High-wear-resistance matte UV printing ink for printing and preparation method of high-wear-resistance matte UV printing ink

By using components such as polyurethane acrylate, photoinitiator, raw tung oil and modified nanopowder in matte UV ink, a dense cross-linked network is formed, which solves the problem of poor wear resistance of matte UV ink and achieves high efficiency. The ink curing and wear resistance are improved, and it is suitable for the coating protection of digital 3C products.

CN118745299AActive Publication Date: 2024-10-08DELIGAO (HUIZHOU) CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411066403.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-08
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing matte UV inks have poor wear resistance, which leads to the need to increase the coating thickness to improve wear resistance, thereby reducing production efficiency.

Method used

It uses components such as polyurethane acrylate, photoinitiator, tung oil, modified nanopowder dispersion and matting powder, and forms a dense cross-linked network through the use of silane coupling agent KH560 modified nanopowder and tung oil. Improve ink adhesion and wear resistance.

Benefits of technology

It achieves high wear resistance and the printing thickness can be reduced to 3~5um. It can maintain the clarity and integrity of patterns and text after 5,000 times of rubbing, improving the durability of electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979465250000091
    Figure BDA0004979465250000091
  • Figure BDA0004979465250000101
    Figure BDA0004979465250000101
Patent Text Reader

Abstract

The invention discloses high-wear-resistance UV matte ink for printing and a preparation method thereof. The high-wear-resistance UV matte ink for printing comprises the following components: urethane acrylate, a photoinitiator, raw tung oil, a UV monomer, a modified nano powder dispersion liquid, matting powder and an auxiliary agent. Compared with an existing product, the ink has excellent printing adaptability, is fine and stable, not prone to agglomeration, uniform and rapid in drying, rapid and efficient in printing, high in adhesiveness, tough and wear-resistant, the printing thickness is only 3-5 microns when the ink is printed on a digital 3C product, and even if the friction frequency reaches more than 5 thousand times, the ink can be still still still still even if the friction frequency reaches more than 5 thousand times. The definition and integrity of patterns and characters can be guaranteed, the durability of electronic products is greatly improved, and the coating can be widely applied to coating protection of digital 3C products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inks, in particular to a highly wear-resistant matte UV ink for printing and a preparation method thereof. Background Art

[0002] With the progress of society and the gradual improvement of people's material and cultural level, digital 3C electronic products such as computers, communications and consumer electronics and other related manufacturing industries have developed rapidly. Digital 3C electronic products are increasingly developing in the direction of diversified functions, refined performance and personalized decoration. Therefore, it is necessary to print coatings on the surfaces of various components of digital 3C electronic products for decoration, marking or other functional purposes.

[0003] Matte UV ink has the characteristics of soft appearance and strong texture. With the advancement of technology and changes in people's aesthetics, high-end digital 3C electronic products now often require highly wear-resistant UV ink with full matte effect. However, the market is currently dominated by high-gloss UV inks, and matte UV inks are less and not wear-resistant. The wear resistance is difficult to reach more than a thousand times. The poor wear resistance of existing matte UV inks may be caused by the fact that existing matte UV inks contain a large amount of extinction powder and wear-resistant powder, and the ink substrate has poor coating of the powder and poor compatibility. In order to improve the wear resistance, it is often necessary to increase the coating thickness (generally more than 10um), and increasing the coating thickness will lead to an increase in the number of printing times and reduce production efficiency. Therefore, reducing the coating thickness and improving the wear resistance of matte UV inks are technical problems that technicians in this field need to solve urgently. Summary of the invention

[0004] In order to solve the above problems, one of the purposes of this application is achieved by adopting the following technical solution:

[0005] A highly wear-resistant matte UV ink for printing comprises the following components by weight: 26-58 parts of polyurethane acrylate, 7-11 parts of photoinitiator, 5-9 parts of raw tung oil, 17-27 parts of UV monomer, 7-13 parts of modified nano powder dispersion, 5-9 parts of matting powder and 1-5 parts of auxiliary agent.

[0006] Preferably, the polyurethane acrylate has 6 to 15 functional groups. After the high-functionality polyurethane acrylate undergoes a photocuring reaction, a relatively dense cross-linking network is formed, which is beneficial to improving the wear resistance of the finished product.

[0007] Preferably, the photoinitiator is one or more of 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 4-(phenylthio)phenyldiphenylsulfonium hexafluorophosphate, and 4,4'-ditolyliodonium hexafluorophosphate. The above-mentioned photoinitiators have good solubility and reactivity in this system, high initiation efficiency, fast curing speed, and good curing effect.

[0008] Preferably, the UV monomer is one or more of dipentaerythritol hexaacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, 1,6-hexanediol diacrylate, isobornyl methacrylate, and isobornyl acrylate.

[0009] Preferably, the matting powder is talc or precipitated silica.

[0010] Preferably, the auxiliary agent includes at least one of a leveling agent and a defoaming agent.

[0011] Preferably, the defoamer is a silicone defoamer or a polyether defoamer.

[0012] Preferably, the method for preparing the modified nanopowder dispersion comprises the following steps:

[0013] Add 50-70 parts of butyl acetate and 5-15 parts of nano powder into a container, heat to 50-70°C, disperse at high speed for 0.5-1.5 hours, then dropwise add 5-15 parts of silane coupling agent KH560 while stirring, and continue to disperse at high speed for 1-3 hours to obtain a mixture a;

[0014] Add 30-50 parts of UV monomer to another container, heat to 75-85°C and keep warm for 10-30 minutes, then add the above mixture a, continue to keep warm and stir for 1-3 hours at a stirring speed of 3000-8000 r / min to obtain a modified nano powder dispersion.

[0015] Preferably, the nano powder is one or more of nano aluminum oxide, nano zirconium oxide, nano silicon oxide, and nano magnesium oxide. Using silane coupling agent KH560 to modify the nano powder can not only improve the water resistance and corrosion resistance of the ink, but also improve the compatibility of the nano powder with polyurethane acrylate.

[0016] The second purpose of this application is achieved by the following technical solution:

[0017] The above-mentioned method for preparing highly wear-resistant matte UV ink for printing comprises the following steps: adding the above-mentioned mass fractions of polyurethane acrylate, photoinitiator, raw tung oil, UV monomer and modified nano powder dispersion into a container, stirring at 3000-8000 r / min for 10-30 min at 80-120°C to obtain a mixed base material, then cooling the mixed base material to room temperature, adding the above-mentioned mass fractions of auxiliary agent and matting powder into the mixed base material, dispersing at 5000-10000 r / min for 10-20 min at normal temperature and pressure to obtain a finished product. The use of a slightly longer stirring time and a higher stirring speed can enable the defoaming agent to exert the best defoaming effect, eliminate the air generated during the ink production process, enable the various components of the ink to be evenly combined, and improve the overall performance of the ink.

[0018] The beneficial effect is that: the present application adopts silane coupling agent KH560 to modify nano powder to obtain a modified nano powder dispersion that is not easy to agglomerate, which can be evenly dispersed in the system to improve the overall stability of the ink. At the same time, raw tung oil is added to the system. Since raw tung oil has good lubricity, it can improve the compatibility between the raw materials, especially the wetting effect of polyurethane acrylate on the modified nano powder, so that the polyurethane acrylate has a better coating effect on the modified nano powder. In addition, the added raw tung oil reacts with UV monomer during the heating and stirring process to obtain modified raw tung oil. The modified raw tung oil and polyurethane acrylate are cross-linked, and a denser cross-linking network can be formed during the ink curing process to improve the adhesion of the ink; and during the ink curing process, the raw tung oil on the surface of the ink will preferentially absorb UV and solidify compared with the raw tung oil inside, thereby causing micro-wrinkles on the surface of the ink, making the surface of the ink rougher, reducing the specular reflection of light and increasing scattered light, and achieving a matte effect. Compared with existing products, the ink of this application not only has excellent printing adaptability, but also is fine and stable, not easy to agglomerate, dries evenly and quickly, is quick and efficient to print, has strong adhesion, and is tough and wear-resistant. When this ink is printed on digital 3C products, the printing thickness only needs to be 3 to 5 um. Even if the number of frictions reaches more than 5,000 times, the clarity and integrity of the pattern and text can be guaranteed, which greatly improves the durability of electronic products and can be widely used in the coating protection of digital 3C products. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can understand the present invention more clearly.

[0020] The following embodiments are only used to illustrate the present invention, but are not limited to the scope of the present invention. Based on the specific embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work belong to the protection scope of the present invention.

[0021] In the examples of the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art; in the examples of the present invention, unless otherwise specified, the technical means used are conventional means well known to those skilled in the art.

[0022] Source of raw materials:

[0023] Polyurethane acrylate, purchased from Aigenmon International Trading (Shanghai) Co., Ltd.;

[0024] 1-Hydroxycyclohexylphenyl ketone was purchased from Shanghai Myril Biochemical Technology Co., Ltd.;

[0025] 2,4,6-Trimethylbenzoyl-diphenylphosphine oxide was purchased from Hubei Xinninghong Biopharmaceutical Technology Co., Ltd.;

[0026] Ethyl 2,4,6-trimethylbenzoylphenylphosphonate was purchased from Hubei Jianchu Biopharmaceutical Co., Ltd.;

[0027] 2-Methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone was purchased from Hubei Huada Fine Chemical Co., Ltd.;

[0028] 4-(Phenylthio)phenyldiphenylsulfonium hexafluorophosphate (TAS) was purchased from Nanjing Jiazhong Chemical Co., Ltd.;

[0029] 4,4'-Dimethylphenyl iodonium hexafluorophosphate was purchased from Shaanxi Didu New Materials Co., Ltd.;

[0030] Raw tung oil was purchased from Shandong Tongxin Chemical Co., Ltd.;

[0031] Dipentaerythritol hexaacrylate was purchased from Zhongshan Dixin Chemical Co., Ltd.

[0032] Pentaerythritol triacrylate, purchased from Jinan Yunuo Chemical Co., Ltd.;

[0033] Trimethylolpropane triacrylate (TMPTA) was purchased from Zhengzhou Aikemu Chemical Co., Ltd.;

[0034] 1,6-Hexanediol diacrylate, purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd.;

[0035] Isobornyl methacrylate was purchased from Jinan Jinbang Environmental Protection Technology Co., Ltd.;

[0036] Isoborneol acrylate was purchased from Shandong Senya New Materials Co., Ltd.;

[0037] Butyl acetate was purchased from Guangdong Qiming Chemical Technology Co., Ltd.;

[0038] Silane coupling agent KH560 was purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0039] Nano-alumina was purchased from Hubei Huifu Nanomaterials Co., Ltd.;

[0040] Nano-zirconia was purchased from Nanjing Tianxing New Materials Co., Ltd.;

[0041] Nano-silicon oxide was purchased from Hangzhou Jiupeng New Materials Co., Ltd.;

[0042] Nano magnesium oxide was purchased from Hebei Chuangzhiyuan Biotechnology Co., Ltd.;

[0043] Matting powder, purchased from Henan Yilu Chemical Technology Co., Ltd.;

[0044] Talc powder was purchased from Foshan Jinlinda Chemical Co., Ltd.

[0045] Precipitated silica was purchased from Shandong Wanhua Tianhe New Materials Co., Ltd.;

[0046] Leveling agent, purchased from Laiyang Shengbang Silicone Technology Co., Ltd.;

[0047] Defoaming agent, purchased from Shanle Qimin Chemical Technology Co., Ltd.;

[0048] The remaining reagents are commercially available.

[0049] Example 1

[0050] The present embodiment provides a highly wear-resistant matte UV ink for printing, which comprises the following components by weight: 42 parts of polyurethane acrylate, 9 parts of photoinitiator, 7 parts of raw tung oil, 22 parts of UV monomer, 10 parts of modified nano powder dispersion, 7 parts of matting powder, and 3 parts of additives;

[0051] The polyurethane acrylate has 15 functional groups, the photoinitiator is obtained by mixing 1-hydroxycyclohexyl phenyl ketone and 4-(phenylthio)phenyl diphenylsulfonium hexafluorophosphate in a ratio of 1:1 by mass, the UV monomer is obtained by mixing dipentaerythritol hexaacrylate and trimethylolpropane triacrylate in a ratio of 1:1 by mass, the matting powder is talcum powder, and the additive is obtained by mixing a leveling agent and a silicone defoamer in a ratio of 1:1 by mass;

[0052] The preparation method of the above-mentioned highly wear-resistant matte UV ink for printing comprises the following steps: adding the above-mentioned mass fractions of polyurethane acrylate, photoinitiator, raw tung oil, UV monomer and modified nano powder dispersion into a container, stirring at 5000 r / min for 20 min at 100° C. to obtain a mixed base material, then cooling the mixed base material to room temperature, adding the above-mentioned mass fractions of auxiliary agent and matting powder into the mixed base material, dispersing at a high speed of 8000 r / min for 15 min at normal temperature and pressure to obtain a finished product;

[0053] The modified nano powder dispersion is prepared by the following method: 60 parts of butyl acetate, 5 parts of nano alumina and 5 parts of nano silicon oxide are added to a container, heated to 60°C, dispersed at high speed for 1 hour, and then 10 parts of silane coupling agent KH560 are added dropwise while stirring, and the high speed dispersion is continued for 2 hours to obtain a mixture a; 40 parts of UV monomer are added to another container, heated to 80°C and kept warm for 20 minutes, and then the above mixture a is added, and the mixture is kept warm and stirred for 2 hours at a stirring speed of 5000r / min to obtain the modified nano powder dispersion.

[0054] Example 2

[0055] The present embodiment provides a highly wear-resistant matte UV ink for printing, which comprises the following components by weight: 58 parts of polyurethane acrylate, 7 parts of photoinitiator, 5 parts of raw tung oil, 17 parts of UV monomer, 7 parts of modified nano powder dispersion, 5 parts of matting powder, and 1 part of auxiliary agent;

[0056] The polyurethane acrylate has 9 functional groups, the photoinitiator is obtained by mixing 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester and 4,4'-xylyl iodonium hexafluorophosphate in a weight ratio of 2:2:3, the UV monomer is obtained by mixing pentaerythritol triacrylate, 1,6-hexanediol diacrylate and trimethylolpropane triacrylate in a weight ratio of 5:5:7, the matting powder is precipitated silica, and the additive is obtained by mixing a leveling agent and a polyether defoamer in a weight ratio of 1:1;

[0057] The preparation method of the above-mentioned high-wear-resistant matte UV ink for printing comprises the following steps: adding the above-mentioned mass fractions of polyurethane acrylate, photoinitiator, raw tung oil, UV monomer and modified nano powder dispersion into a container, stirring at 8000 r / min for 10 min at 120° C. to obtain a mixed base material, then cooling the mixed base material to room temperature, adding the above-mentioned mass fractions of auxiliary agent and matting powder into the mixed base material, dispersing at a high speed of 10000 r / min for 10 min at normal temperature and pressure to obtain a finished product;

[0058] The modified nano powder dispersion is prepared by the following method: 70 parts of butyl acetate, 2.5 parts of nano zirconium oxide and 2.5 parts of nano silicon oxide are added to a container, heated to 70°C, dispersed at high speed for 0.5h, and then 15 parts of silane coupling agent KH560 are added dropwise while stirring, and high-speed dispersion is continued for 3h to obtain a mixture a; 50 parts of UV monomer are added to another container, heated to 85°C and kept warm for 10min, and then the above mixture a is added, and the mixture is kept warm and stirred for 3h at a stirring speed of 8000r / min to obtain the modified nano powder dispersion.

[0059] Example 3

[0060] The present embodiment provides a highly wear-resistant matte UV ink for printing, which comprises the following components by weight: 26 parts of polyurethane acrylate, 11 parts of photoinitiator, 9 parts of raw tung oil, 27 parts of UV monomer, 13 parts of modified nano powder dispersion, 9 parts of matting powder, and 5 parts of additives;

[0061] The polyurethane acrylate has 6 functional groups, the photoinitiator is obtained by mixing 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone and 4-(phenylthio)phenyl diphenylsulfonium hexafluorophosphate in a ratio of 1:1 by weight, the UV monomer is obtained by mixing isobornyl methacrylate, isobornyl acrylate and trimethylolpropane triacrylate in a ratio of 5:5:7 by weight, the matting powder is talc, and the additive is obtained by mixing a leveling agent and a silicone defoamer in a ratio of 1:1 by weight;

[0062] The preparation method of the above-mentioned high-wear-resistant matte UV ink for printing comprises the following steps: adding the above-mentioned mass fractions of polyurethane acrylate, photoinitiator, raw tung oil, UV monomer and modified nano powder dispersion into a container, stirring at 3000 r / min for 30 minutes at 80° C. to obtain a mixed base material, then cooling the mixed base material to room temperature, adding the above-mentioned mass fractions of auxiliary agent and matting powder into the mixed base material, dispersing at a high speed of 5000 r / min for 20 minutes at normal temperature and pressure to obtain a finished product;

[0063] The modified nano powder dispersion is prepared by the following method: 50 parts of butyl acetate and 15 parts of nano powder are added to a container, heated to 50°C, dispersed at high speed for 1.5 hours, and then 5 parts of silane coupling agent KH560 are added dropwise while stirring, and the high-speed dispersion is continued for 1 hour to obtain a mixture a; 30 parts of UV monomer are added to another container, heated to 75°C and kept warm for 30 minutes, and then the above mixture a is added, and the mixture is continued to be kept warm and stirred for 1 hour at a stirring speed of 3000 r / min to obtain the modified nano powder dispersion.

[0064] Comparative Example 1

[0065] The difference between this comparative example and Example 1 is that epoxy acrylate replaces the polyurethane acrylate in Example 1, and the other components and experimental steps are the same as those in Example 1.

[0066] Comparative Example 2

[0067] The difference between this comparative example and Example 1 is that ordinary nano silicon oxide replaces the modified nano powder dispersion in Example 1, and the other components and experimental steps are the same as those in Example 1.

[0068] Comparative Example 3

[0069] The difference between this comparative example and Example 1 is that the polyurethane acrylate is increased to 49 parts, and raw tung oil is not added. The other components and experimental steps are the same as those in Example 1.

[0070] Comparative Example 4

[0071] The difference between this comparative example and Example 1 is that the polyurethane acrylate is increased to 64 parts and no UV monomer is added. The other components and experimental steps are the same as those in Example 1.

[0072] Performance testing method:

[0073] According to the provisions of the standard CYT 227-2020 "Requirements and Test Methods for the Use of UV-curable Inks for Flexographic Printing": the temperature of the production workshop is controlled at (23±5)°C, and the relative humidity is controlled at (60±20)%RH. Examples 1 to 3 of the present application and comparative examples 1 to 4 are coated on digital 3C electronic products (printing thickness 3 to 5um), and the appearance, glossiness, fineness, viscosity, curing effect, anti-adhesion, bonding fastness and abrasion resistance are tested respectively under the above standard environment. The methods for each performance test are as follows:

[0074] Glossiness: Use a glossiness tester to test the glossiness of the printed product just after drying;

[0075] Fineness: Tested according to the test method in GB / T 13217.3-2008 "Test method for fineness of liquid ink";

[0076] Viscosity: Tested according to the test method in GB / T 13217.4-2008 "Test method for viscosity of liquid ink";

[0077] Surface curing effect: Cut the printed matter that has just been dried into several samples with a length × width of 50mm × 50mm. Place the printed surfaces of two samples face to face and fix them with tape. Place them between two pieces of flat glass with a thickness of 0.5mm that are slightly larger than the samples. Place a 2kg weight on the flat glass. After leaving it at room temperature for 10 minutes, peel it off by hand and observe the surface of the printed matter. If there is no adhesion, it is well cured.

[0078] Deep curing effect: Use a friction tester that complies with ASTM D5264, wrap a 5g weight with cotton yarn, completely wet it with acetone, and gently wipe the surface of the sample back and forth 20 times without the cotton yarn fading (one back and forth counts as one time);

[0079] Anti-adhesion: Cut the printed matter just after drying into several samples with length × width of 50mm × 50mm, stick them face to face and fix them with adhesive tape, place them between two 0.5mm thick flat glass plates, put a 2kg weight on the glass plate, put them in a constant temperature and humidity chamber with a temperature of 50℃ and a humidity of 85%, take them out after 2 hours, peel them off by hand at room temperature, and observe the surface of the printed matter. There is no adhesion or falling off;

[0080] Bonding strength: On the printed pattern, use a grid cutter with a spacing of 2mm to draw cross grids, then use a soft brush to sweep away the surface residue, and then use a test tape (width 19mm) with a peel strength of (0.44±0.01)N / mm to test. The tape and the ink surface of the printed matter should be tightly attached without bubbles. The tape is attached for a length of 50mm and kept for 30s. The tape is peeled off at a 45° angle within 1s and the peeling area is recorded;

[0081] Abrasion resistance: The above ink was printed on an ABS board, and the printed pattern was a square with a length × width of 20 mm × 20 mm. After curing under UV light, the abrasion resistance test was performed. The abrasion resistance test was performed using a rubber abrasion tester. The test rubber was a TEBER CS-10 rubber, with a 500g weight, a test stroke of 50 mm, a lap speed of 60 laps / minute, and one round trip of the rubber was counted as one time. The number of times the pattern began to have gaps or the bottom was exposed was recorded.

[0082] The performance test standards are detailed in Table 1.

[0083] Table 1 Performance test standards

[0084] project Performance requirements Appearance No foreign matter, no lumps Fineness ≤10um Viscosity(MPa.s) 15~100 Glossiness / 60° ≤8 Surface curing effect No adhesion Deep curing effect Wipe the surface of the sample back and forth 20 times without losing color. Anti-adhesion The printed surface should be free of adhesion and ink shedding Bonding strength The ink peeling area of ​​the printed matter should not exceed 10% of the test area. Wear resistance (times) ≥300

[0085] The performance test results of Examples 1 to 3 and Comparative Examples 1 to 4 are shown in Table 2.

[0086] Table 2 Performance test results of Examples 1 to 3 and Comparative Examples 1 to 4

[0087]

[0088]

[0089] From the above Table 2, it can be seen that the inks prepared in Examples 1 to 3 have good appearance characteristics and good matte effect, good surface and deep curing effect, high bonding fastness, strong wear resistance, and the ink is printed on digital 3C products. The printing thickness only needs 3 to 5um. Even if the number of frictions reaches more than 5,000 times, the clarity and integrity of the pattern and text can be guaranteed. Compared with Example 1, it is found that in Example 1, epoxy acrylate replaces polyurethane acrylate, and there is agglomeration, decreased viscosity, increased gloss, poor curing effect, poor anti-adhesion, low bonding fastness, and poor wear resistance. This may be due to the poor compatibility of epoxy acrylate with other components in the system, especially with the modified nanopowder dispersion; Comparative Example 2 replaces the modified nanopowder dispersion with ordinary nano-silicon oxide, and agglomeration also occurs, indicating that the nanopowder can be more evenly dispersed in this system after being modified by the silane coupling agent KH560; Comparative Example 3 does not add raw tung oil, and agglomeration also occurs, and the gloss and wear resistance are also greatly affected. This may be because of the lack of raw tung oil. The compatibility between the raw material components deteriorates, resulting in agglomeration. At the same time, in the absence of raw tung oil, polyurethane acrylate cannot further form a denser cross-linked network, resulting in poor ink adhesion, easy to fall off, and poor wear resistance. In addition, due to the absence of raw tung oil, the ink cannot form micro-wrinkles during the curing process, so the matting effect deteriorates, thereby showing high gloss. In Comparative Example 4, after polyurethane acrylate replaced the UV monomer, the viscosity increased, the gloss decreased, the ink was easy to fall off, and the gloss was not good. The increase in viscosity may be due to the increase in the content of polyurethane acrylate, and the other phenomena may be due to the fact that in the absence of UV monomer, the raw tung oil cannot be modified, resulting in the inability to cross-link with polyurethane acrylate to form a denser network.

[0090] In summary, the present application adopts silane coupling agent KH560 to modify nanopowder to obtain a modified nanopowder dispersion that is not easy to agglomerate, which can be evenly dispersed in the system to improve the overall stability of the ink. At the same time, raw tung oil is added to the system. Since raw tung oil has good lubricity, it can improve the compatibility between the raw materials, especially the wetting effect of polyurethane acrylate on the modified nanopowder, so that the polyurethane acrylate has a better coating effect on the modified nanopowder. In addition, the added raw tung oil reacts with UV monomer during the heating and stirring process to obtain modified raw tung oil. The modified raw tung oil and polyurethane acrylate are cross-linked, and a denser cross-linking network can be formed during the ink curing process, thereby improving the adhesion of the ink; and during the ink curing process, the raw tung oil on the surface of the ink will preferentially absorb UV and cure compared to the raw tung oil inside, thereby causing micro-wrinkles on the surface of the ink, making the surface of the ink rougher, reducing the specular reflection of light and increasing scattered light, thereby achieving a matte effect. Compared with existing products, the ink of this application not only has excellent printing adaptability, but also is fine and stable, not easy to agglomerate, dries evenly and quickly, is quick and efficient to print, has strong adhesion, and is tough and wear-resistant. When this ink is printed on digital 3C products, the printing thickness only needs to be 3 to 5 um. Even if the number of frictions reaches more than 5,000 times, the clarity and integrity of the pattern and text can be guaranteed, which greatly improves the durability of electronic products and can be widely used in the coating protection of digital 3C products.

[0091] The above is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A highly wear-resistant matte UV ink for printing, It is characterized in that The invention comprises the following components in parts by weight: 26 to 58 parts of polyurethane acrylate, 7 to 11 parts of photoinitiator, 5 to 9 parts of raw tung oil, 17 to 27 parts of UV monomer, 7 to 13 parts of modified nano powder dispersion, 5 to 9 parts of matting powder and 1 to 5 parts of auxiliary agent.

2. The highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The polyurethane acrylate has 6 to 15 functional groups.

3. The highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The photoinitiator is one or more of 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 4-(phenylthio)phenyldiphenylsulfonium hexafluorophosphate, and 4,4'-xylyliodonium hexafluorophosphate.

4. The highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The UV monomer is one or more of dipentaerythritol hexaacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, 1,6-hexanediol diacrylate, isobornyl methacrylate, and isobornyl acrylate.

5. The highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The matting powder is talcum powder or precipitated silica.

6. The highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The auxiliary agent includes at least one of a leveling agent and a defoaming agent.

7. The highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The defoamer is an organosilicon defoamer or a polyether defoamer.

8. The highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The modified nano powder dispersion preparation method comprises the following steps: Add 50-70 parts of butyl acetate and 5-15 parts of nano powder into a container, heat to 50-70°C, disperse at high speed for 0.5-1.5 hours, then dropwise add 5-15 parts of silane coupling agent KH560 while stirring, and continue to disperse at high speed for 1-3 hours to obtain a mixture a; Add 30-50 parts of UV monomer into another container, heat to 75-85°C and keep warm for 10-30 minutes, then add the above mixture a, continue to keep warm and stir for 1-3 hours at a stirring speed of 3000-8000 r / min to obtain the modified nano powder dispersion.

9. The highly wear-resistant matte UV ink for printing according to claim 8, It is characterized in that The nano powder is one or more of nano aluminum oxide, nano zirconium oxide, nano silicon oxide and nano magnesium oxide.

10. The method for preparing a highly wear-resistant matte UV ink for printing according to claim 1, It is characterized in that The method comprises the following steps: adding polyurethane acrylate, photoinitiator, raw tung oil, UV monomer and modified nano powder dispersion in the specified mass fraction into a container, stirring at 3000-8000 r / min for 10-30 min under the condition of 80-120 DEG C to obtain a mixed base material, cooling the mixed base material to room temperature, adding auxiliary agent and matting powder in the specified mass fraction into the mixed base material, dispersing at a high speed of 5000-10000 r / min for 10-20 min under the condition of normal temperature and pressure to obtain a finished product.

Citation Information

Patent Citations

  • High-transmittance UV roller coating protective ink and preparation method thereof

    CN114231080A

  • Ultraviolet cured printing ink composition and its uses

    CN1800274A