Method for extracting lithium from salt lake lithium precipitation mother liquor
The electrolysis of the lithium precipitation mother liquor and sodium chloride salt after lithium extraction in salt lake brine is formed by electrolysis of the lithium precipitation mother liquor and sodium chloride salt, and combined with pH adjustment pretreatment, extraction, backextraction and nanofiltration, the high purity of lithium extraction in the lithium precipitation mother liquor of salt lake precipitation is solved. , low cost problem, realizes efficient recycling of lithium and reuse of carbonate, and is suitable for the recycling of lithium resources.
Patent Information
- Application Number
- CN202411058983.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to extract lithium from the lithium deposited mother liquor of salt lakes with high purity, low cost and low acid and alkali use, and waste of carbonate is caused during the lithium extraction process.
Provide a method, including electrolyzing the precipitated lithium mother liquor produced by the salt lake brine after lithium extraction and sodium chloride salt, to generate acid and base as lithium extraction reagent, and to achieve pH adjustment pretreatment, extraction, backextraction and nanofiltration treatment. Lithium is extracted at low cost and efficiently and recycled sodium carbonate solution to reduce resource waste.
It has achieved high-purity extraction of lithium in the lithium deposited mother liquor of salt lake, reduced the cost of acid and alkali use, reduced the waste of carbonate, and is suitable for the recycling of lithium resources. It has environmentally friendly processes and realized the recycling of resources.
Smart Images

Figure BDA0004977233080000061 
Figure BDA0004977233080000071 
Figure BDA0004977233080000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium extraction, and in particular to a method for extracting lithium from lithium-precipitated mother liquor in a salt lake. Background Art
[0002] Lithium is an important rare element that promotes the development of modernization and related industries such as science and technology. It is one of the new energy and strategic resources with the greatest development potential. It is widely used in many fields such as high-energy lithium batteries, rubber industry, aerospace, ceramics, lasers, medicine, welding, explosives, cement, smelting and new energy, and is known as the "energy metal of the 21st century". However, there are many sources of lithium, such as the lithium-containing solution remaining after extracting lithium from salt lake brine, the lithium-containing solution remaining after preparing lithium carbonate or lithium hydroxide by the ore method, the lithium-containing wastewater generated during battery recycling and the lithium-containing solution remaining after preparing lithium carbonate, and the lithium-containing solution remaining after preparing battery-grade lithium carbonate from industrial-grade lithium carbonate. There are still considerable lithium in these solutions. Directly discharging these lithium-containing solutions will not only cause waste of resources, but also cause environmental pollution. Therefore, it is necessary to effectively treat these lithium-containing solutions.
[0003] At present, the main methods for extracting lithium from lithium mother liquor in salt lakes include precipitation, solvent extraction and adsorption. Among them, solvent extraction is the most commonly used extraction technology, which uses the special extraction properties of organic solvents to achieve the purpose of lithium extraction. However, the existing solvent extraction method still has the following problems: (1) a large amount of acid and alkali is used in the extraction and stripping process, and the production cost is high; (2) sodium carbonate is mainly used for lithium precipitation in the process of preparing lithium products, and the lithium mother liquor is reused for extraction, and the alkaline substance carbonate cannot be used, resulting in a waste of resources.
[0004] Based on this, how to provide a method for extracting lithium from lithium mother liquor from salt lakes is one of the technical problems that urgently need to be solved in this field. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for extracting lithium from lithium mother liquor from salt lakes, so as to solve the problem that it is difficult to extract lithium carbonate from lithium mother liquor from salt lakes with high purity, low cost and less acid and alkali usage in the prior art, as well as the waste of carbonate ions caused in the lithium extraction process.
[0006] In order to achieve the above-mentioned purpose, the present invention provides a method for extracting lithium from a lithium precipitation mother liquor in a salt lake, comprising: step S1, providing a lithium-containing solution and sodium chloride salt, wherein the lithium-containing solution is a lithium precipitation mother liquor generated after lithium is extracted from salt lake brine, and the sodium chloride salt is a by-product in the process of preparing potassium fertilizer in the salt lake; step S2, preparing the sodium chloride salt into a sodium chloride salt solution, and obtaining a hydrochloric acid solution and a sodium hydroxide solution after electrolysis of the sodium chloride salt solution; step S3, pre-treating the lithium-containing solution by pH adjustment using a sodium hydroxide solution to obtain a pre-treated lithium-containing solution with a pH of 12 to 14; step S4, extracting lithium ions from the pre-treated lithium-containing solution to obtain a loaded extract and a raffinate; step S5, mixing the loaded extract with a hydrochloric acid solution, and performing stripping to obtain a lithium chloride stripping solution and an unloaded stripping solution; step S6, performing lithium precipitation treatment on the lithium chloride stripping solution to obtain a lithium carbonate product and a lithium precipitation waste liquid; step S7, performing nanofiltration treatment on the lithium precipitation waste liquid to obtain a sodium carbonate filtrate and a chloride salt filtrate.
[0007] Furthermore, in step S1, the pH of the lithium-containing solution is 9 to 12.5.
[0008] Furthermore, in step S2, the mass concentration of the sodium chloride salt solution is 10-12%; preferably, before electrolysis, step S2 also includes adsorption treatment of the sodium chloride salt solution to remove calcium ions and / or magnesium ions in the sodium chloride salt solution.
[0009] Furthermore, the electrolysis voltage in step S2 is 55-65V, the electrolysis current is 70-90A, and the electrolysis treatment time is 30-50min.
[0010] Furthermore, the extraction in step S4 includes: mixing the pretreated lithium-containing solution with the extract to obtain a mixed solution, extracting the mixed solution to obtain a loaded extract and a raffinate; preferably, the volume ratio of the pretreated lithium-containing solution to the extract is (1 to 4): 1; preferably, the number of extractions is 1 to 3, and the time for each extraction is 1 to 10 minutes.
[0011] Further, the extract comprises an extractant and a diluent; preferably, the extractant is selected from trioxythiophene oxide, 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione, 1,1,1,2,2-pentafluoro-6,6-dimethyl-3,5-heptanedione, 1,1,1,2,2,3,3-heptafluoro-7,7-dimethyl-4,6-octanedione, benzoyltrifluoroacetone, trialkyl phosphate, dialkyl phosphate, methyl isobutyl ketone, diketone, 1-phenylazo-2-naphthol, n-octanol, isooctyl alcohol, 2-ethylhexanol, 14-crown-4 ether butylphosphonic acid One or more of dibutyl ester, dibutyl butyl phosphate, methylene tetrabutyl bisphosphate, trioctylamine oxide, 1,10-phenanthroline, quaternary ammonium salt N263, dimethyl di(N-octadecyl)ammonium chloride, methyl dioctyl sulfonium chloride, 1-hydroxyethyl-3-methylimidazole bis(trifluoromethylsulfonyl)imide; preferably, the diluent is selected from one or more of n-hexane, n-dodecane, cyclohexane, D70 special solvent oil, D80 special solvent oil, No. 120 solvent oil, No. 160 solvent oil, No. 200 solvent oil, No. 90 kerosene, aviation kerosene and sulfonated kerosene.
[0012] Furthermore, in step S5, the volume ratio of the loaded extract to the hydrochloric acid solution is (4-8):1; preferably, the stripping is carried out at 0-40°C; preferably, the number of strippings is 1-3, and the time of each stripping is 1-10 minutes; more preferably, step S5 also includes returning the unloaded stripping solution to step S4 and mixing it with the extract.
[0013] Furthermore, the lithium precipitation treatment in step S6 also includes: heating the lithium chloride stripping solution, adding sodium carbonate solution to the lithium chloride stripping solution, stirring the reaction and filtering to obtain a lithium carbonate product and lithium precipitation waste liquid; preferably, the heating temperature is 70 to 90° C.; and the stirring reaction time is 30 to 60 minutes.
[0014] Further, in step S7, the nanofiltration treatment is carried out at a pH of 8 to 12; preferably, the operating pressure of the nanofiltration treatment is 1.5 to 2.5 MPa, and / or the operating temperature of the nanofiltration treatment is 5 to 45° C., and / or the operating time of the nanofiltration treatment is 40 to 100 min.
[0015] Furthermore, step S7 also includes returning the sodium carbonate filtrate to step S6 for lithium precipitation treatment; preferably, step S7 also includes returning the chloride filtrate to step S3, mixing it with the lithium-containing solution and then performing pH adjustment pretreatment; preferably, the chloride salt is sodium chloride and / or lithium chloride.
[0016] By applying the technical scheme of the present invention, lithium is further extracted from the lithium precipitation mother liquor generated after lithium extraction from salt lake brine. At the same time, sodium chloride solid, a by-product in the process of preparing potassium fertilizer from the salt lake, is used for electrolysis to obtain acid and alkali, which are respectively used as reagents in the lithium extraction process. This not only utilizes existing resources and solves the problem of salt storage, but also reduces the cost of using acid and alkali. In the process of lithium extraction, pH adjustment pretreatment, extraction, back extraction, lithium precipitation and nanofiltration treatment are adopted, and multiple processes cooperate with each other to achieve low-cost and high-efficiency extraction of lithium from the lithium precipitation mother liquor. The method is suitable for the recovery and reuse of lithium in various lithium resource processing fields. DETAILED DESCRIPTION
[0017] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0018] As described in the background art, the prior art has the problem of difficulty in extracting lithium carbonate from lithium mother liquor from salt lake sediment with high purity, low cost and less acid and alkali usage, as well as the waste of carbonate ions in the lithium extraction process. In order to solve the above technical problems, the present invention provides a method for extracting lithium from a lithium precipitation mother liquor in a salt lake, comprising: step S1, providing a lithium-containing solution and sodium chloride salt, wherein the lithium-containing solution is a lithium precipitation mother liquor generated after lithium is extracted from salt lake brine, and the sodium chloride salt is a by-product in the process of preparing potassium fertilizer in the salt lake; step S2, preparing the sodium chloride salt into a sodium chloride salt solution, and obtaining a hydrochloric acid solution and a sodium hydroxide solution after electrolysis of the sodium chloride salt solution; step S3, pre-treating the lithium-containing solution by pH adjustment using a sodium hydroxide solution to obtain a pre-treated lithium-containing solution with a pH of 12 to 14; step S4, extracting lithium ions from the pre-treated lithium-containing solution to obtain a loaded extract and a raffinate; step S5, mixing the loaded extract with a hydrochloric acid solution, and performing stripping to obtain a lithium chloride stripping solution and an unloaded stripping solution; step S6, performing lithium precipitation treatment on the lithium chloride stripping solution to obtain a lithium carbonate product and a lithium precipitation waste liquid; step S7, performing nanofiltration treatment on the lithium precipitation waste liquid to obtain a sodium carbonate filtrate and a chloride salt filtrate.
[0019] As mentioned in the background technology, the lithium precipitation mother liquor produced after lithium extraction from salt lake brine still contains considerable lithium. Directly discharging these lithium-containing solutions will not only cause waste of resources, but also cause environmental pollution. Therefore, the present invention provides a low-cost and efficient treatment method for the lithium precipitation mother liquor, so as to achieve effective treatment and reuse of conventional lithium extraction waste liquid, i.e., lithium precipitation mother liquor; in the process of lithium extraction, pH adjustment pretreatment, extraction, back extraction, lithium precipitation and nanofiltration treatment are adopted, and multiple processes cooperate with each other to achieve low-cost and efficient extraction of lithium, which is suitable for the recovery and reuse of lithium in various lithium resource processing fields.
[0020] Specifically, the method provided by the present invention uses sodium chloride solid, a byproduct of the process of preparing potassium fertilizer in salt lakes, and electrolyzes the acid and alkali to be used as reagents in the lithium extraction process, which not only utilizes existing resources, solves the problem of salt storage, but also reduces the cost of using the acid and alkali; before starting the extraction, the present invention also includes adjusting the pH of the lithium-containing solution to be extracted to 12.5-14 by electrolyzing the alkaline solution obtained. During the extraction process, the extract can accurately capture Li+ from the lithium-containing solution, and the two phases are fully in contact. Under alkaline conditions, the hydrogen ions in the extract (R) exchange with the Li+ in the lithium-containing solution as follows:
[0021] R-H+Li+→R-Li+H+H++OH-→H2O
[0022] Li+ enters the extracting liquid through exchange, and the presence of hydroxide accelerates the exchange process, thereby greatly improving the efficiency of lithium extraction. Compared with an unadjusted lithium-containing solution with a pH value less than 12, the Li+ exchange can be completed in a very short time, which is conducive to application in large-scale industrial production, ensuring efficient production and achieving a breakthrough from science and technology to scientific and technological production; the lithium-containing solution pretreated by pH adjustment is extracted and stripped to achieve initial extraction of lithium with a high extraction rate, and then lithium precipitation treatment is performed to obtain a lithium carbonate product with a high yield; and the present invention also includes nanofiltration treatment of the lithium precipitation waste liquid after lithium precipitation to achieve zero emission and zero waste, thereby achieving lithium extraction with extremely high environmental friendliness.
[0023] In a typical embodiment, the pH of the lithium-containing solution in step S1 is 9 to 12.5. As mentioned above, the lithium-containing solution targeted by the present invention is a lithium-precipitated mother liquor produced after lithium extraction from salt lake brine. When its pH is 9 to 12.5, it can be better adapted to the process provided by the present invention, thereby achieving a higher lithium extraction rate. After a large number of experiments, the inventors found that in several more typical embodiments, the pH of the lithium-containing solution is preferably 13.2 to 13.5, and found that the lithium recovery rate is higher at this time, and the yield of the final lithium carbonate product is higher, while the cost is lower.
[0024] For the acid and alkali used in the process, the present invention selects the sodium chloride salt, a byproduct of the process of preparing potassium fertilizer from salt lakes, and electrolyzes it to provide. In a preferred embodiment, the mass concentration of the sodium chloride salt solution in step S2 is 10-12%. The inventor has selected this mass concentration range through a large number of experiments on the concentration selection of the electrolytic raw material sodium chloride salt solution, and found that when its mass concentration is within this range, the reaction rate of electrolysis is more suitable, and sodium hydroxide alkali solution and hydrochloric acid solution can be obtained with a higher yield, thereby improving the efficiency and industrial value of the entire lithium extraction process. In a more preferred embodiment, because the sodium chloride salt, a byproduct of the process of preparing potassium fertilizer from salt lakes, contains more calcium and magnesium, before electrolysis, it also includes adsorption treatment of the sodium chloride salt solution to remove calcium ions and / or magnesium ions in the sodium chloride salt solution, and the specific adsorption method is resin adsorption. By adsorbing these two divalent cations before electrolysis, it is possible to more effectively avoid the occurrence of side reactions in the electrolysis process, such as the generation of calcium hydroxide and magnesium hydroxide precipitation, blocking the electrolysis equipment, causing equipment damage, and also improving the output of sodium hydroxide and hydrochloric acid. This will reduce costs and increase the added value of products obtained by extracting lithium from lithium-containing mother liquor.
[0025] In order to significantly improve the efficiency of the electrolysis process and thus shorten the process cycle of lithium extraction, in several typical embodiments, the inventors have adjusted the relevant parameters involved in the electrolysis process through a large number of experiments, and for the specific raw materials in the method provided by the present invention (i.e., the sodium chloride salt solution as a byproduct in the process of preparing potassium fertilizer from salt lakes with a mass concentration of 10-12%), it is preferred that the electrolysis voltage is 55-65V, the current is 70-90A, and the power-on treatment time is 30-50min.
[0026] The lithium-containing solution after pH adjustment treatment enters the extraction section. In a preferred embodiment, the extraction in step S4 includes: mixing the pretreated lithium-containing solution with the extract to obtain a mixed solution, extracting the mixed solution to obtain a loaded extract and a raffinate. Compared with the commonly used extraction method in the art, the extraction method adopted by the present invention is countercurrent extraction. In the countercurrent extraction, the raw material liquid and the extract flow in the same direction in the extractor, but the flow paths are opposite. This flow mode allows the raw material liquid and the extract to continuously contact and separate alternately in the extractor, and the operation is flexible, thereby achieving the extraction of the target component. It can handle extraction systems with low distribution ratios or separation coefficients, thereby improving the extraction selectivity of specific metal ions, and ultimately by appropriately increasing the number of stages, a good separation effect and a high extraction rate can be achieved. Compared with the traditional cross-current extraction method, the countercurrent extraction method has relatively low equipment investment, is suitable for large-scale preparation, and has relatively low difficulty in operation and maintenance, which greatly improves production efficiency.
[0027] In order to improve the extraction effect, the inventors conducted a large number of experiments and found that in a typical embodiment, the volume ratio of the pretreated lithium-containing solution to the extraction solution is preferably (1-4):1, and it is found that at this volume ratio, it is more conducive to the initial extraction of lithium ions in the pretreated lithium-containing solution; in a more typical embodiment, the inventors further preferred that the number of extractions is 1-3, and the time for each extraction is 1-10 minutes, and it is found that extraction under such conditions can achieve lithium extraction with a higher extraction rate, thereby improving the lithium extraction rate.
[0028] Further, the extract comprises an extractant and a diluent; for the lithium extraction process of the present invention, in the extraction stage, the inventors prefer that the extractant is selected from trioxythiophene oxide, 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione, 1,1,1,2,2-pentafluoro-6,6-dimethyl-3,5-heptanedione, 1,1,1,2,2,3,3-heptafluoro-7,7-dimethyl-4,6-octanedione, benzoyltrifluoroacetone, trialkyl phosphate, dialkyl phosphate, methyl isobutyl ketone, diketone, 1-phenylazo-2-naphthol, n-octanol, isooctyl alcohol, 2-ethylhexanol, 1 One or more of 4-crown-4-ether butylphosphonic acid dibutyl ester, dibutyl butyl phosphate, methylene tetrabutyl bisphosphate, trioctylamine oxide, 1,10-phenanthroline, quaternary ammonium salt N263, dimethyl di(N-octadecyl)ammonium chloride, methyl dioctyl sulfonium chloride, 1-hydroxyethyl-3-methylimidazole bis(trifluoromethylsulfonyl)imide; at the same time, the preferred diluent is selected from one or more of n-hexane, n-dodecane, cyclohexane, D70 special solvent oil, D80 special solvent oil, No. 120 solvent oil, No. 160 solvent oil, No. 200 solvent oil, No. 90 kerosene, aviation kerosene and sulfonated kerosene. Compared with the commonly used strong acid extraction liquid system such as hydrochloric acid and sulfuric acid in the art, the present invention preferably uses the above-mentioned hydrophobic liquid as the extraction agent, mixes it with the above-mentioned diluent as the extraction liquid, and effectively improves the safety and service life of the equipment.
[0029] Regarding the selection of the extracting liquid, in several typical embodiments, the inventors provide the following after a large number of experiments: the extracting agent is 1,1,1,2,2,3,3-heptafluoro-7,7-dimethyl-4,6-octanedione and benzoyltrifluoroacetone, the diluent is n-hexane, and the volume proportion of the extracting agent in the extracting liquid is 45%; or, the extracting agent is benzoyltrifluoroacetone and trialkyl phosphate, the diluent is D80 special solvent oil, and the volume proportion of the extracting agent in the extracting liquid is 50%. Because the above-mentioned extracting liquid system is more suitable for the lithium-containing solution system to be extracted in the present invention, the extraction rate of lithium is further improved.
[0030] After extraction, a loaded extract and a raffinate are obtained, and then the loaded extract is mixed with a hydrochloric acid solution for stripping; in several preferred embodiments, the volume ratio of the loaded extract to the hydrochloric acid solution is (4-8): 1. The inventor has found through a large number of experiments that mixing the two at this volume ratio and stripping can more effectively enhance the stripping effect, thereby improving the extraction rate of lithium. Preferably, the stripping is carried out at 0-40°C, which is conducive to the full mixing of the loaded extract and the hydrochloric acid solution and rapid phase separation. The hydrochloric acid solution will not solidify due to too low a temperature (below 0°C), nor will the extract components volatilize due to too high a temperature, affecting its performance, thereby ensuring the stripping efficiency. And more preferably, the number of strippings is 1-3, and the time for each stripping is 1-10 minutes; after a large number of experiments, the inventor has preferably selected the relevant process conditions of stripping as above, and found that under the above conditions, the extraction rate of lithium is higher, and a shorter process cycle can also be achieved.
[0031] In a more preferred embodiment, step S5 also includes returning the empty stripping solution to step S4, mixing it with the extracting solution, and recycling it again, thereby effectively reducing the production cost in the lithium extraction process, while reducing the generation of waste liquid and reducing environmental pollution.
[0032] In order to further improve the efficiency of lithium precipitation treatment, the lithium precipitation treatment in step S6 also includes: heating the lithium chloride stripping solution, adding sodium carbonate solution to the lithium chloride stripping solution, stirring the reaction and filtering to obtain a lithium carbonate product and a lithium precipitation waste liquid. The present invention uses sodium carbonate solution to perform the final lithium precipitation process on the lithium chloride stripping solution. Compared with other lithium precipitation reagents such as sodium phosphate, sodium fluoride, etc., the sodium carbonate solution can be better adapted to the lithium extraction system of the present invention, thereby effectively improving the yield of lithium-containing products; in a more preferred embodiment, the heating temperature is 70 to 90°C; the stirring reaction time is 30 to 60 minutes; the inventor has optimized the two experimental conditions of temperature and reaction time involved in the lithium precipitation process through a large number of experiments, and found that under this experimental condition, the combination of lithium ions and carbonate ions can be more effectively achieved, the reaction rate is more suitable, and the yield of the obtained lithium carbonate product is also higher.
[0033] As described above, the method provided in the present application includes nanofiltration treatment of lithium precipitate waste liquid after lithium precipitation, and in order to improve the effect of nanofiltration treatment, in a typical embodiment, the nanofiltration treatment in step S7 is carried out at a pH of 8 to 12. And, because the present application is directed to nanofiltration of lithium precipitate waste liquid, its purpose is to effectively separate monovalent ions from divalent carbonate ions. The principle is based on the Donnan effect, which affects the performance of the membrane when charged particles approach the semi-permeable membrane, and sometimes even affects the performance of both sides of the membrane. Ions of different valence states have different fluxes when passing through the nanofiltration membrane. Generally, the flux of high-valent ions is smaller than that of low-valent ions. This is because high-valent ions carry more charges and tend to interact with the charges on the membrane surface, thereby being repelled or adsorbed on the membrane, reducing its flux through the membrane. Therefore, the carbonate retention rate is much greater than that of monovalent chloride ions. Therefore, the present invention is aimed at the target system involved in the nanofiltration process, and the operating conditions of the nanofiltration treatment are preferably selected, so that the chloride ions can pass through the membrane, and the carbonate ions are retained outside the membrane, thereby efficiently realizing the separation and enrichment of carbonate ions, improving its recovery rate, and at the same time increasing the product added value of the lithium-containing products obtained by lithium extraction. In a more preferred embodiment, the inventors have optimized the operating pressure of the nanofiltration treatment to be 1.5-2.5Mpa, the operating temperature to be 5-45°C, and the operating time to be 40-80min through a large number of experiments; and found that the nanofiltration treatment under these conditions has a better effect and can more efficiently achieve the enrichment of carbonate ions.
[0034] In a typical embodiment, step S7 also includes returning the sodium carbonate filtrate to step S6 for lithium precipitation treatment, so as to reduce the amount of sodium carbonate solution used in the lithium precipitation treatment process of step S6, further reduce costs, and improve the recycling rate of resources; and more preferably, step S7 also includes returning the chloride filtrate to step S3, mixing it with the lithium-containing solution and performing pH adjustment pretreatment, so as to recycle and extract part of the lithium that may still remain in the chloride filtrate, thereby improving the recovery rate of lithium in the entire method of extracting lithium from the lithium precipitation mother liquor of the salt lake. Preferably, the chloride salt is sodium chloride and / or lithium chloride.
[0035] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0036] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0037] Example 1
[0038] A method for extracting lithium from lithium mother liquor from salt lakes:
[0039] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 48.8ppm, and after being removed by resin ion exchange, it is reduced to below 0.1ppm, which is the ion exchange liquid (hereinafter referred to as ion exchange liquid). The ion exchange liquid is added to the bipolar membrane device, and the voltage and current are set to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0040]
[0041] Take 20L of lithium precipitation mother liquor with pH=10, in which the lithium content is 1.35g / L, add 0.315L of 7.4% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.33g / L.
[0042] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred and extracted for 3 minutes, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.6L of a 6.5% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 3 minutes, and the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0043] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty extract was 0.265 g / L, and the lithium content in the lithium chloride stripping solution was 11.968 g / L.
[0044] Use sodium carbonate solid to prepare 870g of 20% sodium carbonate solution, take 1.6L of lithium chloride stripping solution with a lithium content of 11.968g / L, heat it to 70°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 30min, filter to obtain a lithium carbonate product and lithium precipitation waste liquid, the amount of lithium precipitation waste liquid is 2.307L, the lithium content is 1.6251g / L, pH=11.01, and the carbonate content is 0.2326mol / L.
[0045] Take 2.307L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.850L of monovalent chloride solution (i.e., a mixed solution of lithium chloride and sodium chloride, the same below) and 0.457L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.457L of sodium carbonate filtrate is 1.12mol / L, and the sodium carbonate concentration is 10.79%. Repeat the above operation to prepare a sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0046] Example 2
[0047] A method for extracting lithium from lithium mother liquor from salt lakes:
[0048] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 49.5ppm, which is reduced to below 0.1ppm after resin adsorption. Add the adsorbed water sample to the bipolar membrane device, set the voltage and current to 60V and 80A respectively, and the power-on time is 40min. The treatment results are shown in the table below:
[0049]
[0050] Take 20L of lithium precipitation mother liquor with pH=10.5, in which the lithium content is 1.402g / L, add 0.96L of 8.09% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 13, the lithium content in the solution is 1.337g / L.
[0051] First, 2L of 1,1,1,2,2,3,3-heptafluoro-7,7-dimethyl-4,6-octanedione, 2.5L of benzoyltrifluoroacetone and 5.5L of n-hexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of 1,1,1,2,2,3,3-heptafluoro-7,7-dimethyl-4,6-octanedione and benzoyltrifluoroacetone accounted for 45%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 15°C, with each stage being stirred and extracted for 5min, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.8L of a 7.4% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 5min, and the temperature was 15°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0052] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty raffinate was 0.006 g / L, and the lithium content in the lithium chloride stripping solution was 13.31 g / L.
[0053] Take 1.8L of lithium chloride stripping solution with a lithium content of 13.31g / L, heat it to 80°C, slowly add 2018g of 10.79% sodium carbonate solution (sample prepared in Example 1), stir the reaction for 50min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 3.597L, the lithium content is 1.3262g / L, the pH is 10.18, and the carbonate content is 0.1891mol / L.
[0054] Take 3.597L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 60 minutes under the conditions of pressure 1.8Mpa and temperature 20℃, and obtain 3.170L of monovalent chloride solution and 0.523L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.523L sodium carbonate filtrate is 1.248mol / L, and the sodium carbonate concentration is 12.02%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0055] Example 3
[0056] A method for extracting lithium from lithium mother liquor from salt lakes:
[0057] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 45.9ppm, which is reduced to below 0.1ppm after resin adsorption. Add the adsorbed water sample to the bipolar membrane device, set the voltage and current to 60V and 80A respectively, and the power-on time is 50min. The treatment results are shown in the table below:
[0058]
[0059] Take 20L of lithium precipitation mother liquor with pH=11, in which the lithium content is 1.39g / L, add 3.398L of 8.11% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 13.5, the lithium content in the solution is 1.188g / L.
[0060] First, 2.5L of benzoyltrifluoroacetone, 2.5L of trialkyl phosphate and 5L of D80 special solvent oil are taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of benzoyltrifluoroacetone and trialkyl phosphate accounts for 50%; then 10L of the extract is taken and mixed with 22L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation is performed at a temperature of 25°C, with each stage being stirred and extracted for 8min, and finally the raffinate and the lithium-containing extract are separated; 10L of the lithium-containing extract is taken, 1.8L of a 7.41% concentration hydrochloric acid solution obtained by electrolysis is added thereto, and a two-stage countercurrent stripping operation is performed, with each stage being stirred and mixed for 8min, and the temperature is 25°C, and finally the empty extract and the lithium chloride stripping solution are separated.
[0061] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty raffinate was 0.007 g / L, and the lithium content in the lithium chloride stripping solution was 14.434 g / L.
[0062] Take 1.8L of lithium chloride stripping solution with a lithium content of 14.434g / L, heat it to 85°C, slowly add 1970g of 12.02% sodium carbonate solution (sodium carbonate filtrate obtained by nanofiltration treatment in Example 2), stir the reaction for 50min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 3.534L, the lithium content is 1.4289g / L, the pH is 10.35, and the carbonate content is 0.2078mol / L.
[0063] Take 3.534L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 70 minutes under the conditions of pressure 2.0Mpa and temperature 30℃, and obtain 3.115L of monovalent chloride solution and 0.419L of sodium carbonate solution. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.419L sodium carbonate solution is 1.701mol / L, and the sodium carbonate concentration is 15.74%. Repeat the above operation to prepare a sodium carbonate solution of corresponding concentration, which is reused in the front-end lithium precipitation.
[0064] Example 4
[0065] A method for extracting lithium from lithium mother liquor from salt lakes:
[0066] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 12% sodium chloride aqueous solution, in which the calcium and magnesium content is 54.8ppm, which is reduced to below 0.1ppm after resin adsorption. Add the adsorbed water sample to the bipolar membrane device, set the voltage and current to 60V and 80A respectively, and the power-on time is 40min. The treatment results are shown in the table below:
[0067]
[0068] Take 20L of lithium precipitation mother liquor with pH=10.4, in which the lithium content is 1.431g / L, add 3.32L of 8.06% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 13.3, the lithium content in the solution is 1.227g / L.
[0069] First, take 5L of trioctylamine oxide and 5L of No. 120 solvent oil, mix them evenly in a separatory funnel to obtain an extract, in which the volume of trioctylamine oxide accounts for 50%; then take 10L of the extract, mix it with 23L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and use a two-stage countercurrent extraction operation at a temperature of 35°C, stirring and extracting for 10 minutes at each stage, and finally separating the raffinate and the lithium-containing extract; take 10L of the lithium-containing extract, add 1.9L of 7.38% concentration hydrochloric acid solution obtained by electrolysis, use a two-stage countercurrent stripping operation, stirring and mixing for 10 minutes at each stage, and the temperature is 35°C, and finally separate the empty extract and the lithium chloride stripping solution.
[0070] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty extract was 0.010 g / L, and the lithium content in the lithium chloride stripping solution was 14.7313 g / L.
[0071] Take 1.9L lithium chloride stripping solution with a lithium content of 14.7313g / L, heat it to 85°C, slowly add 1628g of 15.74% sodium carbonate solution (sodium carbonate filtrate obtained by nanofiltration treatment in Example 3), stir the reaction for 60min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 3.276L, the lithium content is 1.3945g / L, the pH is 10.61, and the carbonate content is 0.2259mol / L.
[0072] Take 3.276L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 80 minutes under the conditions of pressure 2.0Mpa and temperature 40℃, and obtain 2.943L of monovalent chloride solution and 0.333L of sodium carbonate solution. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.333L sodium carbonate solution is 2.153mol / L, and the sodium carbonate concentration is 19.34%. Repeat the above operation to prepare a sodium carbonate solution of corresponding concentration, which is reused in the front-end lithium precipitation.
[0073] Example 5
[0074] A method for extracting lithium from lithium mother liquor from salt lakes:
[0075] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 49.5ppm, which is reduced to below 0.1ppm after resin adsorption. Add the adsorbed water sample to the bipolar membrane device, set the voltage and current to 60V and 80A respectively, and the power-on time is 40min. The treatment results are shown in the table below:
[0076]
[0077] Take 20L of lithium precipitation mother liquor with pH=10.48, in which the lithium content is 1.39g / L, add 3.319L of 8.03% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 13.3, the lithium content in the solution is 1.192g / L.
[0078] First, 2L of 1-phenylazo-2-naphthol, 3L of n-octanol and 5L of n-dodecane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of 1-phenylazo-2-naphthol and n-octanol accounted for 50%; then 10L of the extract was taken and mixed with 22.5L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 30°C, with each stage being stirred and extracted for 5min, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.85L of a 7.4% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 5min, and the temperature was 30°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0079] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty extract was 0.074 g / L, and the lithium content in the lithium chloride stripping solution was 13.596 g / L.
[0080] Take 1.85L of lithium chloride stripping solution with a lithium content of 13.596g / L, heat it to 90°C, slowly add 1182g of 19.34% sodium carbonate solution (sodium carbonate filtrate obtained by nanofiltration treatment in Example 4), stir the reaction for 50min, filter to obtain a lithium carbonate product and lithium precipitation waste liquid, the amount of lithium precipitation waste liquid is 2.810L, the lithium content is 1.4200g / L, pH=10.74, and the carbonate content is 0.2276mol / L.
[0081] Take 2.87L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 70min under the conditions of pressure 2.5Mpa and temperature 40℃, and obtain 2.52L of monovalent chloride solution and 0.290L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.290L sodium carbonate filtrate is 2.0775mol / L, and the sodium carbonate concentration is 18.80%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0082] Example 6
[0083] A method for extracting lithium from lithium mother liquor from salt lakes:
[0084] The only difference between this embodiment and embodiment 1 is that the initial pH of the lithium precipitation mother solution is selected to be 9.0, and the other operation and process conditions remain unchanged. Specifically:
[0085] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 48.8ppm, and after being removed by resin ion exchange, it is reduced to below 0.1ppm, which is the post-ion exchange liquid. Add the post-ion exchange liquid to the bipolar membrane device, set the voltage and current to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0086]
[0087] Take 20L of lithium precipitation mother liquor with a pH of 9, in which the lithium content is 1.348g / L, add 0.3244L of 7.39% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, and when the pH is increased to 12.5, the lithium content in the solution is 1.3265g / L.
[0088] As the pH of the lithium precipitation mother liquor decreases, it affects the subsequent extraction alkali adjustment pretreatment. The lower the pH of the mother liquor, the greater the amount of alkali consumed to adjust the alkali to the corresponding extraction pH (compared with Example 1, 0.315L increased to 0.3244L).
[0089] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred and extracted for 3 minutes, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.6L of a 6.49% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 3 minutes, and the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0090] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the raffinate is 0.2643 g / L, and the lithium content in the lithium chloride stripping solution is 11.9497 g / L.
[0091] Use sodium carbonate solid to prepare 870g of 20% sodium carbonate solution, take 1.6L of lithium chloride strip solution with a lithium content of 11.9497g / L, heat it to 80°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 40min, filter to obtain a lithium carbonate product and lithium precipitation waste liquid, the amount of lithium precipitation waste liquid is 2.307L, the lithium content is 1.6189g / L, pH=11.10, and the carbonate content is 0.2336mol / L.
[0092] Take 2.307L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.856L of monovalent chloride solution and 0.451L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.451L sodium carbonate filtrate is 1.14mol / L, and the sodium carbonate concentration is 10.98%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0093] Example 7
[0094] A method for extracting lithium from lithium mother liquor from salt lakes:
[0095] The only difference between this embodiment and embodiment 1 is that the initial pH of the lithium precipitation mother solution is selected to be 12.0, and the other operating and process conditions remain unchanged.
[0096] Take 3kg of salt lake sodium chloride salt sample and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 48.8ppm, which is reduced to below 0.1ppm after resin ion exchange, that is, the post-ion exchange liquid. The post-ion exchange liquid is added to the bipolar membrane device, and the voltage and current are set to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0097]
[0098] Take 20L of lithium precipitation mother liquor with pH=12, in which the lithium content is 1.351g / L, add 0.307L of 7.41% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.3306g / L.
[0099] As the pH of the lithium precipitation mother liquor increases, the amount of alkali consumed to adjust the alkali to the corresponding extraction pH is reduced (compared to Example 1, 0.315 L decreased to 0.307 L).
[0100] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred and extracted for 3 minutes, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.6L of a 6.51% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 3 minutes, and the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0101] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the raffinate is 0.2647 g / L, and the lithium content in the lithium chloride stripping solution is 11.9903 g / L.
[0102] Use sodium carbonate solid to prepare 870g of 20% sodium carbonate solution, take 1.6L of lithium chloride strip solution with a lithium content of 11.9903g / L, heat it to 80°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 40min, filter to obtain a lithium carbonate product and lithium precipitation waste liquid, the amount of lithium precipitation waste liquid is 2.307L, the lithium content is 1.6235g / L, pH=10.96, and the carbonate content is 0.2320mol / L.
[0103] Take 2.307L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.855L of monovalent chloride solution and 0.452L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.452L sodium carbonate filtrate is 1.13mol / L, and the sodium carbonate concentration is 10.80%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0104] Example 8
[0105] A method for extracting lithium from lithium mother liquor from salt lakes:
[0106] The only difference between this embodiment and embodiment 1 is that 3 kg of salt lake sodium chloride salt sample is prepared into a 9% sodium chloride aqueous solution instead of a 10% sodium chloride aqueous solution, and the other operating and process conditions remain unchanged. The salt concentration becomes lower, the ion concentration decreases, the time required to prepare the acid and alkali of the same concentration is longer, and the energy consumption increases. Specifically:
[0107] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 9% sodium chloride aqueous solution, in which the calcium and magnesium content is 48.8ppm, which is reduced to below 0.1ppm after resin ion exchange, i.e., the post-ion exchange liquid. Add the post-ion exchange liquid into the bipolar membrane device, set the voltage and current to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0108]
[0109] Take 20L of lithium precipitation mother liquor with pH=10, in which the lithium content is 1.35g / L, add 0.335L of 6.98% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.328g / L.
[0110] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred for extraction for 3 minutes, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken and the electrolyte was added thereto. 1.8 L of 5.99% hydrochloric acid solution was obtained (compared with Example 1, the stripping conditions of this embodiment were changed, and the amount of hydrochloric acid was increased, because the acid-base concentration prepared by 9% sodium chloride solution under the same treatment time was lower than that of 10% sodium chloride solution, resulting in the same volume of hydrochloric acid. The hydrogen ion content of 5.99% hydrochloric acid was relatively low, and the lithium in the lithium-containing extract could not be completely stripped, so the amount of hydrochloric acid needed to be increased to ensure that the stripping effect and subsequent lithium precipitation conditions remained unchanged), a two-stage countercurrent stripping operation was adopted, each stage was stirred and mixed for 3 minutes, the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0111] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty extract was 0.2651 g / L, and the lithium content in the lithium chloride stripping solution was 10.6293 g / L.
[0112] Use sodium carbonate solid to prepare 870g of 20% sodium carbonate solution, take 1.8L of lithium chloride strip solution with a lithium content of 10.6293g / L, heat it to 70°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 30min, filter to obtain a lithium carbonate product and lithium precipitation waste liquid, the amount of lithium precipitation waste liquid is 2.507L, the lithium content is 1.4938g / L, pH=10.44, and the carbonate content is 0.2150mol / L.
[0113] Take 2.507L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 2.047L of monovalent chloride solution and 0.460L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.460L sodium carbonate filtrate is 1.118mol / L, and the sodium carbonate concentration is 10.79%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0114] Example 9
[0115] A method for extracting lithium from lithium mother liquor from salt lakes:
[0116] The only difference between this embodiment and embodiment 1 is that 3 kg of salt lake sodium chloride salt sample is taken and prepared into a 13% sodium chloride aqueous solution instead of a 10% sodium chloride aqueous solution, and the other operating and process conditions remain unchanged.
[0117] Compared with the 10% sodium chloride aqueous solution in Example 1, the 13% sodium chloride aqueous solution has a higher ion concentration, and it takes less time to prepare the acid and alkali of the same concentration, but at the same time, the content of impurity ions in the water sample, such as potassium, is relatively higher, resulting in an increase in the content of impurity ions in the prepared acid and alkali, which will affect the purity of the stripping solution and may affect the quality of lithium carbonate produced by lithium precipitation. Specifically:
[0118] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 13% sodium chloride aqueous solution, in which the calcium and magnesium content is 64.9ppm, which is reduced to below 0.1ppm after resin ion exchange, i.e., the post-ion exchange liquid. The post-ion exchange liquid is added to the bipolar membrane device, the voltage and current are set to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0119]
[0120] Take 20L of lithium precipitation mother liquor with pH=10, in which the lithium content is 1.349g / L, add 0.290L of 8.10% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.3297g / L.
[0121] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred and extracted for 3 minutes, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.4L of a 7.39% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 3 minutes, and the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0122] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the raffinate is 0.2638 g / L, and the lithium content in the lithium chloride stripping solution is 13.7042 g / L.
[0123] Use sodium carbonate solid to prepare 870g of 20% sodium carbonate solution, take 1.4L of lithium chloride stripping solution with a lithium content of 11.968g / L, heat it to 70°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 30min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 2.106L, the lithium content is 1.6497g / L, the pH is 11.55, and the carbonate content is 0.2454mol / L.
[0124] Take 2.106L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.664L of monovalent chloride solution and 0.442L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.442L sodium carbonate filtrate is 1.116mol / L, and the sodium carbonate concentration is 10.76%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0125] Example 10
[0126] A method for extracting lithium from lithium mother liquor from salt lakes:
[0127] The difference between this embodiment and embodiment 1 is that the prepared 10% sodium chloride aqueous solution is not subjected to adsorption treatment, that is, its calcium and magnesium content is maintained at 48.8ppm. At this time, magnesium will form corresponding hydroxide or carbonate precipitation when entering the equipment, causing membrane blockage and damage to the equipment. Therefore, before the brine enters the equipment, the divalent and trivalent metal ions must be removed, otherwise it is not allowed to enter the equipment.
[0128] Embodiment 11
[0129] A method for extracting lithium from lithium mother liquor from salt lakes:
[0130] The difference between this embodiment and embodiment 1 is that during the electrolysis of 10% sodium chloride aqueous solution, the parameters are changed, specifically: the voltage and current are set to 50V and 60A respectively, and the power-on time is 60min, and the other operating and process conditions remain unchanged.
[0131] In this embodiment, the voltage and current are reduced, resulting in a decrease in electrolytic separation efficiency. The acid and alkali concentrations prepared in the same time cannot reach the set value. The acid and alkali obtained by bipolar membrane treatment are generally 2 mol / L, and the efficiency is lower. Specifically:
[0132] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 13% sodium chloride aqueous solution, in which the calcium and magnesium content is 64.9ppm, which is reduced to below 0.1ppm after resin ion exchange, i.e., the post-ion exchange liquid. The post-ion exchange liquid is added to the bipolar membrane device, the voltage and current are set to 50V and 60A respectively, and the power-on time is 60min. The treatment results are shown in the table below:
[0133]
[0134] Take 20L of lithium precipitation mother liquor with pH=10, in which the lithium content is 1.349g / L, add 0.300L of 7.75% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.3291g / L.
[0135] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred and extracted for 3 minutes, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.4L of a 7.15% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 3 minutes, and the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0136] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the raffinate is 0.2645 g / L, and the lithium content in the lithium chloride stripping solution is 13.6878 g / L.
[0137] Use sodium carbonate solid to prepare 870g of 20% sodium carbonate solution, take 1.4L of lithium chloride strip solution with a lithium content of 11.968g / L, heat it to 70°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 30min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 2.107L, the lithium content is 1.6497g / L, the pH is 11.55, and the carbonate content is 0.2454mol / L.
[0138] Take 2.107L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.850L of monovalent chloride solution and 0.441L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.441L sodium carbonate filtrate is 1.119mol / L, and the sodium carbonate concentration is 10.79%. Repeat the above operation to prepare the sodium carbonate filtrate of the corresponding concentration, which is reused in the front-end lithium precipitation.
[0139] Example 12
[0140] A method for extracting lithium from lithium mother liquor from salt lakes:
[0141] The difference between this embodiment and embodiment 1 is that during the electrolysis of 10% sodium chloride aqueous solution, the parameters are changed, specifically: the voltage and current are set to 70V and 100A respectively, the power-on time is 20min, and the other operating and process conditions remain unchanged.
[0142] A method for extracting lithium from lithium mother liquor from salt lakes:
[0143] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 64.9ppm, which is reduced to below 0.1ppm after resin ion exchange, i.e., the ion exchange liquid. The ion exchange liquid is added to the bipolar membrane device, and the voltage and current are set to 70V and 100A respectively, and the power-on time is 25min. The treatment results are shown in the table below:
[0144]
[0145] It can be seen from the data in the table that when the current and voltage are increased, the electrolytic separation effect does not change significantly, but the energy consumption increases, which is not conducive to industrial application.
[0146] Take 20L of lithium precipitation mother liquor with pH=10, in which the lithium content is 1.349g / L, add 0.303L of 7.69% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.3289g / L.
[0147] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 10L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a two-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred and extracted for 3 minutes, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.4L of a 7.11% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 3 minutes, and the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0148] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the raffinate is 0.2642 g / L, and the lithium content in the lithium chloride stripping solution is 13.688 g / L.
[0149] Use sodium carbonate solid to prepare 870g of 20% sodium carbonate solution, take 1.4L of lithium chloride strip solution with a lithium content of 13.688g / L, heat it to 70°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 30min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 2.107L, the lithium content is 1.6497g / L, the pH is 11.76, and the carbonate content is 0.2544mol / L.
[0150] Take 2.107L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.649L of monovalent chloride solution and 0.457L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.457L sodium carbonate filtrate is 1.118mol / L, and the sodium carbonate concentration is 10.79%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0151] Example 13
[0152] A method for extracting lithium from lithium mother liquor from salt lakes:
[0153] The only difference between this embodiment and embodiment 1 is that in the process of extracting the lithium precipitate mother liquor after the adjustment pretreatment, the mixture of trioxythiophene oxide, 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and n-hexane is not used, but di-(2-ethylhexyl) phosphoric acid and di(2,4,4-trimethylpentyl hypophosphorous acid) are used as the extractant, and the other operating and process conditions remain unchanged.
[0154] A method for extracting lithium from lithium mother liquor from salt lakes:
[0155] Take 3kg of salt lake sodium chloride salt sample and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 48.8ppm, which is reduced to below 0.1ppm after resin ion exchange, that is, the post-ion exchange liquid. The post-ion exchange liquid is added to the bipolar membrane device, and the voltage and current are set to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0156]
[0157] Take 20L of lithium precipitation mother liquor with pH=10, in which the lithium content is 1.35g / L, add 0.315L of 7.4% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.33g / L.
[0158] First, take 2L of di-(2-ethylhexyl) phosphoric acid, 2L of trioxythiophene oxide, 2L of di(2,4,4-trimethylpentyl hypophosphorous acid) and 6L of cyclohexane, mix them evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of di-(2-ethylhexyl) phosphoric acid and di(2,4,4-trimethylpentyl hypophosphorous acid) accounts for 40%; then take 10L of the extract, mix it with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and use a two-stage countercurrent extraction operation at a temperature of 5°C, stirring and extracting for 3 minutes at each stage, and finally separating the raffinate and the lithium-containing extract; take 10L of the lithium-containing extract, add 1.6L of a 6.5% concentration hydrochloric acid solution obtained by electrolysis, use a two-stage countercurrent stripping operation, stirring and mixing for 3 minutes at each stage, and the temperature is 5°C, and finally separating the empty extract and the lithium chloride stripping solution.
[0159] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty raffinate was 0.9974 g / L, and the lithium content in the lithium chloride stripping solution was 3.742 g / L.
[0160] Use sodium carbonate solid to prepare 272g of 20% sodium carbonate solution, take 1.6L of lithium chloride stripping solution with a lithium content of 3.742g / L, heat it to 70°C, slowly add 272g of 20% sodium carbonate solution thereto, stir the reaction for 30min, filter to obtain a lithium carbonate product and lithium precipitation waste liquid, the amount of lithium precipitation waste liquid is 1.823L, the lithium content is 1.305g / L, pH=9.32, and the carbonate content is 0.1399mol / L.
[0161] Take 1.823L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.656L of monovalent chloride solution and 0.167L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.167L sodium carbonate filtrate is 0.96mol / L, and the sodium carbonate concentration is 9.78%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0162] Embodiment 14
[0163] A method for extracting lithium from lithium mother liquor from salt lakes:
[0164] The only difference between this embodiment and embodiment 1 is that in the process of extracting the lithium precipitate mother liquor after the adjustment pretreatment, the volume of the extracting liquid used is changed from 10L to 3L, and the two-stage countercurrent extraction operation is not adopted, but only a single countercurrent extraction operation is adopted, the stirring extraction time is 15min, and the other operations and process conditions remain unchanged.
[0165] The extraction capacity mainly depends on the performance of the extraction liquid and the amount of extraction liquid. The secondary countercurrent extraction can improve the extraction efficiency. The amount of extraction liquid is reduced, and the primary countercurrent extraction leads to a decrease in the lithium extraction rate.
[0166] A method for extracting lithium from lithium mother liquor from salt lakes:
[0167] Take 3kg of sodium chloride salt sample from salt lake and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 48.9ppm, which is reduced to below 0.1ppm after resin ion exchange, i.e., the post-ion exchange liquid. The post-ion exchange liquid is added to the bipolar membrane device, and the voltage and current are set to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0168]
[0169] Take 20L of lithium precipitation mother liquor with pH=10, in which the lithium content is 1.35g / L, add 0.315L of 7.4% concentration liquid alkali obtained by electrolysis for value adjustment pretreatment, when the pH is increased to 12.5, the lithium content in the solution is 1.33g / L.
[0170] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane were taken and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounted for 40%; then 3L of the extract was taken and mixed with 18L of the lithium precipitation mother liquor after the above-mentioned adjustment pretreatment, and a one-stage countercurrent extraction operation was performed at a temperature of 5°C, with each stage being stirred and extracted for 15min, and finally the raffinate and the lithium-containing extract were separated; 10L of the lithium-containing extract was taken, 1.6L of a 6.5% concentration hydrochloric acid solution obtained by electrolysis was added thereto, and a two-stage countercurrent stripping operation was performed, with each stage being stirred and mixed for 3min, and the temperature was 5°C, and finally the empty extract and the lithium chloride stripping solution were separated.
[0171] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty extract was 0.9987 g / L, and the lithium content in the lithium chloride stripping solution was 3.727 g / L.
[0172] Use sodium carbonate solid to prepare 271g of 20% sodium carbonate solution, take 1.6L of lithium chloride strip solution with a lithium content of 3.727g / L, heat it to 70°C, slowly add 271g of 20% sodium carbonate solution thereto, stir the reaction for 30min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 1.823L, the lithium content is 1.2968g / L, the pH is 9.30, and the carbonate content is 0.1393mol / L.
[0173] Take 1.823L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.656L of monovalent chloride solution and 0.167L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.167L sodium carbonate filtrate is 0.95mol / L, and the sodium carbonate concentration is 9.68%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0174] Embodiment 15
[0175] A method for extracting lithium from lithium mother liquor precipitated in a salt lake: The only difference between this embodiment and embodiment 1 is that during the stripping process, the volume of the hydrochloric acid solution used is changed from 1.6 L to 1.2 L, and the stirring and mixing extraction time for each stage in the two-stage countercurrent stripping is 15 min, and the other operating and process conditions remain unchanged.
[0176] In this embodiment, the volume of hydrochloric acid is reduced, and the hydrogen ion content is reduced, which affects the stripping effect of the lithium-containing extract, resulting in residual lithium in the empty extract and a decrease in the lithium precipitation efficiency.
[0177] Comparative Example 1
[0178] A method for extracting lithium from lithium mother liquor from salt lakes:
[0179] The difference between this comparative example and Example 1 is that: instead of using salt lake sodium chloride electrolysis to provide sodium hydroxide solution and hydrochloric acid solution, sodium hydroxide solid and hydrochloric acid solution are purchased from outside and formulated into: 7.4% concentration liquid caustic soda and 6.5% concentration hydrochloric acid solution.
[0180] Although using purchased products as raw materials does not have much impact on the final extraction effect of lithium, it significantly increases the cost investment required for processing, and it is difficult to achieve the effect of increasing the added value of salt lake products.
[0181] Comparative Example 2
[0182] A method for extracting lithium from lithium mother liquor from salt lakes:
[0183] The only difference between this comparative example and Example 1 is that the lithium precipitation mother liquor is not subjected to value adjustment pretreatment.
[0184] In this comparative example, the mother liquor was not adjusted, the pH was low, the extraction driving force was insufficient, and the extraction effect was poor.
[0185] Take 3kg of salt lake sodium chloride salt sample and prepare it into 10% sodium chloride aqueous solution, in which the calcium and magnesium content is 48.8ppm, which is reduced to below 0.1ppm after resin ion exchange, that is, the post-ion exchange liquid. The post-ion exchange liquid is added to the bipolar membrane device, and the voltage and current are set to 60V and 80A respectively, and the power-on time is 30min. The treatment results are shown in the table below:
[0186]
[0187]
[0188] First, 2L of trioxythiophene oxide, 2L of 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione and 6L of cyclohexane are taken, and mixed evenly in a separatory funnel to obtain an extract, wherein the sum of the volumes of trioxythiophene oxide and 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione accounts for 40%; then 18L of lithium precipitation mother liquor with a pH of 10, in which the lithium content is 1.35g / L, is taken, mixed with the above 10L extract, and a two-stage countercurrent extraction operation is performed at a temperature of 5°C, with each stage being stirred and extracted for 3min, and finally the raffinate and the lithium-containing extract are separated; 10L of the lithium-containing extract is taken, 1.6L of a 6.5% concentration hydrochloric acid solution obtained by electrolysis is added thereto, a two-stage countercurrent stripping operation is performed, with each stage being stirred and mixed for 3min, and the temperature is 5°C, and finally the empty extract and the lithium chloride stripping solution are separated.
[0189] Through ICP (inductively coupled plasma spectrometer) analysis, the lithium content in the empty extract was 0.6283 g / L, and the lithium content in the lithium chloride stripping solution was 8.1192 g / L.
[0190] Use sodium carbonate solid to prepare 590g of 20% sodium carbonate solution, take 1.6L of lithium chloride stripping solution with a lithium content of 8.1192g / L, heat it to 70°C, slowly add 870g of 20% sodium carbonate solution thereto, stir the reaction for 30min, and filter to obtain a lithium carbonate product and lithium precipitation waste liquid. The amount of lithium precipitation waste liquid is 2.081L, the lithium content is 1.6393g / L, the pH is 10.26, and the carbonate content is 0.2053mol / L.
[0191] Take 2.081L of the above lithium precipitation waste liquid, treat it with a nanofiltration membrane, run it for 50 minutes under the conditions of pressure 1.5Mpa and temperature 10°C, and obtain 1.76L of monovalent chloride solution and 0321L of sodium carbonate filtrate. The chloride solution is reused in the adjustment section and re-enters the extraction system after liquid alkali pretreatment. The carbonate content in 0.321L of sodium carbonate filtrate is 0.99mol / L, and the sodium carbonate concentration is 10.79%. Repeat the above operation to prepare sodium carbonate filtrate of corresponding concentration, which is reused in the front-end lithium precipitation.
[0192] In the methods provided in the above embodiments and comparative examples, the extraction rate of lithium after extraction and stripping, the yield of lithium carbonate product after lithium precipitation treatment, and the carbonate separation recovery rate after nanofiltration treatment are shown in Table 1.
[0193] Table 1
[0194]
[0195]
[0196] From the above description, it can be seen that the above-mentioned embodiments of the present invention realize the efficient development, recovery and utilization of salt lake resources. First, the sodium chloride produced in the potash fertilizer production process is selected to configure the corresponding salt solution, and then the divalent magnesium ions in the water sample are treated by resin adsorption exchange, and then the water sample after adsorption is treated by membrane equipment to obtain sodium hydroxide and hydrochloric acid solution, with a concentration of about 2 mol / L. Low-value sodium chloride raw materials are consumed in this section, and the acid and alkali required for the extraction section are obtained, which saves the acid and alkali transportation costs and avoids transportation risks; the prepared alkali solution is used to adjust the value of the lithium precipitation mother liquor, and hydrochloric acid is used as the stripping acid. The lithium precipitation mother liquor is extracted and concentrated by extraction and stripping. The lithium content of the obtained lithium chloride stripping solution is as high as about 14g / L, which can be directly precipitated to prepare lithium carbonate products. The use of MVR equipment is avoided, and the production energy consumption is reduced. Finally, the water sample after lithium precipitation is treated with a membrane to separate the monovalent salt solution and the sodium carbonate solution. The monovalent salt water sample is mainly sodium chloride and lithium chloride, which are reused to the extraction end for adjustment and lithium extraction. The sodium carbonate solution is returned to the lithium precipitation section for continued use. The above process not only efficiently recovers lithium resources, but also extracts and reuses carbonate ions in the mother liquor, completing a closed loop of resource extraction, recovery, and reuse.
[0197] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0198] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for extracting lithium from lithium mother liquor from salt lakes, characterized in that: The method comprises: Step S1, providing a lithium-containing solution and sodium chloride salt, wherein the lithium-containing solution is a lithium precipitation mother liquor produced after lithium is extracted from salt lake brine, and the sodium chloride salt is a by-product in the process of preparing potash fertilizer in salt lake; Step S2, preparing the sodium chloride salt into a sodium chloride salt solution, and electrolyzing the sodium chloride salt solution to obtain a hydrochloric acid solution and a sodium hydroxide solution; Step S3, using the sodium hydroxide solution to perform pH adjustment pretreatment on the lithium-containing solution to obtain a pretreated lithium-containing solution with a pH of 12 to 14; Step S4, extracting lithium ions from the pretreated lithium-containing solution to obtain a loaded extract and a raffinate; Step S5, mixing the loaded extract with the hydrochloric acid solution, and performing stripping to obtain a lithium chloride stripping solution and an unloaded stripping solution; Step S6, performing lithium precipitation treatment on the lithium chloride stripping solution to obtain a lithium carbonate product and a lithium precipitation waste liquid; Step S7, performing nanofiltration treatment on the lithium precipitation waste liquid to obtain sodium carbonate filtrate and chloride filtrate.
2. The method according to claim 1, characterized in that In step S1, the pH of the lithium-containing solution is 9 to 12.
5.
3. The method according to claim 1 or 2, characterized in that: In step S2, the mass concentration of the sodium chloride salt solution is 10-12%; Preferably, before the electrolysis, step S2 further comprises performing an adsorption treatment on the sodium chloride salt solution to remove calcium ions and / or magnesium ions in the sodium chloride salt solution.
4. The method according to any one of claims 1 to 3, characterized in that The electrolysis voltage in step S2 is 55-65V, the current is 70-90A, and the electrolysis treatment time is 30-50min.
5. The method according to any one of claims 1 to 4, characterized in that The extraction in step S4 includes: mixing the pretreated lithium-containing solution with an extract to obtain a mixed solution, and performing the extraction on the mixed solution to obtain the loaded extract and the raffinate; Preferably, the volume ratio of the pretreated lithium-containing solution to the extract is (1-4):1; Preferably, the number of extractions is 1 to 3, and the duration of each extraction is 1 to 10 minutes.
6. The method according to claim 5, characterized in that The extract comprises an extractant and a diluent; Preferably, the extractant is selected from trioxythiophene oxide, 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione, 1,1,1,2,2-pentafluoro-6,6-dimethyl-3,5-heptanedione, 1,1,1,2,2,3,3-heptafluoro-7,7-dimethyl-4,6-octanedione, benzoyltrifluoroacetone, trialkyl phosphate, dialkyl phosphate, methyl isobutyl ketone, diketone, 1-phenylene glycol, 1-hydroxy-1-nitroprop ... One or more of azo-2-naphthol, n-octanol, isooctyl alcohol, 2-ethylhexanol, 14-crown-4 ether dibutyl phosphonate, dibutyl butyl phosphate, methylene tetrabutyl bisphosphate, trioctylamine oxide, 1,10-phenanthroline, quaternary ammonium salt N263, dimethyl di(N-octadecyl)ammonium chloride, methyl dioctyl sulfonium chloride, 1-hydroxyethyl-3-methylimidazole bis(trifluoromethylsulfonyl)imide; Preferably, the diluent is selected from one or more of n-hexane, n-dodecane, cyclohexane, D70 special solvent oil, D80 special solvent oil, No. 120 solvent oil, No. 160 solvent oil, No. 200 solvent oil, No. 90 kerosene, aviation kerosene and sulfonated kerosene.
7. The method according to claim 6, characterized in that In step S5, the volume ratio of the loaded extract to the hydrochloric acid solution is (4-8):1; Preferably, the stripping is carried out at 0 to 40°C; Preferably, the number of back extractions is 1 to 3, and the time for each back extraction is 1 to 10 minutes; More preferably, step S5 further comprises returning the unloaded stripping solution to step S4 to mix with the extract.
8. The method according to any one of claims 1 to 7, characterized in that The lithium precipitation treatment in step S6 further includes: heating the lithium chloride stripping solution, adding sodium carbonate solution to the lithium chloride stripping solution, stirring the solution for reaction, and filtering the solution to obtain the lithium carbonate product and the lithium precipitation waste solution; Preferably, the heating temperature is 70-90° C.; and the stirring reaction time is 30-60 min.
9. The method according to any one of claims 1 to 8, characterized in that In step S7, the nanofiltration treatment is performed at a pH of 8 to 12; Preferably, the operating pressure of the nanofiltration treatment is 1.5 to 2.5 MPa; and / or, the operating temperature of the nanofiltration treatment is 5 to 45° C.; and / or, the operating time of the nanofiltration treatment is 40 to 100 min.
10. The method according to any one of claims 1 to 9, characterized in that Step S7 also includes returning the sodium carbonate filtrate to step S6 for lithium precipitation treatment; Preferably, step S7 further comprises returning the chloride salt filtrate to step S3, mixing it with the lithium-containing solution and then performing the pH adjustment pretreatment; Preferably, the chloride salt is sodium chloride and / or lithium chloride.
Citation Information
Cited By
Method for recovering lithium in lithium precipitation mother liquor
CN119913368A
Extraction and recovery process for lithium precipitation mother liquor through multi-stage hardening and tempering