Putty composition as well as preparation method and application thereof
By using a combination of phosphate dispersant, polycarboxylic acid wetting agent and nano-inorganic fiber in putty powder, the problems of clogging, segregation and sagging of putty powder during robot construction are solved, and the construction efficiency and surface smoothness are improved. It is suitable for Intelligent construction.
Patent Information
- Application Number
- CN202410894581.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-08
AI Technical Summary
Existing putty powder products are prone to problems such as clogging of nozzles, segregation, and sagging during robot construction, and the surface after spraying is rough and uneven, making it difficult to meet the needs of intelligent construction.
Phosphate dispersant and polycarboxylic acid wetting agent are used, combined with nano-inorganic fibers, to adjust the dispersion and consistency of the putty composition, solve the problems of powder agglomeration and segregation, and improve construction efficiency and surface smoothness.
It achieves good dispersion, fluidity and anti-sag properties of the putty composition, prolongs the operability time, ensures high construction efficiency, smooth and delicate surface, and is suitable for intelligent construction, especially robot construction.
Smart Images

Figure BDA0004928543650000081 
Figure BDA0004928543650000082 
Figure BDA0004928543650000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a putty composition and a preparation method and application thereof. Background Art
[0002] In the field of construction, intelligent equipment has developed rapidly in both production and manufacturing and construction applications. Intelligent construction is the focus of research today and has received much attention. Among them, robot construction is a new type of intelligent mechanical arm spraying construction method, which has the advantages of high automation, high construction efficiency, good spraying effect, and stable quality. Therefore, the robot construction method is very likely to gradually replace manual labor and become the mainstream construction method in the future. However, the current putty powder products are mainly used for manual scraping, which has a low degree of matching with the robot construction method. During the construction process, it is easy to cause problems such as nozzle clogging, short operating time, slurry segregation under high pressure, and sagging after spraying on the wall, as well as rough and uneven surface of the putty film after spraying on the wall, bubbles, shrinkage holes, etc. Therefore, it is of great practical significance and application value to develop a putty powder product suitable for the field of intelligent construction, especially robot construction. Summary of the invention
[0003] In order to overcome at least one problem existing in the above-mentioned prior art, one of the objects of the present invention is to provide a putty composition, which has excellent dispersibility and workability, can effectively solve the problem of powder agglomeration and clogging of spraying equipment during construction, and has high construction efficiency.
[0004] A second object of the present invention is to provide a method for preparing the above-mentioned putty composition.
[0005] The third object of the present invention is to provide an application of the above putty composition in the field of intelligent construction.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The first aspect of the present invention provides a putty composition, comprising the following raw materials in parts by mass: 60 to 100 parts of filler, 1 to 40 parts of base material, 0.01 to 2 parts of phosphate dispersant, 0.005 to 2 parts of polycarboxylic acid wetting agent, 0.1 to 10 parts of nano inorganic fiber, and 0.1 to 10 parts of functional additive.
[0008] In the putty composition of the present invention, the phosphate ions in the phosphate dispersant have a strong ability to complex metal ions, and can form soluble complexes with metal ions in common fillers or base materials in the putty composition, such as calcium ions, magnesium ions, etc., so as to adjust the dispersion effect of the composition, and the phosphate dispersant can form an electrostatic adsorption effect with the surface of particles such as fillers and base materials, thereby changing the surface charge properties of the particles, reducing the attraction between particles, and increasing the repulsive force, thereby achieving the dispersion of particles. At the same time, the phosphate dispersant is used in conjunction with a polycarboxylic acid wetting agent, and the water reduction efficiency is high and the system stability is strong. The phosphate dispersant and the polycarboxylic acid wetting agent are matched to solve the problems that the single-component putty is prone to powder agglomeration during stirring and swelling during use, so that the slurry consistency is stable and the operable time is extended. In addition, the nano inorganic fiber plays the role of an anti-sagging agent, and its suspension ability in the slurry is strong, and its electrical insulation is good, and it is not affected by electrolytes, which solves the problems of segregation and sagging after spraying in the putty composition during high-pressure spraying. By combining various raw materials, the putty composition obtained by the invention has good dispersibility, fluidity, anti-sagging and construction performance.
[0009] Preferably, in the putty composition, the phosphate dispersant includes at least one of sodium hexametaphosphate, sodium tripolyphosphate or sodium pyrophosphate; further preferably, the phosphate dispersant is selected from sodium hexametaphosphate.
[0010] In the present invention, the use of sodium hexametaphosphate and polycarboxylic acid wetting agent has a better coordination effect, can effectively improve the water reduction efficiency, improve the system dispersibility and enhance the system stability.
[0011] Preferably, in the putty composition, the mass fraction of the phosphate dispersant is 0.03 to 1.5 parts; more preferably, it is 0.05 to 1 part; and even more preferably, it is 0.2 to 0.7 parts.
[0012] Preferably, in the putty composition, the mass fraction of the polycarboxylic acid wetting agent is 0.008 to 1.5 parts; more preferably 0.01 to 1 part; and even more preferably 0.02 to 0.06 parts.
[0013] Preferably, in the putty composition, the nano inorganic fibers are obtained by dispersing and modifying fibrous inorganic minerals with a dispersing modifier; the fibrous inorganic minerals include at least one of attapulgite, sepiolite or asbestos; and the dispersing modifier includes at least one of sodium hexametaphosphate, sodium tripolyphosphate or sodium pyrophosphate.
[0014] Fibrous inorganic minerals in their natural state have many impurities and are difficult to separate to the nanometer level. The dispersing modifier of the present invention has a good dispersing effect on fibrous inorganic minerals, and nanometer-level fibers are obtained, so that the fiber material has good suspension ability and anti-sagging effect in the system.
[0015] Preferably, the fibrous inorganic mineral is selected from attapulgite. Attapulgite is a fibrous agglomerate in its natural state, and its main component is magnesium aluminum silicate. After being dispersed and modified by the method of the present invention, the obtained nano inorganic fiber has a strong suspension ability, which can effectively solve the problems of segregation of putty during high-pressure spraying and sagging after spraying.
[0016] Preferably, the dispersing modifier is selected from sodium hexametaphosphate. Sodium hexametaphosphate has a strong ability to complex metal ions and can effectively disperse and modify fibrous inorganic minerals such as attapulgite.
[0017] Preferably, the mass ratio of the fibrous inorganic mineral to the modified dispersant is 1:(0.01-0.15); more preferably 1:(0.02-0.1); and even more preferably 1:(0.03-0.08).
[0018] Preferably, the dispersion modification is carried out in water.
[0019] Preferably, the mass ratio of the fibrous inorganic mineral to water is 1:(1-3); more preferably 1:(1.2-2.8); and even more preferably 1:(1.5-2.5).
[0020] Preferably, the dispersion modification method is ultrasonic dispersion, stirring dispersion or a combination thereof; further preferably, the dispersion modification method is a combination of ultrasonic dispersion and stirring dispersion.
[0021] Preferably, the ultrasonic frequency of the ultrasonic dispersion is 10 to 30 kHz; more preferably, it is 15 to 25 kHz.
[0022] Preferably, the stirring speed of the stirring and dispersing is 1000 to 3000 r / min; more preferably, it is 1500 to 2500 r / min.
[0023] Preferably, the dispersion modification time is 10 to 60 minutes; more preferably, it is 20 to 40 minutes.
[0024] Preferably, in the putty composition, the mass fraction of the nano inorganic fiber is 0.3 to 8 parts; more preferably 0.5 to 5 parts; further preferably 0.5 to 1 part.
[0025] Preferably, the filler includes at least one of heavy calcium carbonate, light calcium carbonate, talc or wollastonite; further preferably, the filler is selected from heavy calcium carbonate.
[0026] Preferably, the average particle size of the filler is ≥400 mesh; further preferably, the 325 mesh residue of the filler accounts for ≤10%.
[0027] Preferably, the blue light whiteness of the filler is ≥80.
[0028] Preferably, in the putty composition, the mass fraction of filler is 65 to 95 parts; more preferably, it is 70 to 90 parts; and even more preferably, it is 75 to 85 parts.
[0029] Preferably, the base material comprises at least one of lime lime, silicate or gypsum; further preferably, the base material is selected from lime lime.
[0030] Preferably, the average particle size of the base material is ≥400 mesh; further preferably, the 325 mesh residue of the base material accounts for ≤10%.
[0031] Preferably, the blue light whiteness of the base material is ≥80.
[0032] Preferably, in the putty composition, the mass fraction of the base material is 3 to 35 parts; more preferably, it is 5 to 30 parts; and even more preferably, it is 15 to 20 parts.
[0033] Preferably, in the putty composition, the mass fraction of the functional additive is 0.3 to 8 parts; more preferably, it is 0.6 to 5.6 parts; and even more preferably, it is 1 to 3 parts.
[0034] Preferably, the putty composition comprises the following raw materials in parts by mass: 65 to 95 parts of filler, 3 to 35 parts of base material, 0.03 to 1.5 parts of phosphate dispersant, 0.008 to 1.5 parts of polycarboxylic acid wetting agent, 0.3 to 8 parts of nano inorganic fiber, and 0.3 to 8 parts of functional additive.
[0035] Further preferably, the putty composition comprises the following raw materials in parts by mass: 70 to 90 parts of filler, 5 to 30 parts of base material, 0.05 to 1 part of phosphate dispersant, 0.01 to 1 part of polycarboxylic acid wetting agent, 0.5 to 5 parts of nano inorganic fiber, and 0.6 to 5.6 parts of functional additives.
[0036] More preferably, the putty composition comprises the following raw materials in parts by mass: 75-85 parts of filler, 15-20 parts of base material, 0.2-0.7 parts of phosphate dispersant, 0.02-0.06 parts of polycarboxylic acid wetting agent, 0.5-1 parts of nano inorganic fiber, and 1-2 parts of functional additives.
[0037] Preferably, the functional additive comprises cellulose ether, redispersible latex powder or a combination thereof; further preferably, the functional additive comprises cellulose ether and redispersible latex powder.
[0038] Preferably, the cellulose ether includes at least one of hydroxypropyl methylcellulose ether, hydroxyethyl methylcellulose ether or hydroxyethyl cellulose ether; further preferably, the cellulose ether is selected from hydroxypropyl methylcellulose ether.
[0039] Preferably, the viscosity of the cellulose ether in a 2% aqueous solution at 20° C. is 10,000 to 40,000 mPa·s; more preferably, it is 20,000 to 35,000 mPa·s.
[0040] Preferably, in the putty composition, the mass fraction of cellulose ether is 0.02 to 2 parts; more preferably 0.1 to 0.6 parts; and even more preferably 0.2 to 0.5 parts.
[0041] Preferably, the redispersible latex powder includes at least one of ethylene, vinyl chloride and vinyl laurate ternary copolymer latex powder (E / VC / VL), vinyl acetate and ethylene copolymer latex powder (EVA), vinyl acetate and ethylene and higher fatty acid vinyl ester ternary copolymer latex powder (VAC / E / VEOVA), acrylate and styrene copolymer latex powder (A / S), and styrene and butadiene copolymer latex powder (SBR); further preferably, the redispersible latex powder includes at least one of vinyl acetate and ethylene copolymer latex powder (EVA), acrylate and styrene copolymer latex powder (A / S), and styrene and butadiene copolymer latex powder (SBR); further preferably, the redispersible latex powder is selected from vinyl acetate and ethylene copolymer latex powder (EVA).
[0042] Preferably, the solid content of the redispersible latex powder is 98-100%.
[0043] Preferably, the glass transition temperature of the redispersible latex powder is 0 to 10°C.
[0044] Preferably, in the putty composition, the mass fraction of the redispersible latex powder is 0.08 to 8 parts; more preferably 0.5 to 5 parts; further preferably 0.8 to 2.5 parts.
[0045] Preferably, the putty composition comprises the following raw materials in parts by mass: 60 to 100 parts of filler, 1 to 40 parts of base material, 0.01 to 2 parts of phosphate dispersant, 0.005 to 2 parts of polycarboxylic acid wetting agent, 0.1 to 10 parts of nano inorganic fiber, 0.02 to 2 parts of cellulose ether, and 0.08 to 8 parts of redispersible latex powder.
[0046] Further preferably, the putty composition comprises the following raw materials in parts by mass: 70 to 90 parts of filler, 5 to 30 parts of base material, 0.05 to 1 part of phosphate dispersant, 0.01 to 1 part of polycarboxylic acid wetting agent, 0.5 to 5 parts of nano inorganic fiber, 0.1 to 0.6 parts of cellulose ether, and 0.5 to 5 parts of redispersible latex powder.
[0047] More preferably, the putty composition comprises the following raw materials in parts by mass: 75 to 85 parts of filler, 15 to 20 parts of base material, 0.2 to 0.7 parts of phosphate dispersant, 0.02 to 0.06 parts of polycarboxylic acid wetting agent, 0.5 to 1 parts of nano inorganic fiber, 0.2 to 0.5 parts of cellulose ether, and 0.8 to 2.5 parts of redispersible latex powder.
[0048] Preferably, in the putty composition, the raw materials also include water.
[0049] Preferably, in the putty composition, the filler, base material, phosphate dispersant, polycarboxylic acid wetting agent, nano inorganic fiber and functional additive are ash, and the mass ratio of the water to the ash is (0.1-1): 1; more preferably (0.2-0.8): 1; and more preferably (0.3-0.6): 1. In some specific embodiments of the present invention, the mass ratio of the water to the ash is referred to as the water-ash ratio.
[0050] The second aspect of the present invention provides a method for preparing the putty composition described in the first aspect of the present invention, comprising the following steps: mixing various raw materials to obtain the putty composition.
[0051] Preferably, the mixing method is selected from stirring.
[0052] Preferably, the stirring speed is 10 to 650 r / min; more preferably, 20 to 600 r / min.
[0053] Preferably, the mixing time is 10 to 60 minutes; more preferably, it is 15 to 50 minutes.
[0054] Preferably, the preparation method of the putty composition specifically comprises the following steps: firstly, the filler, the base material, the phosphate dispersant, the polycarboxylic acid wetting agent, the nano inorganic fiber and the functional additive are mixed for the first time, and then water is added for the second mixing to obtain the putty composition.
[0055] Preferably, the first mixing speed is 10 to 60 r / min; more preferably, 20 to 40 r / min.
[0056] Preferably, the first mixing time is greater than 10 min; more preferably, it is 15 to 50 min.
[0057] Preferably, the second mixing speed is 350-650 r / min; more preferably 400-600 r / min.
[0058] Preferably, the second mixing time is 1 to 10 minutes; more preferably, it is 3 to 5 minutes.
[0059] Preferably, through the second mixing, the consistency of the putty composition is adjusted to 145-150 mm, where the consistency is measured according to GB / T 1749-1979.
[0060] The third aspect of the present invention provides an application of the putty composition described in the first aspect of the present invention in the field of intelligent construction.
[0061] Preferably, the intelligent construction is robot construction.
[0062] The beneficial effects of the present invention are as follows: the present invention adopts a phosphate dispersant and a polycarboxylic acid wetting agent to obtain a putty composition system with good dispersibility, strong stability, long operability time and high construction efficiency; combined with nano inorganic fibers, the putty composition does not settle and separate during construction under high pressure, and the surface after construction is smooth and delicate without sagging. Therefore, the putty composition provided by the present invention can be widely used in intelligent construction, especially in the field of robot construction.
[0063] Specifically, compared with the prior art, the present invention has the following advantages:
[0064] 1. The putty composition of the present invention has excellent dispersibility and workability, can effectively solve the problem of powder agglomeration and clogging of spraying equipment during construction, and has high construction efficiency.
[0065] 2. The putty composition of the present invention has a longer operable time, is more suitable for long-term continuous spraying construction, has a stable consistency, has a certain fluidity, does not settle and separate under high pressure, and has a smooth and delicate surface after spraying without sagging.
[0066] 3. After the putty composition of the present invention is sprayed and polished, the surface is smooth and delicate, the strength is high, and the powder does not fall off when wet rubbing. It is unnecessary to apply latex paint and can be used as a paint-free surface putty for interior walls. It is low-carbon and environmentally friendly and has good economic benefits. DETAILED DESCRIPTION
[0067] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.
[0068] Among them, it should be noted that:
[0069] The filler used in the embodiments and comparative examples of the present invention is heavy calcium carbonate, specifically ultrafine white heavy calcium carbonate powder with a mesh size of 400 or more, with a 325-mesh sieve residue of no more than 10%; and a blue light whiteness of no less than 84.
[0070] The base material used in the embodiment of the present invention is lime, specifically lime powder with a mesh size of 400 or more, and the residue on a 325-mesh sieve is no more than 10%; the blue light whiteness is no less than 80.
[0071] The phosphate dispersant used in the embodiments and comparative examples of the present invention is sodium hexametaphosphate ((NaPO3)6), which is a white crystalline powder.
[0072] The polycarboxylic acid wetting agent used in the examples and comparative examples of the present invention was purchased from Jiangsu Fujilia Building Materials Co., Ltd., and the model number was 72N.
[0073] The nano inorganic fibers used in the embodiments and comparative examples of the present invention are prepared by the following method: attapulgite clay and water are mixed in a mass ratio of 0.5:1, and 5% of sodium hexametaphosphate by mass of attapulgite clay is added for mixing. The mixing method is stirring while ultrasonic dispersion, the frequency of ultrasonic dispersion is 20kHz, the stirring speed is 2000r / min, the mixing time is 30min, and then solid-liquid separation, drying, grinding, and sieving are performed to obtain the nano inorganic fibers.
[0074] In the embodiments and comparative examples of the present invention, the attapulgite clay used is a fibrous agglomerate mineral powder whose main component is magnesium aluminum silicate. It has more impurities in its natural state and is difficult to separate to the nanoscale. After dispersion modification, the obtained nanoscale fiber filaments have extremely strong suspension ability in the slurry, so that the slurry can maintain excellent supporting force even in a low viscosity state, and it is not affected by electrolytes, thereby solving the problems of segregation of the putty composition during high-pressure spraying and sagging after spraying.
[0075] The functional additives used in the embodiments and comparative examples of the present invention are cellulose ether and redispersible latex powder, the cellulose ether is hydroxypropyl methyl cellulose ether, and the viscosity of its 2% aqueous solution at 20°C is 30000mPa·s; the redispersible latex powder is vinyl acetate and ethylene copolymer latex powder (EVA), and its solid content is 99%±1% and the glass transition temperature is 0-10°C.
[0076] In the examples and comparative examples of the present invention, normal temperature refers to 20 to 30°C.
[0077] Example 1
[0078] A putty composition comprises the following raw materials in parts by mass: 82.68 parts of heavy calcium carbonate, 15 parts of lime calcium, 0.3 parts of cellulose ether, 1 part of redispersible latex powder, 0.5 parts of phosphate dispersant, 0.02 parts of polycarboxylic acid wetting agent and 0.5 parts of nano inorganic fiber.
[0079] The preparation method of the above putty composition comprises the following steps:
[0080] (1) weighing heavy calcium powder, lime calcium, cellulose ether, redispersible latex powder, phosphate dispersant, polycarboxylic acid wetting agent, and nano inorganic fiber in proportion, and sequentially putting various raw material powders into a powder stirring kettle for mixing at a speed of 20 to 40 r / min for a mixing time of more than 10 min, and mixing evenly to obtain a mixed powder material;
[0081] (2) The mixed powder material and water are stirred in a mass ratio of 1: (0.3-0.6) at a stirring speed of 400-600 r / min for 3-5 min to obtain a uniform, particle-free fluid slurry. The consistency of the fluid slurry is adjusted to 150±5 mm in accordance with GB / T 1749-1979. After standing for 10-15 minutes, the slurry is stirred again for 3 minutes before use to obtain a putty composition 1.
[0082] Example 2
[0083] A putty composition comprises the following raw materials in parts by weight: 77.16 parts of heavy calcium carbonate, 20 parts of lime calcium, 0.3 parts of cellulose ether, 1 part of redispersible latex powder, 0.5 parts of phosphate dispersant, 0.04 parts of polycarboxylic acid wetting agent and 1 part of nano inorganic fiber.
[0084] The preparation method of the above putty composition comprises the following steps:
[0085] (1) weighing heavy calcium powder, lime calcium, cellulose ether, redispersible latex powder, phosphate dispersant, polycarboxylic acid wetting agent, and nano inorganic fiber in proportion, and sequentially putting various raw material powders into a powder stirring kettle for mixing at a speed of 20 to 40 r / min for a mixing time of more than 10 min, and mixing evenly to obtain a mixed powder material;
[0086] (2) The mixed powder material and water are stirred in a mass ratio of 1: (0.3-0.6) at a stirring speed of 400-600 r / min for 3-5 min to obtain a uniform, particle-free fluid slurry. The consistency of the fluid slurry is adjusted to 150±5 mm in accordance with GB / T 1749-1979. After standing for 10-15 minutes, the slurry is stirred again for 3 minutes before use to obtain a putty composition 2.
[0087] Example 3
[0088] A putty composition comprises the following raw materials in parts by mass: 76.64 parts of heavy calcium carbonate, 20 parts of lime calcium, 0.3 parts of cellulose ether, 1.5 parts of redispersible latex powder, 0.5 parts of phosphate dispersant, 0.06 parts of polycarboxylic acid wetting agent and 1 part of nano inorganic fiber.
[0089] The preparation method of the above putty composition comprises the following steps:
[0090] (1) weighing heavy calcium powder, lime calcium, cellulose ether, redispersible latex powder, phosphate dispersant, polycarboxylic acid wetting agent, and nano inorganic fiber in proportion, and sequentially putting various raw material powders into a powder stirring kettle for mixing at a speed of 20 to 40 r / min for a mixing time of more than 10 min, and mixing evenly to obtain a mixed powder material;
[0091] (2) The mixed powder material and water are stirred in a mass ratio of 1: (0.3-0.6) at a stirring speed of 400-600 r / min for 3-5 min to obtain a uniform, particle-free fluid slurry. The consistency of the fluid slurry is adjusted to 150±5 mm in accordance with GB / T 1749-1979. After standing for 10-15 minutes, the slurry is stirred again for 3 minutes before use to obtain a putty composition 3.
[0092] Comparative Example 1
[0093] A putty composition. In this comparative example, a water-resistant putty material for interior walls currently available on the market is used to prepare a putty composition 4 according to steps (1) and (2) of the preparation method of the putty composition in Example 1.
[0094] Comparative Example 2
[0095] A putty composition is disclosed. The difference from Example 1 is that the nano inorganic fiber in Example 1 is omitted in this comparative example, and the other parts remain the same. Putty composition 5 is prepared according to the preparation method of the putty composition in Example 1.
[0096] Comparative Example 3
[0097] A putty composition, which differs from Example 1 in that, in this comparative example, the nano inorganic fiber in Example 1 is replaced with unmodified attapulgite clay, and the rest remain the same. Putty composition 6 is prepared according to the preparation method of the putty composition in Example 1.
[0098] Performance Testing
[0099] According to the relevant testing standards in JG / T 298-2010 "Putty for Building Interior Use", the putty compositions of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 were tested, and the test results of physical properties and application properties are shown in Tables 1 to 2.
[0100] Table 1 Physical properties of putty compositions of Examples 1 to 3 and Comparative Examples 1 to 3
[0101]
[0102] Table 2 Application performance of putty compositions of Examples 1 to 3 and Comparative Examples 1 to 3
[0103]
[0104]
[0105] As can be seen from Tables 1 to 2, the putty compositions provided in Examples 1 to 3 of the present invention have better dispersibility, workability and longer operability time than those in Comparative Example 1, and are more suitable for long-term continuous spraying construction, and the construction efficiency is significantly improved. Compared with Comparative Examples 2 to 3, the putty compositions provided in Examples 1 to 3 have better anti-sagging properties, stable consistency, and no segregation during high-pressure spraying. The putty compositions of Examples 1 to 3 of the present invention are suitable for robot construction and can be used as paint-free surface putty for interior walls.
[0106] The putty compositions obtained in Examples 1 to 3 of the present invention have excellent dispersibility and workability, can effectively solve the problem of powder agglomeration and clogging of spraying equipment during construction, and have high construction efficiency; moreover, have a longer operable time, are more suitable for long-term continuous spraying construction, have stable consistency, have certain fluidity, do not settle and separate under high pressure, and have a smooth and delicate surface after spraying without sagging; after the putty compositions of Examples 1 to 3 are sprayed and polished, the surface is smooth and delicate, the strength is high, and the powder does not fall off when wet rubbing, latex paint can be avoided, and can be used as a paint-free surface putty for interior walls, which is low-carbon and environmentally friendly and has good economic benefits.
[0107] In summary, the present invention adopts a phosphate dispersant and a polycarboxylic acid wetting agent to obtain a putty composition system with good dispersibility, strong stability, long operability time and high construction efficiency. Combined with nano inorganic fibers, the putty composition does not settle and separate during construction under high pressure, and the surface after construction is smooth and delicate without sagging. Therefore, the putty composition provided by the present invention can be widely used in intelligent construction, especially in the field of robot construction.
Claims
1. A putty composition, characterized in that: The invention comprises the following raw materials in parts by weight: 60 to 100 parts of filler, 1 to 40 parts of base material, 0.01 to 2 parts of phosphate dispersant, 0.005 to 2 parts of polycarboxylic acid wetting agent, 0.1 to 10 parts of nano inorganic fiber and 0.1 to 10 parts of functional additive.
2. The putty composition according to claim 1, characterized in that The phosphate dispersant includes at least one of sodium hexametaphosphate, sodium tripolyphosphate or sodium pyrophosphate.
3. The putty composition according to claim 1, characterized in that The nano inorganic fiber is obtained by dispersing and modifying a fibrous inorganic mineral with a dispersing modifier; the fibrous inorganic mineral includes at least one of attapulgite, sepiolite or asbestos; and the dispersing modifier includes at least one of sodium hexametaphosphate, sodium tripolyphosphate or sodium pyrophosphate.
4. The putty composition according to claim 3, characterized in that The mass ratio of the fibrous inorganic mineral to the modified dispersant is 1:(0.01-0.15); and / or, the dispersion modification is carried out in water, and the mass ratio of the fibrous inorganic mineral to water is 1:(1-3); And / or, the dispersion modification method is ultrasonic dispersion, stirring dispersion or a combination thereof.
5. The putty composition according to claim 1, characterized in that: The filler includes at least one of heavy calcium carbonate, light calcium carbonate, talc or wollastonite; and / or, the base material comprises at least one of lime lime, silicate or gypsum; And / or, the functional additive includes cellulose ether, redispersible latex powder or a combination thereof.
6. The putty composition according to claim 5, characterized in that: The cellulose ether includes at least one of hydroxypropyl methyl cellulose ether, hydroxyethyl methyl cellulose ether or hydroxyethyl cellulose ether; And / or, the redispersible latex powder includes at least one of ternary copolymer latex powder of ethylene, vinyl chloride and vinyl laurate, copolymer latex powder of vinyl acetate and ethylene, ternary copolymer latex powder of vinyl acetate, ethylene and higher fatty acid vinyl ester, copolymer latex powder of acrylate and styrene, or copolymer latex powder of styrene and butadiene.
7. The putty composition according to claim 1, characterized in that: The raw materials also include water. Preferably, the filler, base material, phosphate dispersant, polycarboxylic acid wetting agent, nano inorganic fiber and functional additive are used as ash, and the mass ratio of the water to the ash is (0.1-1):
1.
8. A method for preparing the putty composition according to any one of claims 1 to 7, characterized in that: The following steps are involved: The raw materials are mixed to obtain the putty composition.
9. The preparation method according to claim 8, characterized in that: The mixing method is selected from stirring, and the stirring speed is preferably 10 to 650 r / min; And / or, the mixing time is 10 to 60 minutes.
10. Use of the putty composition according to any one of claims 1 to 7 in the field of intelligent construction.
Citation Information
Patent Citations
Antibacterial environment-friendly interior wall putty and preparation method thereof
CN116254015A
Method of preparing an easily-dispersed rheology-grade product from a pseudolaminar silicate, product thus obtained and methods of using same