Light reflective heat-insulating real stone paint with aging resistance and preparation method thereof

The lightweight reflective heat-insulating real stone paint prepared through technical means such as nanocomposite hydrotalcite and nano-TiO2/lightweight polymer hollow microspheres solves the problems of reflective heat-insulating performance and large construction costs in the existing technology, and achieves efficient Reflective insulation and anti-aging while being lightweight and safe.

CN118745321AActive Publication Date: 2024-10-08HEBEI SANKESHU COATING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411021701.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-08
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

While the existing reflective and insulating real stone paint improves the heat insulation performance, it is difficult to ensure the reflective effect of the coating, and the construction amount is large, which poses safety risks. Moreover, the lightweight real stone paint lacks the three-dimensional effect and reflective heat insulation performance of imitation stone.

Method used

It uses nanocomposite hydrotalcite, nanometer TiO2/light polymer hollow microspheres, silane coupling agent modified silica sol-pure acrylic composite emulsion, HALS/UVA compound agent, reflective insulation resin sand, resin color flakes and other raw materials. , a lightweight reflective heat-insulating real stone paint with anti-aging properties is prepared through mechanical mixing, electrostatic self-assembly and stirring to form a dense film structure and improve the reflective heat-insulating performance and anti-aging properties.

Benefits of technology

It achieves excellent anti-aging performance of reflective heat insulation in outdoor environments, reduces the thermal conductivity of the coating, increases reflectivity, reduces construction dosage, enhances the light stability and anti-aging properties of the coating, and is lightweight Design improves safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745321A_ABST
    Figure CN118745321A_ABST
Patent Text Reader

Abstract

The invention relates to a light reflective heat-insulating real stone paint with aging resistance. The coating is characterized by being prepared from the following raw materials in parts by weight: 225 to 275 parts of water, 1.5 to 2.5 parts of a dispersing wetting agent, 5 to 15 parts of nano composite hydrotalcite, 5 to 15 parts of nano TiO2 / light polymer hollow microspheres, 0.5 to 1.5 parts of high-purity nano montmorillonite, 1 to 2 parts of hydroxyethyl cellulose, 1 to 2 parts of a pH regulator, 120 to 180 parts of inorganic-organic composite emulsion, 0.5 to 3.5 parts of a de-foaming agent, 6 to 10 parts of a coalescing agent and 4 to 6 parts of an anti-freezing agent. The reflective heat-insulating coating is prepared from the following components in parts by weight: 100-200 parts of a reflective heat-insulating resin sand, 4-6 parts of a HALS / UVA compound agent, 0.5-1.5 parts of a bactericide, 2-4 parts of a thickening agent, 400-450 parts of reflective heat-insulating resin sand and 100-150 parts of reflective heat-insulating resin color sheets. According to the invention, not only is the contradiction problem between the light weight safety and the reflective heat insulation property of the real stone paint solved, but also the reflective heat insulation property and the excellent ageing resistance under the exposure of an outdoor environment are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of architectural coatings, and in particular to a lightweight reflective heat-insulating real stone paint with anti-aging properties and a preparation method thereof. Background Art

[0002] As the country strengthens ecological environmental protection and people's awareness of energy conservation and environmental protection increases, architectural reflective thermal insulation coatings as a green energy-saving and environmentally friendly coating have received widespread attention. Reflective thermal insulation real stone paint has the advantages of highly realistic imitation stone effect, rich color decoration options, low cost and convenient construction. It not only meets the diversity of building exterior wall decoration, but also can effectively reduce the energy consumption of buildings, reduce urban heat island effect and improve indoor comfort by reflecting solar radiation and reducing heat conduction. It has been widely used in the market.

[0003] However, most of the reflective heat-insulating real stone paints in the industry currently add a certain amount of reflective heat-insulating pigments, aerogels, hollow glass microspheres and other highly reflective or heat-insulating materials to the ordinary real stone paint formula, so as to reflect sunlight or prevent heat transfer. The addition of easily floating raw materials such as aerogels and hollow glass microspheres brings great inconvenience to production and even causes harm to the health of production workers. The addition of reflective heat-insulating titanium dioxide and color paste seriously changes the finishing effect of natural colored sand real stone paint, greatly reduces the sand grain clarity and color fusion of the final coating, reduces the imitation stone effect, etc. It mainly achieves the purpose of reflective heat insulation on the basis of sacrificing properties such as weather resistance and color retention.

[0004] Faced with the limitations of the above products and the contradictions in performance, relevant researchers have taken a series of improvement measures. For example, Chinese patent CN117624992B discloses a reflective heat-insulating real stone paint, which uses two organic silicon substances, sodium methyl silicate and octadecyl trimethoxy chlorosilane, to modify the surface of sepiolite and succinic anhydride and diphenylmethane diisocyanate to modify the internal pore surface of expanded vermiculite to improve the hydrophobicity of the paint film, reduce the thermal conductivity of the paint film, and give the real stone paint excellent and stable thermal insulation performance. However, this patent only improves the thermal insulation performance, and it is difficult to ensure the reflective effect of the coating. At the same time, it is also optimized and improved on the basis of traditional real stone paint. Relying on the natural sand with its own specific gravity, the real stone paint has a large construction dosage, and its coating amount is 3-5kg / m2, which has a large bearing capacity for buildings and poses a safety hazard.

[0005] For example, Chinese patent CN111073415B discloses a light-weight real stone paint without colored sand. By adding hollow glass microspheres and selecting water-based ultra-fine colored rock flakes as raw materials and fillers for the color effect display of the real stone paint, the real stone paint not only has a more gorgeous and rich color effect, but also makes the real stone paint itself lighter and the consumption becomes lower, thereby achieving the purpose of lightness. However, although the coating amount of the real stone paint prepared by the patent is greatly reduced, it is too thin and lacks the three-dimensional effect of imitation stone, and cannot achieve the performance of reflective heat insulation. Summary of the invention

[0006] The present invention provides a lightweight reflective heat-insulating real stone paint with anti-aging properties and a preparation method thereof, which not only solves the contradiction between the lightweight safety and reflective heat-insulating properties of the real stone paint, but also ensures that the reflective heat-insulating performance has excellent anti-aging properties when exposed to an outdoor environment.

[0007] To achieve the above object, the technical solution of the present invention is:

[0008] A lightweight reflective heat-insulating real stone paint with anti-aging properties, characterized in that it is composed of the following raw materials in parts by weight: 225-275 parts of water, 1.5-2.5 parts of dispersing wetting agent, 5-15 parts of nano-composite hydrotalcite, 5-15 parts of nano-TiO2 / light polymer hollow microspheres, 0.5-1.5 parts of high-purity nano-montmorillonite, 1-2 parts of hydroxyethyl cellulose, 1-2 parts of pH regulator, 120-180 parts of inorganic-organic composite emulsion, 0.5-3.5 parts of defoaming agent, 6-10 parts of film-forming aid, 4-6 parts of antifreeze agent, 4-6 parts of HALS / UVA compounding agent, 0.5-1.5 parts of bactericide, 2-4 parts of thickener, 400-450 parts of reflective heat-insulating resin sand, and 100-150 parts of reflective heat-insulating resin color flakes.

[0009] The preparation method of the nano-TiO2 / light polymer hollow microspheres is as follows: mechanically mixing light polymer hollow microspheres and nano-TiO2 in a certain ratio, and obtaining the nano-TiO2 / light polymer hollow microspheres after the mixture is uniformly cooled to room temperature.

[0010] The organic-inorganic composite emulsion is prepared by compounding pure acrylic emulsion and silica sol in a mass ratio of 2:3 to 4:1 and modified by a silane coupling agent. The preparation method is as follows: adding a silane coupling agent (KH570 or KH550) to the silica sol at room temperature and a rotation speed of 200-300 rpm, mixing evenly to obtain an intermediate mixed liquid, then adding the intermediate mixed liquid to the pure acrylic emulsion at a water bath temperature of 40-50°C and a rotation speed of 300-500 rpm, and continuously stirring for 2-3 hours to obtain the organic-inorganic composite emulsion; the silane coupling agent accounts for 3-4% of the total mass of the pure acrylic emulsion and the silica sol;

[0011] The HALS / UVA compound is a compound of a hindered amine light stabilizer and an ultraviolet absorber in a mass ratio of 1:2 to 2:1.

[0012] Furthermore, the nano-composite hydrotalcite is a composite of hydrotalcite and carboxylated multi-walled carbon nanotubes in a mass ratio of 7:3 to 9:1 through an electrostatic self-assembly method. The preparation method is as follows: adding hydrotalcite and carboxylated multi-walled carbon nanotubes into 200-300 ml of deionized water, stirring at a speed of 600-800 rpm for 1-2 hours, then centrifugally washing with deionized water and ethanol, and drying to obtain a gray nano-composite hydrotalcite.

[0013] Furthermore, the particle size of the lightweight polymer hollow microspheres is 35-55 μm;

[0014] The mass ratio of the light polymer hollow microspheres to nano-TiO2 is 2:3 to 1:9;

[0015] The mechanical mixing is to place the light polymer hollow microspheres and nano-TiO2 in a ball mill, with a ball milling time of 30-60 minutes and a rotation speed of 100-300 r / min.

[0016] Furthermore, the reflective heat-insulating resin sand is a compound of reflective heat-insulating resin white sand and reflective heat-insulating resin sand in a mass ratio of 8:1 to 5:1;

[0017] The mesh sizes of the reflective heat-insulating resin sand are 40-80 meshes and 80-120 meshes, and are compounded in a mass ratio of 1:6 to 2:5.

[0018] Furthermore, the thickness of the thermal insulation resin colored sheet is 0.04-0.06 mm;

[0019] The sizes of the thermal insulation resin colored sheets are 8-40 meshes and 14-60 meshes, and the mass ratio is 1:5 to 1:1.

[0020] Furthermore, when the pure acrylic emulsion and the silica sol are modified and composited by a silane coupling agent, the silane coupling agent and the silica sol are first mixed uniformly into an intermediate mixed liquid at room temperature and under stirring, and then the intermediate mixed liquid is added to the pure acrylic emulsion at a water bath temperature of 40-45°C, and stirring is continued for more than 2 hours to obtain the organic-inorganic composite emulsion.

[0021] Furthermore, during the electrostatic self-assembly of the nanocomposite hydrotalcite, the hydrotalcite and carboxylated multi-walled carbon nanotubes are added into deionized water, stirred for 1-2 hours, then washed by centrifugation with deionized water and ethanol, and dried to obtain the nanocomposite hydrotalcite.

[0022] Furthermore, the method for preparing the anti-aging lightweight reflective heat-insulating real stone paint comprises the following steps performed in sequence:

[0023] (1) Add water to a dispersion tank, adjust the speed to 500-700 rpm, add defoamer, dispersing wetting agent, nano-composite hydrotalcite, nano-TiO2 / light polymer hollow microspheres and high-purity nano-montmorillonite in sequence at this dispersion speed, increase the speed to 700-1000 rpm and disperse for 6-10 minutes until the dispersion is completely uniform, keep the speed unchanged, add hydroxyethyl cellulose and pH regulator in sequence, and continue to disperse for 3-5 minutes;

[0024] (2) After the above dispersion is uniform and viscous, reduce the speed to 500-700 rpm, then slowly add the inorganic-organic composite emulsion, continue to disperse for 3-5 minutes, then add the film-forming aid, antifreeze agent, HALS / UVA compound, fungicide and thickener in sequence, and continue to disperse for 5-7 minutes;

[0025] (3) After the above dispersion is uniform and non-agglomerated particles are mixed, add reflective insulation resin sand and reflective insulation resin color sheets, increase the speed to 1200-1500rpm, continue to disperse for 8-10 minutes, reduce the speed to 500-700rpm, and continue to disperse for another 8-10 minutes to obtain a lightweight reflective insulation real stone paint with anti-aging properties.

[0026] The advantages of the present invention are:

[0027] 1. The present invention can prevent the chain initiation and chain growth of the resin caused by ultraviolet light by introducing nano-composite hydrotalcite, and play a role in ultraviolet blocking for reflective heat-insulating resin sand and resin sheet.

[0028] 2. The present invention avoids the dispersion and agglomeration of nano-TiO2 and improves the utilization rate of effective ingredients through surface modification of nano-TiO2 lightweight polymer hollow microsphere composite particles. At the same time, an air film can be formed on the dry paint film, which greatly reduces the thermal conductivity of the coating film and cooperates with the high reflectivity of nano-TiO2 to sunlight to improve the reflective heat insulation performance of the coating.

[0029] 3. The present invention adopts a silica sol-pure acrylic composite emulsion modified by a silane coupling agent. Since the silica sol has a small particle size, it can fill the gaps during the film-forming process, preventing external tiny particle pollutants from being embedded in the coating film, which helps to form a dense film. At the same time, the Si-O bond after the silica sol is formed into a film is an ionic structure with electrical conductivity. It is not easy to generate charge accumulation and thus does not generate static electricity, thus avoiding the coating from absorbing dust in the atmosphere, which leads to a decrease in the reflective performance of the coating.

[0030] 4. The present invention adopts HALS / UVA compound to synergistically increase the protective effect of the coating. UVA absorbs ultraviolet radiation to prevent or delay the degradation of the substrate by ultraviolet light. HALS protects the substrate by capturing free radicals generated during the degradation process. The two have different light stabilization mechanisms, which can minimize the damage of ultraviolet light to the coating and enhance the anti-aging property of the reflective heat insulation performance.

[0031] 5. The present invention adopts reflective heat-insulating resin sand, which has a smooth particle surface, uniform particle size, more stable physical properties, smaller density and specific gravity, and weighs about 0.5 times that of ordinary sand compared to ordinary sand. At the same time, reflective heat-insulating resin color sheets are introduced to replace coarse-grained colored sand as color dots to further reduce the dead weight of the coating. Compared with ordinary real stone paint, it can reduce the consumption by about 75%, thereby achieving the purpose of lightweight. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Comparison of reflectivity and thermal insulation temperature difference of real stone paint prepared in Examples 1-3 and Comparative Examples 1-3

[0033] Figure 2 The reflection performance attenuation index curve of the real stone paint prepared in Examples 1-3 and Comparative Examples 1-3 is shown in FIG. Specific implementation methods

[0035] The specific implementation method of the present invention is described in detail below. The specific implementation method described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0036] Example 1

[0037] The lightweight reflective heat-insulating real stone paint with anti-aging properties in this embodiment is composed of the following raw materials in parts by weight: 275 parts of water, 1.5 parts of dispersing wetting agent, 15 parts of nano-composite hydrotalcite, 15 parts of nano-TiO2 / lightweight polymer hollow microspheres, 0.5 parts of high-purity nano-montmorillonite, 1 part of hydroxyethyl cellulose, 1 part of pH regulator, 120 parts of inorganic-organic composite emulsion, 0.5 parts of defoaming agent, 6 parts of film-forming aid, 4 parts of antifreeze agent, 6 parts of HALS / UVA compounding agent, 0.5 parts of bactericide, 4 parts of thickener, 400 parts of reflective heat-insulating resin sand, and 150 parts of reflective heat-insulating resin color flakes.

[0038] The nano-TiO2 / light polymer hollow microspheres are prepared by the following method: light polymer hollow microspheres and nano-TiO2 are mechanically mixed at a mass ratio of 2:3, and after the mixture is uniformly mixed, the nano-TiO2 / light polymer hollow microspheres are obtained after being cooled to room temperature.

[0039] The organic-inorganic composite emulsion is prepared by compounding pure acrylic emulsion and silica sol in a mass ratio of 2:3 and modified by a silane coupling agent. The preparation method is as follows: adding 3% silane coupling agent KH570 to silica sol at room temperature and a rotation speed of 200 rpm, mixing evenly to obtain an intermediate mixed liquid, then adding the intermediate mixed liquid to the pure acrylic emulsion at a water bath temperature of 40° C. and a rotation speed of 300 rpm, and continuously stirring for 2 hours to obtain the organic-inorganic composite emulsion;

[0040] The HALS / UVA compound is a compound of a hindered amine light stabilizer and an ultraviolet absorber in a mass ratio of 1:2.

[0041] The nanocomposite hydrotalcite of this embodiment is prepared by electrostatic self-assembly of hydrotalcite and carboxylated multi-walled carbon nanotubes in a mass ratio of 7:3. The preparation method is as follows: adding hydrotalcite and carboxylated multi-walled carbon nanotubes into 200 ml of deionized water, stirring at a speed of 600 rpm for 1 hour, washing by centrifugation with deionized water and ethanol, and drying to obtain a gray nanocomposite hydrotalcite.

[0042] The particle size of the lightweight polymer hollow microspheres described in this embodiment is 35-55 μm;

[0043] The mass ratio of the light polymer hollow microspheres to nano-TiO2 is 2:3;

[0044] The mechanical mixing is to place the light polymer hollow microspheres and nano-TiO2 in a ball mill, with a ball milling time of 30 minutes and a rotation speed of 100 r / min.

[0045] The reflective heat-insulating resin sand in this embodiment is a compound of reflective heat-insulating resin white sand and reflective heat-insulating resin sand in a mass ratio of 8:1;

[0046] The mesh sizes of the reflective heat-insulating resin sand are 40-80 meshes and 80-120 meshes, which are compounded at a mass ratio of 1:6.

[0047] The thickness of the thermal insulation resin color sheet in this embodiment is 0.04-0.06mm;

[0048] The sizes of the thermal insulation resin colored sheets are 8-40 mesh and 14-60 mesh, and the mass ratio is 1:5.

[0049] The method for preparing the anti-aging lightweight reflective heat-insulating real stone paint described in this embodiment is characterized by comprising the following steps performed in sequence:

[0050] (1) Add water to a dispersion tank, adjust the speed to 500 rpm, add defoamer, dispersing wetting agent, nano-composite hydrotalcite, nano-TiO2 / light polymer hollow microspheres and high-purity nano-montmorillonite in sequence at this dispersion speed, increase the speed to 700 rpm and disperse for 10 minutes until the dispersion is completely uniform, keep the speed unchanged, add hydroxyethyl cellulose and pH regulator in sequence, and continue to disperse for 5 minutes;

[0051] (2) After the above dispersion is uniform and viscous, reduce the speed to 500 rpm, then slowly add the inorganic-organic composite emulsion, continue to disperse for 5 minutes, then add the film-forming aid, antifreeze agent, HALS / UVA compound, fungicide and thickener in sequence, and continue to disperse for 7 minutes;

[0052] (3) After the above dispersion is uniform and free of agglomerated particles, add reflective insulation resin sand and reflective insulation resin color flakes, increase the speed to 1200 rpm, continue to disperse for 10 minutes, reduce the speed to 500 rpm, and continue to disperse for another 10 minutes to obtain a lightweight reflective insulation real stone paint with anti-aging properties.

[0053] Example 2

[0054] The lightweight reflective heat-insulating real stone paint with anti-aging properties in this embodiment is composed of the following raw materials in parts by weight: 250 parts of water, 2 parts of dispersing wetting agent, 10 parts of nano-composite hydrotalcite, 10 parts of nano-TiO2 / light polymer hollow microspheres, 1 part of high-purity nano-montmorillonite, 1.5 parts of hydroxyethyl cellulose, 1.5 parts of pH regulator, 150 parts of inorganic-organic composite emulsion, 2 parts of defoaming agent, 8 parts of film-forming aid, 5 parts of antifreeze agent, 5 parts of HALS / UVA compounding agent, 1 part of bactericide, 3 parts of thickener, 430 parts of reflective heat-insulating resin sand, and 120 parts of reflective heat-insulating resin color flakes.

[0055] The preparation method of the nano-TiO2 / light polymer hollow microspheres is as follows: mechanically mixing light polymer hollow microspheres and nano-TiO2 in a certain ratio, and obtaining the nano-TiO2 / light polymer hollow microspheres after the mixture is uniformly cooled to room temperature.

[0056] The organic-inorganic composite emulsion is prepared by compounding a pure acrylic emulsion and a silica sol in a mass ratio of 4:3 and modified by a silane coupling agent. The preparation method is as follows: adding 3.5% of a silane coupling agent KH570 to the silica sol at room temperature and a rotation speed of 250 rpm, mixing evenly to obtain an intermediate mixed liquid, then adding the intermediate mixed liquid to the pure acrylic emulsion at a water bath temperature of 45° C. and a rotation speed of 400 rpm, and continuously stirring for 2.5 hours to obtain the organic-inorganic composite emulsion;

[0057] The HALS / UVA compound is a compound of a hindered amine light stabilizer and an ultraviolet absorber in a mass ratio of 1:1.

[0058] The nanocomposite hydrotalcite described in this embodiment is a composite of hydrotalcite and carboxylated multi-walled carbon nanotubes in a mass ratio of 6:1 through an electrostatic self-assembly method. The preparation method is: add hydrotalcite and carboxylated multi-walled carbon nanotubes into 250 ml of deionized water, stir for 1.5 hours at a speed of 700 rpm, then centrifuge and wash with deionized water and ethanol, and dry to obtain a gray nanocomposite hydrotalcite.

[0059] The particle size of the lightweight polymer hollow microspheres described in this embodiment is 35-55 μm;

[0060] The mass ratio of the light polymer hollow microspheres to nano-TiO2 is 1:5;

[0061] The mechanical mixing is to place the light polymer hollow microspheres and nano-TiO2 in a ball mill, with a ball milling time of 45 minutes and a rotation speed of 200 r / min.

[0062] The reflective heat-insulating resin sand in this embodiment is a compound of reflective heat-insulating resin white sand and reflective heat-insulating resin sand in a mass ratio of 6:1;

[0063] The mesh sizes of the reflective heat-insulating resin sand are 40-80 meshes and 80-120 meshes, which are compounded at a mass ratio of 1:4.

[0064] The thickness of the thermal insulation resin color sheet in this embodiment is 0.04-0.06mm;

[0065] The sizes of the thermal insulation resin colored sheets are 8-40 mesh and 14-60 mesh, and the mass ratio is 1:3.

[0066] The method for preparing the anti-aging lightweight reflective heat-insulating real stone paint described in this embodiment is characterized by comprising the following steps performed in sequence:

[0067] (1) Add water to a dispersion tank, adjust the speed to 700 rpm, add defoamer, dispersing wetting agent, nano-composite hydrotalcite, nano-TiO2 / light polymer hollow microspheres and high-purity nano-montmorillonite in sequence at this dispersion speed, increase the speed to 1000 rpm and disperse for 6 minutes until the dispersion is completely uniform, keep the speed unchanged, add hydroxyethyl cellulose and pH regulator in sequence, and continue to disperse for 3 minutes;

[0068] (2) After the above dispersion is uniform and viscous, reduce the speed to 700 rpm, then slowly add the inorganic-organic composite emulsion, continue to disperse for 3 minutes, and then add the film-forming aid, antifreeze agent, HALS / UVA compound, fungicide and thickener in sequence, and continue to disperse for 5 minutes;

[0069] (3) After the above dispersion is uniform and free of agglomerated particles, add reflective insulation resin sand and reflective insulation resin color flakes, increase the speed to 1500 rpm, continue to disperse for 8 minutes, reduce the speed to 700 rpm, and continue to disperse for another 8 minutes to obtain a lightweight reflective insulation real stone paint with anti-aging properties.

[0070] Example 3

[0071] The lightweight reflective heat-insulating real stone paint with anti-aging properties in this embodiment is composed of the following raw materials in parts by weight: 225 parts of water, 2.5 parts of dispersing wetting agent, 5 parts of nano-composite hydrotalcite, 5 parts of nano-TiO2 / lightweight polymer hollow microspheres, 1.5 parts of high-purity nano-montmorillonite, 2 parts of hydroxyethyl cellulose, 2 parts of pH regulator, 180 parts of inorganic-organic composite emulsion, 3.5 parts of defoaming agent, 10 parts of film-forming aid, 6 parts of antifreeze agent, 4 parts of HALS / UVA compounding agent, 1.5 parts of bactericide, 2 parts of thickener, 450 parts of reflective heat-insulating resin sand, and 100 parts of reflective heat-insulating resin color flakes.

[0072] The preparation method of the nano-TiO2 / light polymer hollow microspheres is as follows: mechanically mixing light polymer hollow microspheres and nano-TiO2 in a certain ratio, and obtaining the nano-TiO2 / light polymer hollow microspheres after the mixture is uniformly cooled to room temperature.

[0073] The organic-inorganic composite emulsion is prepared by compounding a pure acrylic emulsion and a silica sol at a mass ratio of 4:1 and modified by a silane coupling agent. The preparation method is as follows: adding 4% silane coupling agent KH550 to the silica sol at room temperature and a rotation speed of 300 rpm, mixing evenly to obtain an intermediate mixed liquid, then adding the intermediate mixed liquid to the pure acrylic emulsion at a water bath temperature of 50° C. and a rotation speed of 500 rpm, and continuously stirring for 3 hours to obtain the organic-inorganic composite emulsion;

[0074] The HALS / UVA compound is a compound of a hindered amine light stabilizer and an ultraviolet absorber in a mass ratio of 2:1.

[0075] The nanocomposite hydrotalcite described in this embodiment is a composite of hydrotalcite and carboxylated multi-walled carbon nanotubes in a mass ratio of 9:1 through an electrostatic self-assembly method. The preparation method is: add hydrotalcite and carboxylated multi-walled carbon nanotubes into 300 ml of deionized water, stir at a speed of 800 rpm for 2 hours, then centrifuge and wash with deionized water and ethanol, and dry to obtain a gray nanocomposite hydrotalcite.

[0076] The particle size of the lightweight polymer hollow microspheres described in this embodiment is 35-55 μm;

[0077] The mass ratio of the light polymer hollow microspheres to nano-TiO2 is 1:9;

[0078] The mechanical mixing is to place the light polymer hollow microspheres and nano-TiO2 in a ball mill, with a ball milling time of 60 minutes and a rotation speed of 300 r / min.

[0079] The reflective heat-insulating resin sand in this embodiment is a compound of reflective heat-insulating resin white sand and reflective heat-insulating resin sand in a mass ratio of 5:1;

[0080] The mesh sizes of the reflective heat-insulating resin sand are 40-80 meshes and 80-120 meshes, which are compounded at a mass ratio of 2:5.

[0081] The thickness of the thermal insulation resin color sheet in this embodiment is 0.04-0.06mm;

[0082] The sizes of the thermal insulation resin colored sheets are 8-40 mesh and 14-60 mesh in a mass ratio of 1:1.

[0083] The method for preparing the anti-aging lightweight reflective heat-insulating real stone paint described in this embodiment is characterized by comprising the following steps performed in sequence:

[0084] (1) Add water to a dispersion tank, adjust the speed to 600 rpm, add defoamer, dispersing wetting agent, nano-composite hydrotalcite, nano-TiO2 / light polymer hollow microspheres and high-purity nano-montmorillonite in sequence at this dispersion speed, increase the speed to 800 rpm and disperse for 8 minutes until the dispersion is completely uniform, keep the speed unchanged, add hydroxyethyl cellulose and pH regulator in sequence, and continue to disperse for 4 minutes;

[0085] (2) After the above dispersion is uniform and viscous, reduce the speed to 600 rpm, then slowly add the inorganic-organic composite emulsion, continue to disperse for 4 minutes, then add the film-forming aid, antifreeze agent, HALS / UVA compound, fungicide and thickener in sequence, and continue to disperse for 6 minutes;

[0086] (3) After the above dispersion is uniform and free of agglomerated particles, add reflective insulation resin sand and reflective insulation resin color flakes, increase the speed to 1300 rpm, continue to disperse for 9 minutes, reduce the speed to 600 rpm, and continue to disperse for another 9 minutes to obtain a lightweight reflective insulation real stone paint with anti-aging properties.

[0087] Comparative Example 1: Commercially available ordinary real stone paint (the colored sand used is natural colored quartz sand).

[0088] Comparative Example 2: Commercially available reflective heat-insulating real stone paint (the colored sand used is reflective heat-insulating calcined quartz sand).

[0089] Comparative Example 3: Commercially available lightweight true stone paint (the color flakes used are water-based ultra-fine colored rock flakes, without colored sand).

[0090] The obtained lightweight reflective heat-insulating real stone paint with anti-aging properties was analyzed and tested accordingly:

[0091] Detection method: The reflective insulation performance detection indicators of the anti-aging lightweight reflective insulation real stone paint prepared in this embodiment include brightness (L*), solar reflectance (TSR), near-infrared reflectance (NIR), hemispherical reflectivity and insulation temperature difference with the reference blackboard, which are measured according to the method specified in the national standard GB / T 25261-2018 "Reflective insulation coating for construction"; the construction coating amount index is based on the outdoor wall construction of the simulated construction site under the same putty and primer, etc., so as to cover the bottom layer and calculate the single square consumption; the anti-aging of reflective insulation performance is in accordance with the national standard GB / T 1865-2009 "Artificial weathering aging and artificial radiation exposure of paints and varnishes to filtered xenon arc radiation", and the Ci5000 xenon lamp artificial weathering tester of ATLAS Company in the United States is used for xenon lamp aging test, and the test conditions are: irradiance (340nm) 0.51W / m 2 ; Relative humidity (40-60)%; Black mark temperature (65±2)℃; Rainfall cycle 18min / 102min (water spraying time / no water spraying time). Conduct 5000h xenon lamp artificial accelerated aging test. Depending on the test object, each 0-500h aging time is an inspection stage. The reflective performance of the anti-aging lightweight reflective insulation real stone paint after aging is inspected, and the initial reflectivity is compared to obtain a statistical reflective performance attenuation index curve.

[0092] Test results: Figure 1The reflectivity of the real stone paint prepared by Examples 1-3 and Comparative Examples 1-3 and the thermal insulation temperature difference comparison with the reference blackboard are shown in the figure. It can be seen from the figure that Comparative Examples 1 and 3 have no reflective thermal insulation performance. The reflective thermal insulation resin sand added in Examples 1-3 is not only lighter than ordinary sand, but also exhibits excellent reflective and thermal insulation performance in the product. The introduction of reflective thermal insulation resin color flakes to replace the coarse sand color dots does not affect the reflective thermal insulation performance of the coating. In addition, the thermal insulation temperature difference bar graph structure with the reference blackboard shows that the thermal insulation temperature difference of Examples 1-3 is about 3-4°C higher than that of Comparative Example 2, which is equivalent to a 4-5°C lower temperature in the building. This is attributed to the introduction of nano-TiO2 / lightweight polymer hollow microspheres in the formula structure of the product of the present invention. Through the introduction of the hollow structure, air is used in the coating as a medium to block heat conduction, which is conducive to improving the thermal insulation capacity of the coating.

[0093] Figure 2 The attenuation index curve of the reflective performance of the real stone paint prepared by Examples 1-3 and Comparative Examples 1-3 shows that with the increase of aging time, the reflective performance of the coating gradually decays, but the attenuation degree of the embodiment is significantly lower than that of the comparative example, which indicates that the anti-aging property of the reflective performance is significantly higher than that of the comparative example. The reason is that the present invention introduces nano-composite hydrotalcite to prevent the reflective insulation resin sand and the resin sheet from causing chain initiation and chain growth of the resin due to ultraviolet light, thereby causing performance failure, and the use of HALS / UVA compounding can synergistically increase the protective effect of the coating, partially absorb the ultraviolet light path before it reaches the surface of the reflective insulation resin sand and the resin sheet, and prevent or delay the degradation of the substrate by ultraviolet light. Under the above dual synergistic protection, the damage of ultraviolet light to the coating is reduced, and the anti-aging property of the reflective insulation performance is enhanced.

[0094] The reflective heat insulation performance and construction coating amount test results of real stone paints of different brightness prepared by different colored sands are shown in Table 1 below:

[0095] Table 1 Test results of different brightness reflective insulation performance and construction coating amount

[0096]

[0097] Since Comparative Examples 1 and 2 do not have reflective heat-insulating properties, Comparative Example 2 was selected to compare the reflective heat-insulating properties and construction coating amounts of Example 1 with relatively better reflective heat-insulating properties at different brightnesses. As shown in Table 1, the addition of different colored sands has a greater impact on the color, reflectance and temperature difference of the coating film, and a smaller impact on the reflectivity. The results show that for the same product, as the brightness continues to increase, the reflectance of the reflective heat-insulating coating and the thermal insulation temperature difference with the reference blackboard also increase, and the reflective performance and thermal insulation performance are better; by comparing Example 2 and Comparative Example 2 at the same brightness, it can be found that the impact on TSR and NIR is relatively small, and the reflectivity of Example 2 is generally higher than that of Comparative Example 2, and the thermal insulation temperature difference with the reference blackboard is also better than that of Comparative Example 2; in addition, through outdoor construction comparison, the coating amount of Example 2 with different brightnesses is 1.2-1.6kg / m 2 , while the coating amount of comparative example 2 is 3.2-4.5kg / m 2 It can be seen that the product of the present invention has high reflective heat insulation performance under different brightness, and at the same time, the construction coating amount is lower, which is lighter and safer.

[0098] The sources of the principles of the above embodiments

[0099] Pure acrylic emulsion Badufu Group Co., Ltd.

[0100] Silica Sol Qingdao Ocean Chemical Co., Ltd.

[0101] Silane coupling agent Jinan Dazuoxing Chemical Co., Ltd.

[0102] Hydrotalcite MacLean Reagent Co., Ltd.

[0103] Multi-walled carbon nanotubes Nanjing Xianfeng Nanomaterials Technology Co., Ltd.

[0104] Hindered Amine Light Stabilizer BASF (China) Co., Ltd.

[0105] UV absorber Longkou Yuxiong Fine Chemical Co., Ltd. Lightweight polymer hollow microspheres Akzo Nobel

[0106] Nano TiO2 Wenxian Medilin Nanomaterial Development Co., Ltd.

[0107] Dispersing and wetting agent Hairun Chemical Co., Ltd.

[0108] High Purity Nano-montmorillonite Zhejiang Fenghong New Materials Co., Ltd.

[0109] Hydroxyethyl Cellulose Shanghai Xinshou Additives Co., Ltd.

[0110] PH RegulatorShanghai Deshangrui Technology Trading Co., Ltd.

[0111] Film-forming agent Dena Chemical Binhai Co., Ltd.

[0112] Antifreeze Xiamen Xinlianfa Import and Export Co., Ltd.

[0113] Fungicide Hofmann Chemical Company

[0114] Thickener Shanghai Xiangyue Industrial Co., Ltd.

[0115] Reflective insulation resin sandSuzhou Hanya Environmental Protection Building Materials Technology Co., Ltd.

[0116] Reflective insulation resin color film Longyancai Building Materials Technology Co., Ltd.

[0117] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A lightweight reflective heat-insulating real stone paint with anti-aging properties, characterized by: The invention is composed of the following raw materials in parts by weight: 225-275 parts of water, 1.5-2.5 parts of dispersing and wetting agent, 5-15 parts of nano composite hydrotalcite, 5-15 parts of nano TiO2 light polymer hollow microspheres, 0.5-1.5 parts of high-purity nano montmorillonite, 1-2 parts of hydroxyethyl cellulose, 1-2 parts of pH regulator, 120-180 parts of inorganic-organic composite emulsion, 0.5-3.5 parts of defoaming agent, 6-10 parts of film-forming aid, 4-6 parts of antifreeze agent, 4-6 parts of HALS / UVA compounding agent, 0.5-1.5 parts of bactericide, 2-4 parts of thickener, 400-450 parts of reflective heat insulation resin sand and 100-150 parts of reflective heat insulation resin color flakes.

2. The nano-TiO2 light polymer hollow microspheres are prepared by the following method: mechanically mixing light polymer hollow microspheres and nano-TiO2 in a mass ratio of 2:3 to 1:9 until uniform, and cooling to room temperature to obtain the nano-TiO2 light polymer hollow microspheres; The inorganic-organic composite emulsion is prepared by compounding pure acrylic emulsion and silica sol in a mass ratio of 2:3 to 4:1 and modified by a silane coupling agent; The HALS / UVA compound is prepared by compounding a hindered amine light stabilizer and an ultraviolet absorber in a mass ratio of 1:2 to 2:

1.

3. The anti-aging lightweight reflective heat-insulating real stone paint according to claim 1 is characterized in that: The nano composite hydrotalcite is composited by hydrotalcite with a mass ratio of 7:3 to 9:1 and carboxyl-containing multi-walled carbon nanotubes through an electrostatic self-assembly method.

4. The anti-aging lightweight reflective heat-insulating real stone paint according to claim 1 is characterized in that: The particle size of the nano-TiO2 lightweight polymer hollow microspheres ranges from 35 to 55 μm; The nano-TiO2 light polymer hollow microspheres are mixed using a ball mill with a ball milling time of 30-60 min and a rotation speed of 100-300 r / min.

5. The anti-aging lightweight reflective heat-insulating real stone paint according to claim 1 is characterized in that: The reflective heat-insulating resin sand is compounded by reflective heat-insulating resin white sand and reflective heat-insulating resin colored sand in a mass ratio of 8:1 to 5:1; The reflective heat-insulating resin sand is compounded with mesh sizes of 40-80 meshes and 80-120 meshes at a mass ratio of 1:6 to 2:

5.

6. The anti-aging lightweight reflective heat-insulating real stone paint according to claim 1, characterized in that: The thickness of the reflective heat-insulating resin colored sheet is in the range of 0.04-0.06 mm; The size of the thermal insulation resin colored sheet is compounded by 8-40 mesh and 14-60 mesh in a mass ratio of 1:5 to 1:

1.

7. The anti-aging lightweight reflective heat-insulating real stone paint according to claim 1, characterized in that: When the pure acrylic emulsion and the silica sol are modified and compounded by a silane coupling agent, the silane coupling agent and the silica sol are first mixed uniformly into an intermediate mixed liquid at room temperature and under stirring, and then the intermediate mixed liquid is added to the pure acrylic emulsion at a water bath temperature of 40-45°C, and stirring is continued for more than 2 hours to obtain the organic-inorganic composite emulsion.

8. The anti-aging lightweight reflective heat-insulating real stone paint according to claim 1, characterized in that: During the electrostatic self-assembly of the nanocomposite hydrotalcite, hydrotalcite and carboxylated multi-walled carbon nanotubes are added into deionized water, and then stirred for 1-2 hours, followed by centrifugal washing with deionized water and ethanol, and drying to obtain the nanocomposite hydrotalcite.

9. A method for preparing a lightweight reflective heat-insulating real stone paint with anti-aging properties as claimed in any one of claims 1 to 7, characterized in that: The method includes the following steps in sequence: (1) Add water to the dispersion tank and adjust the speed to 500-700 rpm. At this dispersion speed, add defoamer, dispersing wetting agent, nano-composite hydrotalcite, nano-TiO2 lightweight polymer hollow microspheres and high-purity nano-montmorillonite, increase the speed to 700-1000 rpm and disperse for 6-10 min until it is completely dispersed. Keep the speed unchanged, add hydroxyethyl cellulose and pH regulator in sequence, and continue to disperse for 3-5 min. (2) After the above dispersion is uniform and viscous, reduce the speed to 500-700 rpm, then slowly add the inorganic-organic composite emulsion, continue to disperse for 3-5 minutes, then add the film-forming aid, antifreeze agent, HALS / UVA compound, fungicide and thickener in sequence, and continue to disperse for 5-7 minutes; (3) After the above dispersion is uniform and free of agglomerated particles, add reflective insulation resin sand and reflective insulation resin color flakes, increase the speed to 1200-1500 rpm, continue to disperse for 8-10 minutes, then reduce the speed to 500-700 rpm, continue to disperse for another 8-10 minutes, and obtain a lightweight reflective insulation real stone paint with anti-aging properties.

Citation Information

Patent Citations

  • Natural stone paint and preparation method thereof

    CN102827522A

  • Hollow polymeric microsphere modified heat-insulating energy-saving coating for exterior wall and preparation method thereof

    CN103232777A

  • Antibacterial and anti-ageing silica sol / polymeric emulsion composite paint as well as preparation method and application thereof

    CN106519859A

  • Elastic reflective thermal-insulation slice, preparation method thereof, stone-like coating and preparation method thereof

    CN108715706A

  • Preparation method for odor-less all-effect latex paint

    CN109266137A