl acetate copolymer, styrene-butadiene-styrene thermoplastic elastomer, methyl methacrylate-butadiene-styrene terpolymer, acrylonitrile-butadiene-styrene copolymer, chlorinated polyethylene and random polypropylene;

[0011] The coupling agent is one or more of a silane coupling agent, a titanate coupling agent and an aluminate coupling agent; the silane coupling agent comprises one or more of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane; the titanate coupling agent is one or more of triisostearate isopropyl titanate, a compound of triisostearate isopropyl titanate and isopropyl trioleate acyloxy titanate; the aluminate coupling agent is isopropoxy distearate acyloxy aluminate.

[0012] Preferably, the dispersant is low molecular weight ethylene-vinyl acetate copolymer wax and polyolefin wax, the mass ratio of low molecular weight ethylene-vinyl acetate copolymer wax and polyolefin wax is 1-2:1-2; the polyolefin wax is low molecular weight polypropylene wax or low molecular weight polyethylene wax; the number average molecular weight of the dispersant is 4000-8000.

[0013] Preferably, the antioxidant is a compound of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite; the compound is Irganox B215 or Irganox B225;

[0014] The stabilizer is poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate or poly{6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-bis[(2,2,6,6-tetramethylpiperidinyl)imino]-1,6-hexadiene[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}.

[0015] Preferably, the mesh sizes of the micro-nano calcite powder and wollastonite short fibers are independently 800-5000 meshes, and the diameter of the chopped glass fibers is 10-13 μm and the length is 3-4.5 mm.

[0016] The present invention also provides a method for preparing the composite functional masterbatch based on the functional modifier, comprising the following steps:

[0017] 1) performing surface activation treatment on the functional modifier and the coupling agent to obtain an activated functional modifier;

[0018] 2) pre-dispersing the activated functional modifier and the dispersant to obtain a pre-dispersed activated functional modifier;

[0019] 3) The pre-dispersed activated functional modifier, toughening agent, antioxidant and stabilizer are mixed and then plasticized, mixed, extruded and granulated in sequence to obtain a composite functional masterbatch.

[0020] Preferably, the surface activation treatment in step 1) is a dry surface activation treatment, the time of the surface activation treatment is based on the activation degree of the functional modifier reaching 100%, and the temperature of the surface activation treatment is 100-120°C;

[0021] The temperature of the pre-dispersion treatment in step 2) is 80-130° C., and the time of the pre-dispersion treatment is 3-10 minutes; and the mixing time in step 3) is 3-10 minutes.

[0022] Preferably, in the process of plasticizing, mixing, extruding and granulating in step 3), the temperature is 110-230° C. and the rotation speed is 200-500 rpm;

[0023] The rotation speeds of the surface activation treatment in step 1), the pre-dispersion treatment in step 2) and the mixing in step 3) are independently 930 to 1030 rpm.

[0024] The present invention also provides a plastic sheet comprising the composite functional masterbatch based on the functional modifier, wherein the plastic sheet comprises the composite functional masterbatch based on the functional modifier and resin; in the plastic sheet, the mass fraction of the composite functional masterbatch based on the functional modifier is 10 to 80%.

[0025] The beneficial effects of the present invention include the following:

[0026] 1) The present invention uses micro-nano calcite powder, wollastonite short fibers and chopped glass fibers in the functional modifier as reinforcing materials, and relies on the particle toughening mechanism of the micro-nano calcite powder in the functional modifier and the pulling out, debonding and fiber bridging toughening mechanisms of the wollastonite short fibers and chopped glass fibers to obtain a high-performance composite functional masterbatch with enhanced toughening effects. The high-performance composite functional masterbatch of the present invention is generally applicable to plastic sheets made of various resins, thereby obtaining high-performance plastic sheets. While significantly reducing the cost of plastic sheets, the mechanical properties of the plastic sheets, such as tensile strength, impact strength and bending performance, can be significantly improved.

[0027] 2) The present invention uses a functional modifier as a reinforcing and toughening material, and adopts a coupling agent to perform dry surface activation treatment on the functional modifier. According to the surface wetting theory and the chemical bond theory, the method of dry surface activation is that the coupling agent is uniformly applied to the surface of the filler powder particles by high-speed mixing and a certain temperature in a dry state to form an extremely thin surface treatment layer; the coupling agent is a kind of substance with an amphoteric group structure, which combines with the filler surface at one end and entangles or reacts with the polymer resin at the other end through chemical reaction or physicochemical action, so that the inorganic filler and the polymer with different surface properties are firmly combined, thereby improving the dispersion state of the inorganic filler in the polymer matrix, improving the compatibility and the mechanical properties and performance of the filled polymer.

[0028] 3) According to the strengthening and toughening principle of the toughening agent, the high-performance composite functional masterbatch based on the functional modifier prepared by the present invention is also suitable for application fields such as sheets, pipes, various injection molded parts, extruded parts, rotational molded parts, etc. made of resins of different materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a SEM image of the composite functional masterbatch of Example 1 in a polypropylene plastic sheet. DETAILED DESCRIPTION

[0030] The present invention provides a composite functional masterbatch based on a functional modifier, wherein the composite functional masterbatch comprises the following raw materials in parts by weight: 45 to 85 parts of a functional modifier, 10 to 50 parts of a toughening agent, 1 to 3.5 parts of a coupling agent, 1.5 to 4.5 parts of a dispersant, 0.001 to 0.005 parts of an antioxidant, and 0.001 to 0.005 parts of a stabilizer;

[0031] The functional modifier comprises micro-nano calcite powder, wollastonite short fibers and chopped glass fibers, and the mass ratio of the micro-nano calcite powder, wollastonite short fibers and chopped glass fibers is 30-50:20-35:8-35.

[0032] In the present invention, the raw materials for preparing the composite functional masterbatch contain 45 to 85 parts of the functional modifier, preferably 50 to 80 parts, more preferably 55 to 75 parts, and even more preferably 60 to 70 parts.

[0033] In the present invention, the functional modifier preferably comprises micro-nano calcite powder, wollastonite short fibers and chopped glass fibers, and the mass ratio of micro-nano calcite powder, wollastonite short fibers and chopped glass fibers is preferably 32-45:23-32:10-30, and more preferably 35-40:24-30:16-24.

[0034] In the present invention, the mesh sizes of the micro-nano calcite powder and wollastonite short fibers are independently preferably 800-5000 meshes, more preferably 1000-4000 meshes, and more preferably 2000-3000 meshes; the diameter of the chopped glass fibers is preferably 10-13 μm, more preferably 11-12 μm, and more preferably 11.5 μm, and the length of the chopped glass fibers is preferably 3-4.5 mm, and more preferably 3.5-4 mm.

[0035] In the present invention, the functional modifier is preferably a dry functional modifier. When the functional modifier contains water, the functional modifier is preferably dried; the temperature of the drying treatment is preferably 100-120°C, more preferably 105-115°C, and more preferably 110°C; the drying treatment is preferably carried out in a high-speed mixer.

[0036] In the present invention, the raw materials for preparing the composite functional masterbatch contain 10 to 50 parts of toughening agent, preferably 15 to 45 parts, more preferably 20 to 40 parts, and more preferably 25 to 30 parts.

[0037] In the present invention, the toughening agent preferably comprises one or more of ethylene-vinyl acetate copolymer (EVA), styrene-butadiene-styrene thermoplastic elastomer (SBS), methyl methacrylate-butadiene-styrene terpolymer (MBS), acrylonitrile-butadiene-styrene copolymer (ABS), chlorinated polyethylene (CPE) and random polypropylene, and further preferably comprises ethylene-vinyl acetate copolymer (EVA) and random polypropylene. The mass ratio of EVA to random polypropylene is preferably 1 to 3:1, and more preferably 2:1.

[0038] Toughening of polymers is to change the fracture mode of polymers from brittle fracture to tough fracture, so that the polymers have a higher elongation at break when stretched, are less likely to be damaged when impacted, and can absorb more fracture energy once damaged. The toughening agent of the present invention has good compatibility with other polymer resins, so the high-performance composite functional masterbatch based on the functional modifier can be used for plastic sheets of different resin materials.

[0039] In the present invention, the raw materials for preparing the composite functional masterbatch contain 1 to 3.5 parts of coupling agent, preferably 1.5 to 3.2 parts, more preferably 2 to 3 parts, and more preferably 2.5 parts.

[0040] In the present invention, the coupling agent is preferably one or more of a silane coupling agent, a titanate coupling agent and an aluminate coupling agent; the silane coupling agent preferably comprises one or more of γ-aminopropyltriethoxysilane (silane coupling agent KH-550), γ-(2,3-epoxypropoxy)propyltrimethoxysilane (silane coupling agent KH-560) and γ-methacryloxypropyltrimethoxysilane (silane coupling agent KH-570); the titanate coupling agent is preferably one or more of isopropyl triisostearate titanate, a compound of isopropyl triisostearate titanate and isopropyl trioleate acyloxy titanate; the aluminate coupling agent is preferably isopropoxy distearate acyloxy aluminate.

[0041] In the present invention, the raw materials for preparing the composite functional masterbatch contain 1.5 to 4.5 parts of dispersant, preferably 2 to 4 parts, more preferably 2.5 to 3.5 parts, and more preferably 3 parts.

[0042] In the present invention, the dispersant is preferably a low molecular weight ethylene-vinyl acetate copolymer wax (EVA wax) and a polyolefin wax, and the mass ratio of the low molecular weight ethylene-vinyl acetate copolymer wax to the polyolefin wax is preferably 1 to 2: 1 to 2, and more preferably 1: 1; the polyolefin wax is preferably a low molecular weight polypropylene wax or a low molecular weight polyethylene wax; the number average molecular weight of the dispersant is preferably 4000 to 8000, more preferably 5000 to 7000, and more preferably 6000.

[0043] In the present invention, the raw materials for preparing the composite functional masterbatch contain 0.001 to 0.005 parts of antioxidant, preferably 0.002 to 0.004 parts, and more preferably 0.003 parts.

[0044] In the present invention, the antioxidant is preferably a compound of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1010) and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168); the compound is preferably Irganox B215 or Irganox B225.

[0045] In the present invention, the raw materials for preparing the composite functional masterbatch contain 0.001 to 0.005 parts of stabilizer, preferably 0.002 to 0.004 parts, and more preferably 0.003 parts.

[0046] In the present invention, the stabilizer is preferably poly (4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate (light stabilizer 622), bis (2,2,6,6-tetramethyl-4-piperidinyl) sebacate (light stabilizer 770) or poly {6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-bis[(2,2,6,6-tetramethylpiperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]} (light stabilizer 944).

[0047] In the present invention, the particle size of the composite functional masterbatch is preferably Φ3×3-4mm, more preferably Φ3×3.5mm; the water content is preferably ≤0.2%, more preferably ≤0.15%; the whiteness value is preferably ≥94%, more preferably ≥95%.

[0048] The present invention also provides a method for preparing the composite functional masterbatch based on the functional modifier, comprising the following steps:

[0049] 1) performing surface activation treatment on the functional modifier and the coupling agent to obtain an activated functional modifier;

[0050] 2) pre-dispersing the activated functional modifier and the dispersant to obtain a pre-dispersed activated functional modifier;

[0051] 3) The pre-dispersed activated functional modifier, toughening agent, antioxidant and stabilizer are mixed and then plasticized, mixed, extruded and granulated in sequence to obtain a composite functional masterbatch.

[0052] In the present invention, the coupling agent in step 1) is preferably added in the form of a coupling agent solution, the coupling agent solution comprises a coupling agent and liquid paraffin, and the mass ratio of the coupling agent to the liquid paraffin is preferably 1-2:1-2, more preferably 1:1.

[0053] In the present invention, the surface activation treatment in step 1) is preferably a dry surface activation treatment, the time of the surface activation treatment is preferably based on the activation degree of the functional modifier reaching 100%, and the temperature of the surface activation treatment is preferably 100-120° C., more preferably 105-115° C., and more preferably 110° C.;

[0054] The temperature of the pre-dispersion treatment in step 2) is preferably 80-130°C, more preferably 90-120°C, and more preferably 100-110°C; the time of the pre-dispersion treatment is preferably 3-10 min, more preferably 5-8 min, and more preferably 6-7 min; the time of the mixing in step 3) is preferably 3-10 min, more preferably 5-8 min, and more preferably 6-7 min.

[0055] In the present invention, after the pre-dispersion treatment is completed, the obtained material is preferably cooled to room temperature to obtain a pre-dispersed activated functional modifier.

[0056] In the present invention, the plasticizing, mixing, extruding and granulating in step 3) are preferably carried out in a twin-screw extruder, and the temperature of each zone of the twin-screw extruder is preferably 110-230°C, more preferably 100-120°C in zone 1, 180-200°C in zone 2, 190-220°C in zone 3, 190-220°C in zone 4, 200-220°C in zone 5, 200-220°C in zone 6, 200-220°C in zone 7, 200-220°C in zone 8. The temperature of the first zone is 110-115°C, the second zone is 190-193°C, the third zone is 195-200°C, the fourth zone is 200-210°C, the fifth zone is 210-212°C, the sixth zone is 210-215°C, the seventh zone is 210-215°C, the eighth zone is 215-220°C, the ninth zone is 215-220°C, and the head is 215-220°C.

[0057] In the present invention, the feeding speed is preferably 20 to 30 rpm, more preferably 22 to 28 rpm, and more preferably 25 to 26 rpm; the rotation speed of the extruder is preferably 200 to 500 rpm, more preferably 300 to 400 rpm, and more preferably 320 to 350 rpm.

[0058] In the present invention, the surface activation treatment in step 1), the pre-dispersion treatment in step 2) and the mixing in step 3) are preferably carried out in a high-speed mixer, and the rotation speed of the high-speed mixer is independently preferably 930 to 1030 rpm, more preferably 950 to 1000 rpm, and more preferably 970 to 980 rpm.

[0059] In the present invention, the functional modifier with surface hydrophilicity is changed to organic through dry surface activation treatment, which can improve the coupling between the polymer resin molecular chain and the functional modifier particles, so that the functional modifier particles can be evenly dispersed in the polymer resin; in addition, the surface energy of the functional modifier particles can be reduced, the van der Waals force between the particles is reduced, and new steric repulsion is generated, thereby preventing the particles from agglomerating, and further improving the dispersibility of the functional modifier particles.

[0060] In the present invention, the dispersant has a low molecular weight, good flowability and good compatibility with the polymer resin; adding the dispersant to the activated functional modifier can make the activated functional modifier produce the effects of wetting, dispersion and stabilization, and the particles thereof are less likely to "agglomerate" with each other; at the same time, the activated functional modifier treated with the dispersant and other additives are "fused" together under the full kneading action of the twin-screw extruder, thereby improving the overall dispersibility and the performance of the functional masterbatch.

[0061] The present invention also provides a plastic sheet comprising the composite functional masterbatch based on the functional modifier, wherein the plastic sheet comprises the composite functional masterbatch based on the functional modifier and resin; in the plastic sheet, the mass fraction of the composite functional masterbatch based on the functional modifier is 10 to 80%.

[0062] In the plastic sheet of the present invention, the mass fraction of the composite functional masterbatch based on the functional modifier is preferably 20 to 70%, more preferably 30 to 60%, and even more preferably 40 to 50%.

[0063] In the present invention, the resin is a resin of different materials that can be used to prepare plastic sheets, and the type of the resin is determined according to the needs of the plastic sheets.

[0064] In the present invention, the preparation method of the plastic sheet is a preparation method well known in the art, and the composite functional masterbatch based on the functional modifier and the resins of different materials are uniformly mixed and then prepared according to the conventional preparation method of the plastic sheet.

[0065] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0066] In the embodiment, the micro-nano calcite powder is CC-2500 with a mesh size of 2500, which is from Jiangxi Guangyuan Chemical Co., Ltd.; the wollastonite short fiber is GY-2000 with a mesh size of 2000 and an aspect ratio of 10:1, which is from Jiangxi Guangyuan Chemical Co., Ltd.; the chopped glass fiber is 508A-E with a length of 3 mm and a diameter of 10 μm, which is from China Jushi Co., Ltd.; the coupling agent is from Yizheng Tianyang Chemical Co., Ltd.; the molecular weight of the low molecular weight ethylene-vinyl acetate copolymer wax (EVA wax) is 6000, the molecular weight of the low molecular weight polypropylene wax is 4000, and the molecular weight of the low molecular weight polyethylene wax is 4000, and the low molecular weight ethylene-vinyl acetate copolymer wax, the low molecular weight polypropylene wax and the low molecular weight polyethylene wax are all from Changzhou Branch of Qingdao Bonnie Chemical Co., Ltd.; other raw materials are conventional raw materials in the field.

[0067] Example 1

[0068] 40 parts by mass of micro-nano calcite powder, 24 parts of wollastonite short fibers, and 16 parts of chopped glass fibers were mixed and placed in a high-speed mixer, heated to 110°C, stirred at a speed of 490 rpm, and then stirred at a speed of 980 rpm for 3 minutes to discharge water, and the stirring was temporarily stopped. γ-aminopropyltriethoxysilane dilution (2.4 parts of KH-550, and the mass ratio of γ-aminopropyltriethoxysilane to liquid paraffin in the KH-550 dilution was 1:1) was added, and then stirring was continued at 110°C and stirred at a speed of 980 rpm for 8 minutes to obtain an activated functional modifier with an activation degree of 100%.

[0069] 1.5 parts of low molecular weight ethylene-vinyl acetate copolymer wax and 1.5 parts of low molecular weight polypropylene wax were added to a high-speed mixer, and pre-dispersed with the activated functional modifier at 110° C. and 980 rpm for 5 minutes, and then the material was naturally cooled to room temperature to obtain a pre-dispersed activated functional modifier.

[0070] Toughener, antioxidant and stabilizer were added to the pre-dispersed activated functional modifier. Toughener was 10 parts of EVA and 4.5 parts of random polypropylene (average molecular weight 5000); antioxidant was 0.002 parts of Irganox B225; stabilizer was 0.001 parts of light stabilizer 770, and the mixture was stirred at 980rpm in a high-speed mixer for 10 minutes. Then it was fed into a twin-screw extruder for plasticization, mixing, extrusion and granulation to obtain a composite functional masterbatch based on functional modifier. Among them, the temperature ranges of the twin-screw extruder were: 115℃ in zone 1, 193℃ in zone 2, 195℃ in zone 3, 210℃ in zone 4, 212℃ in zone 5, 215℃ in zone 6, 215℃ in zone 7, 220℃ in zone 8, 220℃ in zone 9, and 220℃ in die head; the feeding speed was 26rpm, and the extruder speed was 320rpm.

[0071] The composite functional masterbatch based on the functional modifier in this embodiment has a particle size of Φ3×3.5 mm, a water content of 0.15%, and a whiteness value of 95%.

[0072] Example 2

[0073] 32 parts by mass of micro-nano calcite powder, 24 parts of wollastonite short fibers, and 24 parts of chopped glass fibers were mixed and placed in a high-speed mixer, heated to 110°C, stirred at a speed of 490 rpm, and then stirred at a speed of 950 rpm for 3 minutes to discharge water, and the stirring was temporarily stopped. Triisostearate isopropyl titanate dilution (triisostearate isopropyl titanate is 2.0 parts, and the mass ratio of triisostearate isopropyl titanate to liquid paraffin in the dilution is 1:1) was added, and then stirring was continued at 110°C and stirred at a speed of 950 rpm for 8 minutes to obtain an activated functional modifier with an activation degree of 100%.

[0074] 1.5 parts of low molecular weight ethylene-vinyl acetate copolymer wax and 1.5 parts of low molecular weight polypropylene wax were added to a high-speed mixer, and pre-dispersed with the activated functional modifier at 110° C. and 950 rpm for 8 minutes, and then the material was naturally cooled to room temperature to obtain a pre-dispersed activated functional modifier.

[0075] Toughener, antioxidant and stabilizer were added to the pre-dispersed activated functional modifier. Toughener was 9 parts EVA and 6 parts random polypropylene (average molecular weight 7000); antioxidant was 0.001 parts Irganox B225; stabilizer was 0.001 parts light stabilizer 622, and the mixture was stirred at 950rpm in a high-speed mixer for 10min. Then it was fed into a twin-screw extruder for plasticization, mixing, extrusion and granulation to obtain a composite functional masterbatch based on functional modifier. Among them, the temperature ranges of the twin-screw extruder were: 115℃ in zone 1, 193℃ in zone 2, 195℃ in zone 3, 210℃ in zone 4, 212℃ in zone 5, 215℃ in zone 6, 215℃ in zone 7, 220℃ in zone 8, 220℃ in zone 9, and 220℃ in die head; the feeding speed was 26rpm, and the extruder speed was 320rpm.

[0076] The composite functional masterbatch based on the functional modifier in this embodiment has a particle size of Φ3×3.3 mm, a water content of 0.18%, and a whiteness value of 94%.

[0077] Example 3

[0078] 40 parts by mass of micro-nano calcite powder, 32 parts of wollastonite short fibers, and 8 parts of chopped glass fibers are mixed and placed in a high-speed mixer, heated to 110°C, stirred at a speed of 490rpm, and then stirred at a speed of 1000rpm for 3min to discharge water, and the stirring is temporarily stopped. An isopropoxy distearate acyloxyaluminate dilution (2.6 parts of isopropoxy distearate acyloxyaluminate, and the mass ratio of isopropoxy distearate acyloxyaluminate to liquid paraffin in the isopropoxy distearate acyloxyaluminate dilution is 1:1) is added, and then stirring is continued at 110°C and 1000rpm for 8min to obtain an activated functional modifier with an activation degree of 100%.

[0079] 1.5 parts of low molecular weight ethylene-vinyl acetate copolymer wax and 1.5 parts of low molecular weight polypropylene wax were added to a high-speed mixer, and pre-dispersed with the activated functional modifier at 110° C. and 1000 rpm for 5 minutes, and then the material was naturally cooled to room temperature to obtain a pre-dispersed activated functional modifier.

[0080] Toughener, antioxidant and stabilizer were added to the pre-dispersed activated functional modifier. The toughener was 14.6 parts of EVA; the antioxidant was 0.002 parts of Irganox B215; the stabilizer was 0.002 parts of light stabilizer 944, and the mixture was stirred at 1000rpm for 5 minutes in a high-speed mixer. Then it was fed into a twin-screw extruder for plasticization, mixing, extrusion and granulation to obtain a composite functional masterbatch based on functional modifiers. Among them, the temperature ranges of the twin-screw extruder were: 115℃ in zone 1, 193℃ in zone 2, 195℃ in zone 3, 210℃ in zone 4, 212℃ in zone 5, 215℃ in zone 6, 215℃ in zone 7, 220℃ in zone 8, 220℃ in zone 9, and 220℃ in die head; the feeding speed was 26rpm, and the extruder speed was 320rpm.

[0081] The composite functional masterbatch based on the functional modifier in this embodiment has a particle size of Φ3×3.7 mm, a water content of 0.2%, and a whiteness value of 95%.

[0082] The composite functional masterbatch based on the functional modifier of Example 1 and polypropylene resin are used to prepare a polypropylene plastic sheet sample. In the plastic sheet, the mass fraction of the polypropylene resin is 70%, and the mass fraction of the composite functional masterbatch is 30%. The SEM image of the composite functional masterbatch of Example 1 in the polypropylene plastic sheet is as follows: Figure 1 shown.

[0083] The composite functional masterbatches of Examples 1 to 3 were respectively prepared with polypropylene resin to form polypropylene plastic sheet samples, while Comparative Example 1 only contained polypropylene resin and did not contain the composite functional masterbatch. The samples of the Examples and Comparative Examples were subjected to mechanical property tests, and the mass content of each raw material in the samples and the mechanical property test results were shown in Table 1; the composite functional masterbatch of Example 1 and different resins were prepared into plastic sheet samples, while the Comparative Examples only contained different resins and did not contain the composite functional masterbatch. The samples of Example 1 and Comparative Example 1 were subjected to mechanical property tests, and the mass content of each raw material in the samples and the mechanical property test results were shown in Table 2; wherein the tensile properties were measured in accordance with GB / T 1040-2006; the bending properties were measured in accordance with GB / T 9341-2006; and the notched impact strength was measured in accordance with GB / T 1040-2006.

[0084] Table 1 Mass content of each raw material in the examples and comparative examples and mechanical properties of the samples

[0085]

[0086]

[0087] Table 2 The mass content of each raw material in the samples of Example 1 and Comparative Example 1 and the mechanical properties of the samples

[0088]

[0089]

[0090] It can be seen from Table 1 and Table 2 that the high-performance composite functional masterbatch prepared by the present invention has good strengthening and toughening effects while effectively reducing the cost of raw materials, and significantly improves the mechanical properties of plastic sheets.

[0091] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A composite functional masterbatch based on a functional modifier, characterized in that: The composite functional masterbatch comprises the following raw materials in parts by weight: 45-85 parts of functional modifier, 10-50 parts of toughening agent, 1-3.5 parts of coupling agent, 1.5-4.5 parts of dispersant, 0.001-0.005 parts of antioxidant, and 0.001-0.005 parts of stabilizer; The functional modifier comprises micro-nano calcite powder, wollastonite short fibers and chopped glass fibers, and the mass ratio of the micro-nano calcite powder, wollastonite short fibers and chopped glass fibers is 30-50:20-35:8-35.

2. The composite functional masterbatch based on the functional modifier according to claim 1, characterized in that: The toughening agent comprises one or more of ethylene-vinyl acetate copolymer, styrene-butadiene-styrene thermoplastic elastomer, methyl methacrylate-butadiene-styrene terpolymer, acrylonitrile-butadiene-styrene copolymer, chlorinated polyethylene and random polypropylene; The coupling agent is one or more of a silane coupling agent, a titanate coupling agent and an aluminate coupling agent; the silane coupling agent comprises one or more of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane; the titanate coupling agent is one or more of triisostearate isopropyl titanate, a compound of triisostearate isopropyl titanate and isopropyl trioleate acyloxy titanate; the aluminate coupling agent is isopropoxy distearate acyloxy aluminate.

3. The composite functional masterbatch based on the functional modifier according to claim 1 or 2, characterized in that: The dispersant is low molecular weight ethylene-vinyl acetate copolymer wax and polyolefin wax, the mass ratio of low molecular weight ethylene-vinyl acetate copolymer wax to polyolefin wax is 1-2:1-2; the polyolefin wax is low molecular weight polypropylene wax or low molecular weight polyethylene wax; the number average molecular weight of the dispersant is 4000-8000.

4. The composite functional masterbatch based on the functional modifier according to claim 3, characterized in that: The antioxidant is a compound of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite; the compound is Irganox B215 or Irganox B225; The stabilizer is poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate or poly{6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-bis[(2,2,6,6-tetramethylpiperidinyl)imino]-1,6-hexadiene[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}.

5. The composite functional masterbatch based on the functional modifier according to claim 1 or 4, characterized in that: The mesh numbers of the micro-nano calcite powder and wollastonite short fibers are independently 800-5000 meshes, the diameter of the short glass fibers is 10-13 μm, and the length is 3-4.5 mm.

6. The method for preparing a composite functional masterbatch based on a functional modifier according to any one of claims 1 to 5, characterized in that: The following steps are included: 1) performing surface activation treatment on the functional modifier and the coupling agent to obtain an activated functional modifier; 2) pre-dispersing the activated functional modifier and the dispersant to obtain a pre-dispersed activated functional modifier; 3) The pre-dispersed activated functional modifier, toughening agent, antioxidant and stabilizer are mixed and then plasticized, mixed, extruded and granulated in sequence to obtain a composite functional masterbatch.

7. The preparation method according to claim 6, characterized in that: Step 1) The surface activation treatment is a dry surface activation treatment, the surface activation treatment time is based on the activation degree of the functional modifier reaching 100%, and the surface activation treatment temperature is 100-120°C; The temperature of the pre-dispersion treatment in step 2) is 80-130° C., and the time of the pre-dispersion treatment is 3-10 minutes; and the mixing time in step 3) is 3-10 minutes.

8. The preparation method according to claim 6 or 7, characterized in that: Step 3) During the plasticizing, mixing, extruding and granulating process, the temperature is 110-230° C. and the rotation speed is 200-500 rpm; The rotation speeds of the surface activation treatment in step 1), the pre-dispersion treatment in step 2) and the mixing in step 3) are independently 930 to 1030 rpm.

9. Application of the composite functional masterbatch based on the functional modifier according to any one of claims 1 to 5 in plastic sheets, characterized in that: The plastic sheet comprises a composite functional masterbatch based on a functional modifier and a resin; in the plastic sheet, the mass fraction of the composite functional masterbatch based on a functional modifier is 10 to 80%.

Citation Information

Patent Citations

  • Polymer master batch with good dispersibility and its production method and application

    CN101429686A

  • Functional master batch for reinforcing and toughening polylactic acid fibers and preparation method thereof and reinforcing and toughening polylactic acid material

    CN111534066A

  • Antibacterial dust-adsorption-resistant composite plastic master batch and preparation method thereof

    CN113372588A

  • Multifunctional filling modified polypropylene master batch as well as preparation method and application thereof

    CN115772296A