Method for preventing boron ion pollution in brine adsorption lithium extraction process

By adding a regeneration solution elution step in the brine adsorption and lithium extraction process, the problem of poisoning of lithium extraction materials is solved, ensuring the effective extraction of lithium and the removal of boron, and improving the quality of the desorption solution and the stability of the adsorbent.

CN118745510APending Publication Date: 2024-10-08JIANGSU JIUWU HITECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411006426.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

During the process of lithium extraction by brine adsorption, boron ions and lithium ions compete for adsorption sites, causing the lithium extraction material to be poisoned and affecting the adsorption and desorption efficiency. Especially when the boron content in the original brine is high, conventional adsorption and desorption cannot effectively remove boron, resulting in Lithium extraction materials are contaminated with boron salts.

Method used

A regeneration process is added between adsorption and desorption. A high-concentration salt solution of sodium chloride, magnesium chloride, lithium chloride or ammonium chloride with a pH value between 3 and 6 is used as the regeneration solution to elute the adsorbed lithium material. of boron ions, and rinse to remove residual regeneration solution before desorption to ensure effective elution of lithium.

Benefits of technology

It effectively avoids contamination of lithium extraction materials by boron ions, improves the stability of the adsorbent and the quality of the desorption solution, reduces the concentration of impurity ions in the desorption solution, extends the service life of the adsorbent, and improves the quality of lithium salt products. purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745510A_ABST
    Figure CN118745510A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preventing boron ion pollution in a brine adsorption lithium extraction process. The method comprises the following steps: fully contacting brine with a lithium extraction material to complete lithium extraction adsorption; introducing regeneration liquid to elute boron adsorbed on the lithium extraction material; introducing a desorption agent to perform lithium elution on the lithium extraction material subjected to boron elution to obtain a lithium-rich desorption solution; the regeneration liquid is one or a mixture of more of a sodium chloride solution, a magnesium chloride solution, a lithium chloride solution and an ammonium chloride solution with the pH value of 3-6. According to the method, a regeneration process is added between adsorption and desorption, boron adsorbed by a lithium extraction material together with lithium in the adsorption stage can be eluted through the regeneration liquid, and meanwhile, it can be ensured that lithium cannot be eluted together, so that the situation that an adsorbent is polluted by boron ions in brine and consequently the adsorbent loses efficacy is avoided, and the service life of the adsorbent is prolonged. And the quality of the desorption liquid is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preventing boron ion pollution in the process of lithium extraction by brine adsorption, and belongs to the technical field of lithium extraction by adsorption. Background Art

[0002] With the rapid development of the new energy industry, lithium, as the best resource for new energy, has a high strategic application value and is widely used in high-tech industries such as batteries, medical treatment, ceramics, and nuclear energy. Especially in the battery industry, due to the rapid development of the electric vehicle market, technological competition, and subsequent reserves, the upstream brine lithium extraction industry is also developing rapidly.

[0003] At present, the main methods for extracting lithium from brine include adsorption, high-temperature calcination, extraction, etc. Among them, the adsorption method is considered to be the mainstream method today due to its advantages such as good separation effect, green and pollution-free, low cost, and easy operation. The core of the adsorption method lies in the selectivity of the lithium extraction adsorbent for lithium. When the boron content in some brines is high, boron competes with lithium ions for adsorption sites. If the elution and desorption process cannot remove boron in time and enters the next adsorption cycle, it will cause the boron in the lithium extraction material to gradually enrich and occupy more and more adsorption sites that originally belong to lithium, thereby causing the lithium extraction material to be poisoned and affecting the efficiency of lithium adsorption and desorption. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preventing boron ion contamination during brine adsorption lithium extraction, so as to solve the problem in the prior art that when using lithium extraction materials for adsorption lithium extraction, if the boron content in the original brine is high, direct conventional adsorption and desorption will lead to boron salt poisoning of the lithium extraction material, thereby affecting the adsorption and desorption efficiency of the lithium extraction material.

[0005] To achieve the above object, the present invention adopts the following technical solution: A method for preventing boron ion contamination during lithium extraction by brine adsorption, comprising: Fully contact the brine with the lithium extraction material to complete lithium extraction adsorption; Passing regeneration liquid to elute the boron adsorbed on the lithium extraction material; A desorbent is introduced to remove lithium from the lithium-extracting material after boron elution to obtain a lithium-rich desorbent; The regeneration solution is a mixture of one or more of a sodium chloride solution, a magnesium chloride solution, a lithium chloride solution and an ammonium chloride solution with a pH value between 3 and 6.

[0006] Furthermore, before introducing the desorbent to elute lithium, the method further includes: introducing leaching water to remove the regeneration liquid remaining on the lithium extraction material.

[0007] Furthermore, the chloride ion concentration in the regeneration liquid is greater than 100 g / L.

[0008] Furthermore, the lithium extraction material is a material having a selective adsorption function for lithium, such as an aluminum-based adsorbent.

[0009] Furthermore, the brine is a composite salt solution containing lithium ions, such as salt lake brine, concentrated brine, salt production tail water, underground associated brine, etc.

[0010] Furthermore, the elution water is a mixture of one or more of pure water, tap water, industrial fresh water and desorption qualified liquid.

[0011] Furthermore, the desorbent is a mixture of one or more of pure water, tap water, industrial reverse osmosis water and lithium-rich solution.

[0012] Furthermore, the lithium-rich desorption solution is a mixed solution containing one or more ions of lithium ions, sodium ions, potassium ions, calcium ions, magnesium ions and boron ions.

[0013] Compared with the prior art, the present invention has the following beneficial effects: The present invention adds a regeneration process between adsorption and desorption, and uses a regeneration liquid to elute the boron adsorbed by the lithium extraction material together with the lithium in the adsorption stage. Since the regeneration liquid is a high-concentration salt solution, it can ensure that the lithium is not eluted together, thereby avoiding the lithium extraction material from being contaminated by boron ions and causing failure. At the same time, the concentration of impurity ions in the desorption qualified liquid can be reduced, thereby improving the quality of the desorption qualified liquid. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is a flow chart of the method of the present invention; Figure 2 It is a process flow chart of Example 1 and Example 2 of the present invention; Figure 3 It is the process flow chart of comparative example 1 and comparative example 2; Figure 4 is a process flow chart of Example 3 of the present invention; Figure 5 It is the process flow chart of comparative example 3. DETAILED DESCRIPTION

[0015] The present invention will be further described below in conjunction with specific examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the present invention.

[0016] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the present invention belongs.

[0017] In the present invention, the ions to be extracted from the brine are lithium ions, and the brine can be salt lake brine with a high boron content, underground associated water, salt production tail water, etc. In the lithium extraction process, the prior art obtains qualified liquid for subsequent production of lithium salt products through adsorption and desorption of lithium extraction materials. The adsorption process has requirements for the ion composition of the brine. When the boron content is high, it will cause adsorbent poisoning or high concentration of impurity ions in the qualified liquid, affecting the stable operation of the overall process.

[0018] The technical concept of the present invention is to add a regeneration process between adsorption and desorption, and elute the boron adsorbed by the lithium extraction material together with the lithium in the adsorption stage through the regeneration liquid, while ensuring that the lithium is not eluted together, and the lithium extraction material will not be contaminated by boron ions and cause failure. At the same time, the concentration of impurity ions in the qualified liquid can be reduced, and the quality of the desorption qualified liquid can be improved.

[0019] The aluminum-based adsorbent used in the present invention is a product produced by our company.

[0020] like Figure 1 As shown, the present invention provides a method for preventing boron ion contamination in the process of lithium extraction by brine adsorption, comprising the following steps: Step 1, fully contacting the brine with the lithium extraction material to complete lithium extraction adsorption; Step 2, introducing a regeneration liquid to elute the boron adsorbed on the lithium extraction material; Step 3, introducing a desorbent to remove lithium from the lithium-extracting material after boron elution to obtain a lithium-rich desorption solution.

[0021] Before introducing the desorbent to elute lithium, the process also includes: introducing leaching water to remove the regeneration liquid remaining on the lithium extraction material.

[0022] Example 1

[0023] The brine used in this embodiment is old brine from a salt lake as raw material, and the lithium extraction material used is an aluminum-based adsorbent. The concentrations of main ions lithium ion, sodium ion, potassium ion, calcium ion, magnesium ion and boron ion contained in the brine are 1.3g / L, 4.5g / L, 0.5g / L, 0.08g / L, 70g / L and 1.9g / L respectively, and the pH value of the old brine is 6.9. The old brine is passed into a resin column filled with aluminum adsorbent, with 50mL of adsorbent = 1BV, adsorption parameters: adsorption flow rate of 50BV / h, end after 2h of cyclic adsorption, and empty the resin column; the regeneration liquid is passed into the resin column, regeneration parameters: the regeneration liquid is a pure magnesium chloride solution with pH = 6 and chloride ion concentration of more than 180g / L, the flow rate is 20BV / h, the cyclic regeneration ends after 20min, and the resin column is emptied; finally, industrial reverse osmosis fresh water is passed into the resin column, desorption parameters: flow rate of 10BV / h, end after 1h of downstream desorption. The process flow is as follows Figure 2 shown.

[0024] Example 2

[0025] The brine used in this embodiment is raw brine from a salt lake, and the lithium extraction material used is an aluminum-based adsorbent. The concentrations of main ions lithium ion, sodium ion, potassium ion, calcium ion, magnesium ion and boron ion contained in the brine are 0.25g / L, 80g / L, 8g / L, 0.05g / L, 20g / L and 0.8g / L respectively, and the pH value of the raw brine is 7.1. The raw brine is passed into a resin column filled with aluminum adsorbent, with 50 mL of adsorbent = 1 BV, and adsorption parameters: adsorption flow rate is 6 BV / h, and downstream adsorption ends after 2 hours, and the resin column is emptied; the regeneration liquid is passed into the resin column, and the regeneration parameters are: the regeneration liquid is a mixed solution of sodium chloride, lithium chloride and magnesium chloride with a pH of 3 and a chloride ion concentration of more than 100 g / L, and the flow rate is 20 BV / h. The cycle regeneration ends after 20 minutes, and the resin column is emptied; finally, tap water is passed into the resin column, and the desorption parameters are: flow rate 10 BV / h, and downstream desorption ends after 1 hour. The process flow is as follows: Figure 2 shown.

[0026] Example 3

[0027] The brine used in this embodiment is a salt production tail water as raw material, and the lithium extraction material used is an aluminum adsorbent, wherein the concentrations of lithium ions, sodium ions, potassium ions, calcium ions, magnesium ions, and boron ions in the brine are 0.78g / L, 0.5g / L, 0.1g / L, 0.05g / L, 50g / L, and 2.5g / L, respectively, and the pH value of the brine is 7.3. The brine is sent to a continuous ion exchange device equipped with an aluminum adsorbent for lithium extraction, and the process flow is as follows: Figure 4 As shown, columns 1-16 are adsorption areas; column 17 is the top-feeding area; columns 18-23 are desorption areas; columns 24-27 are elution areas; and columns 28-30 are regeneration areas. The desorption area uses pure water, the regeneration area uses a sodium chloride and lithium chloride mixed solution with a pH of 4-5 and a chloride ion concentration of more than 150g / L for cyclic regeneration, and the top-feeding area uses tail halogen. The process flow is as follows Figure 4 shown.

[0028] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that no regeneration process is performed. Figure 3 shown.

[0029] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that no regeneration process is performed. Figure 3 shown.

[0030] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that no regeneration process is performed. Figure 5 shown.

[0031] After 15 cycles of adsorption and lithium extraction experiments using the methods of Examples 1-3 and Comparative Examples 1-3, the adsorption capacity changes of the adsorbents were tested respectively. The test results are shown in Table 1.

[0032] Table 1 Changes in adsorption capacity of adsorbents

[0033] It can be seen from Table 1 that after 15 cycles of cyclic adsorption and lithium extraction experiments, the adsorption capacities of Examples 1-3 were maintained at 3.15 g / L, 2.29 g / L, and 2.52 g / L, respectively, with no obvious downward trend. On the contrary, after 15 cycles of cyclic adsorption and lithium extraction experiments, the adsorption capacities of Comparative Examples 1-3 decreased to 1.02 g / L, 1.36 g / L, and 0.66 g / L, respectively, and the adsorption capacities continued to decrease, indicating that the adsorbent was poisoned, indicating that the regeneration process added during the adsorption and desorption process successfully prevented the contamination of the adsorbent by boron ions in the brine.

[0034] The average values ​​of the ion contents in the desorption solutions obtained after the first three cycles of cyclic adsorption and lithium extraction in Examples 1-3 and Comparative Examples 1-3 were tested respectively, and the test results are shown in Table 2.

[0035] Table 2 Average values ​​of ion content in the desorption solution

[0036] As can be seen from Table 2, after the first three cycles of cyclic adsorption and lithium extraction, the concentrations of boron ions and magnesium ions in the desorption qualified liquid obtained in Examples 1-3 are 1.5-2 times lower than those in the desorption qualified liquid obtained in the corresponding Comparative Examples 1-3, and the lithium ion concentration in the qualified liquid obtained in Examples 1-3 is about 15% higher than that in the corresponding Comparative Examples 1-3, indicating that the regeneration process can significantly reduce the concentration of impurity ions in the desorption qualified liquid and improve the quality of the desorption qualified liquid.

[0037] The present invention adds a new regeneration process to the original adsorption process, thereby avoiding the adsorbent being contaminated by boron ions in the brine and causing the adsorbent to fail, improving the quality of the desorption liquid, reducing the boron-to-lithium ratio of the qualified desorption liquid, reducing the cost of boron removal in the subsequent lithium salt refining stage, and improving the purity of the lithium salt product.

[0038] The present invention has been disclosed above with preferred embodiments, but they are not intended to limit the present invention. Any technical solutions obtained by adopting equivalent replacement or equivalent transformation solutions fall within the protection scope of the present invention.

Claims

1. A method for preventing boron ion contamination during lithium extraction from brine by adsorption, characterized in that: include: Fully contact the brine with the lithium extraction material to complete lithium extraction adsorption; Passing regeneration liquid to elute the boron adsorbed on the lithium extraction material; A desorbent is introduced to remove lithium from the lithium-extracting material after boron elution to obtain a lithium-rich desorbent; The regeneration solution is a mixture of one or more of a sodium chloride solution, a magnesium chloride solution, a lithium chloride solution and an ammonium chloride solution with a pH value between 3 and 6.

2. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 1, characterized in that: Before introducing the desorbent to elute lithium, the process also includes: introducing leaching water to remove the regeneration liquid remaining on the lithium extraction material.

3. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 1, characterized in that: The chloride ion concentration in the regeneration liquid is greater than 100 g / L.

4. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 1, characterized in that: The lithium extraction material is a material that has a selective adsorption function for lithium.

5. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 1, characterized in that: The lithium extraction material is an aluminum-based adsorbent.

6. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 1, characterized in that: The brine is a composite salt solution containing lithium ions.

7. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 2, characterized in that: The rinsing water is a mixture of one or more of pure water, tap water, industrial fresh water and desorption qualified liquid.

8. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 1, characterized in that: The desorbent is a mixture of one or more of pure water, tap water, industrial reverse osmosis water and lithium-rich solution.

9. The method for preventing boron ion contamination during lithium extraction from brine by adsorption according to claim 1, characterized in that: The lithium-rich desorption solution is a mixed solution containing one or more ions of lithium ions, sodium ions, potassium ions, calcium ions, magnesium ions and boron ions.