Novel backwater putty paste as well as preparation method and application thereof
By coating nano-silver with acid-modified starch and compounding it with different mesh numbers of silica, combined with infiltration crystallization, the problems of mildew and bacterial growth of putty in warm and humid areas are solved, and the anti-mildew and antibacterial functions of putty are achieved. Improved indoor living environment.
Patent Information
- Application Number
- CN202410926278.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Existing putty is prone to mildew and bacterial growth in warm, hot and humid areas, and lacks anti-mildew and antibacterial functions, causing indoor living environment problems.
Acid-modified starch is used to coat nano-silver, combined with silica of different mesh sizes, and infiltrated crystals are added to form a new type of backwater putty paste with anti-fungal and anti-bacterial effects.
It can effectively prevent mildew and inhibit bacterial growth, significantly improve the indoor living environment, and meet the requirements of anti-fungal and antibacterial functions.
Smart Images

Figure BDA0004938256650000071 
Figure BDA0004938256650000081 
Figure BDA0004938256650000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a novel back-water putty paste and a preparation method and application thereof. Background Art
[0002] With the improvement of living standards, people have more and more stringent requirements for indoor living environment, and a living environment that can inhibit the growth of bacteria has become an urgent need for consumers. Putty, as an indispensable building material before painting, will make a great contribution to the improvement of indoor living environment if it has certain anti-mildew and antibacterial functions.
[0003] Existing putties generally use carboxymethyl starch and pregelatinized starch as raw materials. Although the putties prepared do not contain harmful substances, they have poor mildew resistance and do not have antibacterial functions. Especially in warm and humid areas, mildew and bacterial growth are very serious, which leads to serious economic losses and even threatens human health. Therefore, proposing a putty with mildew resistance and antibacterial functions has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0004] The purpose of the present invention is to provide a putty with anti-mildew and antibacterial functions, which can effectively resist mildew and inhibit bacterial growth, thereby improving the indoor living environment.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] One of the technical solutions of the present invention:
[0007] A novel back-water putty paste comprises the following raw materials in parts by weight: 20-40 parts of silicate cement, 10-30 parts of lime lime, 1-10 parts of modified starch, 10-30 parts of composite silicon dioxide, 1-10 parts of cellulose, 1-5 parts of osmotic crystallization, 1-5 parts of lubricant and 1-5 parts of water reducing agent;
[0008] Preferably, the following raw materials are included in parts by weight: 30 parts of silicate cement, 20 parts of lime lime, 5 parts of modified starch, 20 parts of composite silica, 5 parts of cellulose, 2 parts of osmotic crystallizer, 3 parts of lubricant and 3 parts of water reducing agent.
[0009] Furthermore, the preparation method of the modified starch comprises the following steps:
[0010] Step 1, subjecting starch to acid modification treatment to obtain acid-modified starch;
[0011] Step 2: coating the acid-modified starch obtained in step 1 with nano-silver to obtain starch-coated nano-silver, i.e., the modified starch;
[0012] Furthermore, in step 1, the acid modification treatment is specifically as follows: dissolving starch in water according to a starch to water mass volume ratio of 1 g: (5-15) mL to form a starch suspension, then adding an acidic solvent, modifying at a modification temperature of 40-60° C. and a stirring speed of 40 rpm for 30-60 min, then alkaline neutralization, washing with water, and drying at 35° C.;
[0013] Preferably, the mass volume ratio of starch to water is 1 g:10 mL, the modification temperature is 55° C., and the modification time is 45 min;
[0014] Furthermore, the volume ratio of the starch suspension to the acidic solvent is 1:(0.5-1.5);
[0015] Preferably, the volume ratio of starch suspension to acidic solvent is 1:1;
[0016] Furthermore, the acidic solvent is a hydrochloric acid solution with a concentration of 0.3 mol / L or an acetic acid solution with a concentration of 0.8 mol / L;
[0017] Furthermore, before dissolving the starch in water, the starch can be etched using volatiles of a high concentration acidic solvent. Specifically, the starch is placed above a hydrochloric acid solution with a concentration of 4 mol / L or an acetic acid solution with a concentration of 10 mol / L, and the starch is etched using hydrogen chloride or acetic acid gas evaporated from the acidic solvent at 40°C.
[0018] The present invention utilizes acid to modify starch, that is, acid-treats starch, which can effectively improve the mildew-proof and antibacterial properties of putty. After analysis, the reasons are: first, acid has an etching effect, and the starch particles after acid modification have a structural characteristic of a large number of micropores and dispersed micropore distribution, which makes it possible to coat as many silver nanoparticles as possible when coating silver nanoparticles in the subsequent process, and allows the silver nanoparticles to be better attached to the inside of the starch (that is, the silver particles are grafted in each tiny hole, and will not aggregate, which is not conducive to the mildew-proof and antibacterial effect); secondly, acid can destroy glycosidic bonds to a certain extent, that is, destroy the long starch chain, so the starch molecular chain after acid modification is generally shorter, which makes it possible for the silver nanoparticles to have enough space to contact the atmospheric environment after the subsequent coating of the silver nanoparticles, and effectively play a mildew-proof and antibacterial role.
[0019] In addition, compared with ordinary starch, acid-modified starch has the characteristic of not expanding after absorbing water (ordinary starch will expand significantly after absorbing water). Therefore, if ordinary starch is used as filler in a relatively humid and hot environment, the starch in the putty will expand, causing the putty layer to fall off.
[0020] In addition, the pregelatinized starch in the prior art also has a rich porous structure. However, since the pregelatinization process cannot break the glycosidic bonds in the long starch chains, the subsequently coated silver nanoparticles cannot be given enough space to contact the atmospheric environment, which ultimately leads to a deterioration in the anti-mildew and antibacterial effects.
[0021] Furthermore, in step 2, the coating is specifically as follows: dissolving the acid-modified starch in water according to the mass volume ratio of the acid-modified starch to water of 1 g: (5-15) mL to form an acid-modified starch solution, and then adding a 2×10 -2 mol / L silver nitrate solution was reacted at a reaction temperature of 80-100°C and a stirring speed of 500 rpm for 1-2 hours, and finally a 2×10 -2 mol / L glucose solution, filtered, and dried at 35°C;
[0022] Preferably, the mass volume ratio of acid-modified starch to water is 1 g:10 mL, the reaction temperature is 90° C., and the reaction time is 1.5 h;
[0023] Furthermore, the dropwise addition is controlled to be 30 to 40 drops per minute;
[0024] Furthermore, the volume ratio of the acid-modified starch solution, the silver nitrate solution and the glucose solution is 5:(2-3):(1-2);
[0025] Preferably, the volume ratio of the acid-modified starch solution, the silver nitrate solution and the glucose solution is 5:2.5:1.5.
[0026] The present invention encapsulates nano-silver in starch, utilizes the anti-mildew and anti-bacterial effect of nano-silver itself, and combines the microporous structure of acid-modified starch to achieve the anti-mildew and anti-bacterial effect of putty more efficiently.
[0027] Further, the composite silicon dioxide is formed by mixing 325 mesh silicon dioxide and 2000 mesh silicon dioxide, wherein the mass ratio of 325 mesh silicon dioxide to 2000 mesh silicon dioxide is 2:(3-5);
[0028] Preferably, the mass ratio of 325 mesh silica to 2000 mesh silica is 2:3.5.
[0029] The present invention compounds two silicas with different mesh sizes, which can utilize the filling and reinforcing effect of 2000-mesh silica and the microporous property of 325-mesh silica, thereby ultimately increasing the air permeability of the putty while ensuring the mechanical properties of the putty, allowing the silver nanoparticles to better contact with the air, thereby achieving efficient mildew and antibacterial effects.
[0030] In addition, since the low mesh number silica has micropores, it can also provide crystal growth space for penetration crystallization, effectively preventing moisture in the air from entering the putty, thereby preventing the putty from mildewing caused by moisture entering the putty.
[0031] Furthermore, the osmotic crystallization is tartaric acid, sodium silicate or calcium chloride.
[0032] The osmotic crystals added in the present invention can form dendrite-like crystals with the hydration product of putty, calcium hydroxide, that is, if moisture in the atmosphere enters the putty, the formed hydration product will react with the osmotic crystals to form dendrite-like crystals. The presence of dendrite-like crystals can effectively prevent moisture from further entering the putty, reduce the contact between the putty and water, and thus achieve the effect of preventing mildew.
[0033] The second technical solution of the present invention:
[0034] The preparation method of the novel back-water putty paste comprises the following steps:
[0035] The raw materials are weighed according to the mass parts, the silicate cement, lime lime, modified starch and composite silicon dioxide are premixed, and then cellulose, osmotic crystallization, lubricant and water reducing agent are added and mixed to obtain the novel back-water putty paste.
[0036] The third technical solution of the present invention:
[0037] The application of the above-mentioned novel back-water putty paste in wall construction.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The invention adopts the technical scheme of acid-modified starch coated nano-silver, composite addition of silicon dioxide of different mesh sizes, and added penetration crystallization, so that the backwater putty paste has the functions of resisting mildew and inhibiting bacterial growth, and effectively improves the indoor living environment. DETAILED DESCRIPTION
[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Unless otherwise specified, the "parts" described in the present invention are all based on mass parts; in the following examples, the raw materials are weighed according to 1 part = 1 g.
[0042] In the following embodiments, the novel back-water putty paste comprises the following raw materials by weight: 20-40 parts of silicate cement, 10-30 parts of lime, 1-10 parts of modified starch, 10-30 parts of composite silicon dioxide, 1-10 parts of cellulose, 1-5 parts of osmotic crystallization, 1-5 parts of lubricant and 1-5 parts of water reducing agent;
[0043] Wherein, the preparation method of modified starch comprises the following steps:
[0044] 1) dissolving starch in water according to the mass volume ratio of starch to water of 1 g: (5-15) mL to form a starch suspension, then adding an acidic solvent, modifying at a modification temperature of 40-60° C. and a stirring speed of 40 rpm for 30-60 min, then alkali washing and neutralizing with a sodium hydroxide solution with a concentration of 0.1 mol / L, washing with water until the pH of the washing solution is ≈ 7, and drying at 35° C. to obtain an acid-modified starch;
[0045] The volume ratio of the starch suspension to the acidic solvent is 1:(0.5-1.5);
[0046] The acidic solvent is a hydrochloric acid solution with a concentration of 0.3 mol / L or an acetic acid solution with a concentration of 0.8 mol / L. It has been verified that the selection of any one of the two acidic solvents will not have a decisive effect on the experimental results. Therefore, in the following examples, only the hydrochloric acid solution is used as an example;
[0047] 2) dissolving the acid-modified starch obtained in step 1) in water at a mass volume ratio of 1 g:(5-15) mL of acid-modified starch to water to form an acid-modified starch solution, and then adding a 2×10 -2 mol / L silver nitrate solution was reacted at a reaction temperature of 80-100°C and a stirring speed of 500 rpm for 1-2 hours, and finally a 2×10 -2 mol / L glucose solution, filtered, and dried at 35°C;
[0048] The dropwise addition is controlled at 30 to 40 drops per minute;
[0049] The volume ratio of the acid-modified starch solution, the silver nitrate solution and the glucose solution is 5:(2-
[0050] 3):(1~2);
[0051] Before the starch is acid-modified, the starch can also be placed on a hydrochloric acid solution with a concentration of 4 mol / L or an acetic acid solution with a concentration of 10 mol / L, and the starch can be etched at 40°C using hydrogen chloride or acetic acid gas volatilized from the solvent;
[0052] The composite silicon dioxide is prepared by mixing 325 mesh silicon dioxide and 2000 mesh silicon dioxide and stirring for 5 to 20 minutes, wherein the mass ratio of 325 mesh silicon dioxide to 2000 mesh silicon dioxide is 2:(3 to 5);
[0053] Wherein, the cellulose is carboxypropyl methyl cellulose;
[0054] Among them, the osmotic crystallization is tartaric acid, sodium silicate or calcium chloride. It has been verified that the selection of any one of the three osmotic crystallizations will not have a decisive influence on the experimental results. Therefore, in the following examples, only calcium chloride is used as an example.
[0055] In the following embodiments, the silicate cement is white silicate cement purchased from Jinan Zhongxin Chemical Co., Ltd.; the lime is 2000 mesh lime powder purchased from Quzhou Liangcheng Calcium Industry Co., Ltd.; the starch is industrial-grade starch purchased from Jiangsu Longcheng Fine Chemical Co., Ltd.; the 325 mesh silica is 325 mesh white carbon black purchased from Jinan Kasong Chemical Co., Ltd.; the 2000 mesh silica is 2000 mesh white carbon black purchased from Jinan Kasong Chemical Co., Ltd.; the carboxypropyl methylcellulose is purchased from Renqiu Shangxiang Environmental Protection Materials Factory; the lubricant is a thixotropic lubricant for gypsum cement mortar purchased from Jinan Junhai Chemical Co., Ltd.; the water reducer is a polycarboxylic acid water reducer purchased from Jinan Junhai Chemical Co., Ltd.
[0056] Example 1
[0057] A new type of back water putty paste
[0058] 1) Weigh each raw material according to the mass fraction recorded in 1# in Table 1;
[0059] 2) Starch modification: The starch weighed in step 1) was mixed with water at a mass volume ratio of 1 g:10 mL to obtain a starch suspension, and then 10 mL of a 0.3 mol / L hydrochloric acid solution was added, and the stirring speed was controlled to be 40 rpm at 55° C. for modification for 45 min, and then the mixture was neutralized by alkaline washing with a sodium hydroxide solution with a concentration of 0.1 mol / L, washed with water until the pH of the washing solution was ≈ 7, and dried at 35° C. to obtain an acid-modified starch;
[0060] 3) Starch-coated nanosilver: The acid-modified starch obtained in step 2) was mixed with water at a mass volume ratio of 1 g:10 mL to obtain an acid-modified starch solution, and then 5 mL of 2×10 -2 mol / L silver nitrate solution was stirred at 500 rpm at 90°C for 1.5 h, and finally 3 mL 2×10 -2 mol / L glucose solution, filtered and dried at 35°C to obtain starch-coated nanosilver;
[0061] 4) Composite silica: The 325-mesh silica and 2000-mesh silica weighed in step 1) were mixed and stirred for 10 minutes to obtain composite silica;
[0062] 5) Premixing: The silicate cement and lime lime weighed in step 1), the starch-coated nanosilver obtained in step 3), and the composite silicon dioxide obtained in step 4) are mixed and stirred for 30 minutes to obtain a premix;
[0063] 6) Mixing: adding the cellulose, osmotic crystallization, lubricant and water reducing agent weighed in step 1) to the premix obtained in step 5), and mixing for 30 minutes to obtain the novel back-water putty paste.
[0064] Example 2
[0065] A new type of back water putty paste
[0066] Same as Example 1, except that: each raw material was weighed according to the mass fraction recorded in 2# in Table 1.
[0067] Example 3
[0068] A new type of back water putty paste
[0069] Same as Example 1, except that: each raw material was weighed according to the mass fraction recorded in 3# in Table 1.
[0070] Example 4
[0071] A new type of back water putty paste
[0072] Same as Example 1, except that: each raw material is weighed according to the mass fraction recorded in 4# in Table 1.
[0073] Example 5
[0074] A new type of back water putty paste
[0075] Same as Example 1, except that: each raw material was weighed according to the mass fraction recorded in 5# in Table 1.
[0076] Example 6
[0077] A new type of back water putty paste
[0078] The same as Example 1, except that: before step 2), the starch is placed on a hydrochloric acid solution with a concentration of 4 mol / L or an acetic acid solution with a concentration of 10 mol / L, and the starch is etched at 40°C using hydrogen chloride or acetic acid gas evaporated from the solvent, and then the starch is acid-modified.
[0079] Table 1 Raw material dosage (parts)
[0080]
[0081]
[0082] Comparative Example 1
[0083] A back water putty paste
[0084] The same as Example 1, except that step 2) is omitted, that is, the starch is directly coated with silver nanoparticles.
[0085] Comparative Example 2
[0086] A back water putty paste
[0087] The same as Example 1, except that step 2) is omitted and the silver nanoparticles are coated with directly purchased pregelatinized starch.
[0088] Comparative Example 3
[0089] A back water putty paste
[0090] The same as Example 1, the only difference is that step 3) is omitted, that is, the silver nano-coating of starch is omitted.
[0091] Comparative Example 4
[0092] A back water putty paste
[0093] Same as Example 1, except that: each raw material is weighed according to the mass fraction recorded in 1@ in Table 2, and step 4) is omitted.
[0094] Comparative Example 5
[0095] A back water putty paste
[0096] Same as Example 1, except that: each raw material is weighed according to the mass fraction recorded in 2@ in Table 2, and step 4) is omitted.
[0097] Comparative Example 6
[0098] A back water putty paste
[0099] The same as Example 1, except that the raw materials are weighed according to the mass fractions recorded in 3@ in Table 2, and the addition of the infiltration crystal in step 6) is omitted.
[0100] Table 2 Raw material dosage (parts)
[0101] raw material 1# 2# 3# Portland cement 30 30 30 Gray calcium 20 20 20 starch 5 5 5 325 mesh silica 20 0 7 2000 mesh silica 0 20 13 Cellulose 5 5 5 Osmotic crystallization 2 2 0 Lubricants 3 3 3 Water reducing agent 3 3 3
[0102] Effect verification:
[0103] The mechanical properties of the back-water putty pastes prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were tested according to the method described in the industry standard JC / T2514-2019, and the test results are shown in Table 3;
[0104] The back-water putty pastes prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were subjected to a mildew resistance test according to the method described in the national standard GB / T1741-2020. The test results are shown in Table 3;
[0105] The back-water putty pastes prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were tested for their antibacterial rates against Escherichia coli and Staphylococcus aureus according to the method described in the national standard GB / T20944.2-2007. The test results are shown in Table 3.
[0106] Table 3 Performance test
[0107]
[0108]
[0109] Note: Negative antibacterial value is recorded as 0.
[0110] It can be seen from Table 3 that the back-water putty paste prepared by the present invention can meet the mechanical properties specified in the industry standards, and the bonding strength is significantly better than the standard state ≥0.50 given in the industry standards, and ≥0.30 after immersion in water.
[0111] It can be seen from Table 3 that the back water putty paste prepared by the present invention can achieve good anti-mildew effect, and the mildew resistance grade reaches level 0.
[0112] It can be seen from Table 3 that the back-water putty paste prepared by the present invention can achieve good antibacterial effect, and the antibacterial rates against Escherichia coli and Staphylococcus aureus are both above 99%.
[0113] It can be seen from Examples 1 to 3 and Comparative Examples 4 to 5 that when the mass ratio of 325 mesh silica to 2000 mesh silica is 2:3.5, the best mildew and antibacterial effect is achieved. Too much or too little addition of 325 mesh silica will have an adverse effect on the final mildew and antibacterial effect.
[0114] It can be seen from Comparative Examples 1 to 3 that the two modification methods of starch, namely, acid modification of starch and coating of silver particles, or the change or lack thereof will have an adverse effect on the final anti-mildew and antibacterial effect.
[0115] It can be seen from Comparative Example 6 that the penetrating crystal is a key filler for mildew prevention and antibacterial properties. If the filler is omitted, dendrite-like crystals cannot be formed, thereby failing to achieve mildew prevention and antibacterial properties.
[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A novel back-water putty paste, characterized in that: The invention comprises the following raw materials in parts by weight: 20 to 40 parts of silicate cement, 10 to 30 parts of lime lime, 1 to 10 parts of modified starch, 10 to 30 parts of composite silicon dioxide, 1 to 10 parts of cellulose, 1 to 5 parts of osmotic crystallizer, 1 to 5 parts of lubricant and 1 to 5 parts of water reducing agent.
2. A novel back-water putty paste according to claim 1, characterized in that: The preparation method of the modified starch comprises the following steps: Step 1, subjecting starch to acid modification treatment to obtain acid-modified starch; Step 2: coating the nano-silver in the acid-modified starch obtained in step 1 to obtain starch-coated nano-silver, namely the modified starch.
3. A novel back-water putty paste according to claim 2, characterized in that: In step 1, the acid modification treatment specifically comprises: dissolving starch in water to form a starch suspension, and then adding an acidic solvent for modification.
4. A novel back-water putty paste according to claim 3, characterized in that: The acidic solvent is hydrochloric acid or acetic acid.
5. A novel back-water putty paste according to claim 2, characterized in that: In step 2, the coating is specifically as follows: dissolving the acid-modified starch in water, then adding the silver nitrate solution, and finally adding the glucose solution drop by drop.
6. A novel back-water putty paste according to claim 1, characterized in that: The composite silicon dioxide is prepared by mixing 325 mesh silicon dioxide and 2000 mesh silicon dioxide, wherein the mass ratio of 325 mesh silicon dioxide to 2000 mesh silicon dioxide is 2:(3-5).
7. A novel back-water putty paste according to claim 1, characterized in that: The osmotic crystal is tartaric acid, sodium silicate or calcium chloride.
8. A method for preparing the novel back-water putty paste according to any one of claims 1 to 7, characterized in that: The following steps are involved: The raw materials are weighed according to the mass parts, the silicate cement, lime lime, modified starch and composite silicon dioxide are premixed, and then cellulose, osmotic crystallization, lubricant and water reducing agent are added and mixed to obtain the novel back-water putty paste.
9. Use of the new water-repellent putty paste as claimed in any one of claims 1 to 7 in wall construction.
Citation Information
Patent Citations
Method for preparing starch core-shell silver antibacterial agent
CN102132709A
Method for preparing nano-silver gel through one-pot method
CN105345029A
Environment-friendly waterproof anti-bacteria putty powder and preparing method thereof
CN105754398A
Method for preparing silver nanoparticles with water-soluble starch
CN106001608A
Neutral environment-friendly putty
CN107057438A