Method for removing flotation reagent in ammonium tungstate solution
Through activated carbon mixture and chemical treatment, the problem of foam and Ti exceeding the standard caused by flotation reagents in the tungsten metallurgical process is solved, the TOC is effectively removed and the sedimentation efficiency is improved, and the production efficiency and product quality of the tungsten metallurgical process are improved.
Patent Information
- Application Number
- CN202410889297.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-08
AI Technical Summary
In the traditional tungsten metallurgical process, the flotation reagents used in the scheelite beneficiation process cause problems such as foam formation, adsorption of fine particles, reduced production efficiency, and excessive Ti elements in the subsequent process.
Activated carbon mixture is used to filter the ammonium tungstate solution, combined with ammonia dissolution, hydrochloric acid reaction and impurity removal and aging process. By adding magnesium sulfate and copper sulfate solution, the temperature and pH value are controlled, the flotation agent is removed, and the TOC removal rate and sedimentation rate are improved. chemical efficiency.
Effectively remove TOC in ammonium tungstate solution, with a removal rate of ≥98%, eliminate foam, shorten the aging time, reduce the Ti element content in ammonium paratungstate to <4ppm, and improve production efficiency and product quality.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tungsten metallurgy, and in particular relates to a method for removing a flotation agent in an ammonium tungstate solution. Background Art
[0002] The traditional "alkali decomposition + ion exchange" process for treating scheelite has problems such as tungsten slag being hazardous waste, high production cost and large amount of wastewater, which makes it increasingly difficult to meet the requirements of national environmental protection policies; while the new classic process "hydrochloric acid leaching + ammonia dissolution and impurity removal" for treating scheelite has gradually become a development trend due to its high tungsten recovery rate, low production cost and tungsten slag being a byproduct of calcium sulfate. However, a large amount of flotation reagents are used in the scheelite beneficiation process. These flotation reagents will be adsorbed on the surface of the mineral and enter the concentrate during the flotation process, and enter the ammonium tungstate solution in the subsequent hydrochloric acid leaching, tungsten acid ammonia dissolution and other processes, and bring the following adverse effects: First, it causes thick foam to form on the surface of the ammonium tungstate solution, and the "bridging" of the foam makes the liquid level detection of the tank inaccurate, and even causes the tank liquid to "bubble" accident; second, the foam will absorb fine particles and float in the solution for a long time, making it difficult to precipitate the subsequent impurity removal slag phase, greatly reducing production efficiency; third, the residual flotation reagents will adsorb the Ti element, causing the final product Ti to exceed the standard. Summary of the invention
[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for removing flotation reagents in ammonium tungstate solution.
[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0005] A method for removing flotation reagents from ammonium tungstate solution comprises the following steps:
[0006] S1, filtering the tungstate ammonia solution to obtain ammonia slag and ammonium tungstate solution;
[0007] S2, the ammonium tungstate solution passes through an activated carbon mixture, the activated carbon mixture is composed of 10wt% of 40-60 mesh activated carbon, 30-40wt% of 90-110 mesh activated carbon, and 50-60wt% of 140-160 mesh activated carbon. The flow rate of the ammonium tungstate solution is controlled to be 1-1.5 times the volume of the activated carbon mixture per hour to obtain the ammonium tungstate solution with the flotation agent removed.
[0008] As a preferred embodiment of the method for removing flotation reagents from an ammonium tungstate solution described in the present invention, in the step S1, tungstic acid is dissolved in ammonia water, wherein the concentration of ammonia water is 9-10wt%, the liquid-solid ratio of ammonia water to tungstic acid is (2-3) mL:1g, the reaction temperature is room temperature, the reaction time is 1-2h, and the ammonia slag and the ammonium tungstate solution are obtained by filtration.
[0009] As a preferred embodiment of the method for removing flotation reagents from ammonium tungstate solution described in the present invention, wherein: in the step S1, a scheelite flotation concentrate with a WO3 content of 48-50wt% is taken, and hydrochloric acid with a concentration of 24-25wt% is added according to a liquid-solid ratio of hydrochloric acid to the scheelite flotation concentrate of (2-4)mL:1g, the reaction temperature is 80-90°C, the reaction time is 4-6h, and tungstic acid is obtained by cooling and filtering.
[0010] As a preferred embodiment of the method for removing flotation reagents from ammonium tungstate solution of the present invention, in step S2, the TOC content in the ammonium tungstate solution from which the flotation reagents are removed is ≤7.5 mg / L, and the TOC removal rate is ≥98%.
[0011] As a preferred embodiment of the method for removing flotation reagents from ammonium tungstate solution described in the present invention, the ammonium tungstate solution from which the flotation reagents are removed is subjected to decontamination and aging, wherein magnesium sulfate is added in an amount of 1.5 to 2.0 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, stirred for reaction for 1 to 1.5 hours, and then added to a container to observe the aging time; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95 to 100° C., and the pH value of the crystallization endpoint is 6.4 to 6.9, and then filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy.
[0012] As a preferred embodiment of the method for removing flotation reagents from ammonium tungstate solution of the present invention, the concentration of copper sulfate solution is 20-25wt%, and the amount thereof added is 1.5-1.8vol% of the volume of the ammonium tungstate solution; the concentration of ammonium sulfate solution is 75-80wt%, and the amount thereof added is 1.6-1.8vol% of the volume of the ammonium tungstate solution.
[0013] As a preferred embodiment of the method for removing flotation reagents from ammonium tungstate solution described in the present invention, the aging time is ≤40min, and the Ti content in the ammonium paratungstate is <4ppm.
[0014] As a preferred embodiment of the method for removing flotation reagents from ammonium tungstate solution described in the present invention, the flotation reagents are xanthate and pine oil.
[0015] The beneficial effects of the present invention are as follows:
[0016] The invention provides a method for removing flotation reagents in ammonium tungstate solution. The ammonium tungstate solution is passed through an activated carbon mixture, which can not only effectively remove TOC in the ammonium tungstate solution, with a TOC removal rate of ≥98%, eliminate foam in the solution, but also greatly improve the sedimentation efficiency of fine particle slag after impurity removal, with an aging time of ≤40min, and solve the problem of excessive Ti element in ammonium paratungstate (Ti element content in ammonium paratungstate <4ppm). DETAILED DESCRIPTION
[0017] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] According to one aspect of the present invention, the present invention provides the following technical solution:
[0019] A method for removing flotation reagents from ammonium tungstate solution comprises the following steps:
[0020] S1, filtering the tungstate ammonia solution to obtain ammonia slag and ammonium tungstate solution;
[0021] S2, the ammonium tungstate solution passes through an activated carbon mixture, the activated carbon mixture is composed of 10wt% of 40-60 mesh activated carbon, 30-40wt% of 90-110 mesh activated carbon, and 50-60wt% of 140-160 mesh activated carbon. The flow rate of the ammonium tungstate solution is controlled to be 1-1.5 times the volume of the activated carbon mixture per hour to obtain the ammonium tungstate solution with the flotation agent removed.
[0022] Preferably, in step S1, tungstic acid is dissolved in ammonia water, wherein the concentration of ammonia water is 9-10wt%, the liquid-solid ratio of ammonia water to tungstic acid is (2-3)mL:1g, the reaction temperature is room temperature, the reaction time is 1-2h, and the ammonia slag and ammonium tungstate solution are obtained by filtration.
[0023] Preferably, in step S1, a scheelite flotation concentrate having a WO3 content of 48 to 50 wt% is taken, and hydrochloric acid having a concentration of 24 to 25 wt% is added according to a liquid-solid ratio of hydrochloric acid to the scheelite flotation concentrate of (2 to 4) mL:1 g, the reaction temperature is 80 to 90° C., the reaction time is 4 to 6 h, and tungstic acid is obtained by cooling and filtering.
[0024] Preferably, in step S2, the TOC content in the ammonium tungstate solution from which the flotation agent is removed is ≤7.5 mg / L, and the TOC removal rate is ≥98%.
[0025] Preferably, the ammonium tungstate solution from which the flotation agent has been removed is subjected to decontamination and aging, wherein the amount of magnesium sulfate added is 1.5 to 2.0 times the molar amount of the P element, and then the ammonium sulfide solution and the copper sulfate solution are added, and the mixture is stirred for reaction for 1 to 1.5 hours and then added to a container to observe the aging time; after aging, the mixture is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95 to 100° C., and the pH value of the crystallization endpoint is 6.4 to 6.9, and then filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy.
[0026] Preferably, the concentration of the copper sulfate solution is 20-25wt%, and the amount thereof added is 1.5-1.8vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 75-80wt%, and the amount thereof added is 1.6-1.8vol% of the volume of the ammonium tungstate solution.
[0027] Preferably, the aging time is ≤40 min, and the Ti content in the ammonium paratungstate is <4 ppm.
[0028] Preferably, the flotation reagents are xanthate and pine oil, and the mass ratio of xanthate to pine oil is (1-2):(4-20).
[0029] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0030] The preparation method of the ammonium tungstate solution of each embodiment and comparative example is as follows: taking a scheelite flotation concentrate with a WO3 content of 50wt% (the flotation reagent is xanthate and pine oil with a mass ratio of 2:5), adding hydrochloric acid with a concentration of 24wt% according to the liquid-solid ratio of hydrochloric acid to the scheelite flotation concentrate of 3mL:1g, the reaction temperature is 85°C, the reaction time is 5h, and cooling and filtering to obtain tungstic acid; tungstic acid is dissolved in ammonia water, wherein the ammonia concentration is 9wt%, the liquid-solid ratio of ammonia water to tungstic acid is 2.5mL:1g, the reaction temperature is room temperature, the reaction time is 1.5h, and filtering to obtain ammonia slag and ammonium tungstate solution.
[0031] Example 1
[0032] A method for removing flotation reagents from ammonium tungstate solution comprises the following steps:
[0033] S1, tungstate ammonia solution is filtered to obtain ammonia slag and ammonium tungstate solution; the TOC content of the flotation reagent in the ammonium tungstate solution is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 384.6 mg / L and the thickness of the foam layer is 2 cm;
[0034] S2, the ammonium tungstate solution passes through an activated carbon mixture, which is composed of 10wt% of 40-60 mesh activated carbon, 30wt% of 90-110 mesh activated carbon, and 60wt% of 140-160 mesh activated carbon. The flow rate of the ammonium tungstate solution is controlled to be 1 times the volume of the activated carbon mixture per hour to obtain the ammonium tungstate solution with the flotation agent removed.
[0035] In this embodiment, the ammonium tungstate solution from which the flotation agent is removed is used to determine the TOC content by using a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 6.2 mg / L, the flotation agent removal rate is 98.4%, and the foam layer thickness is 0 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 35min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.7; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is less than 4ppm.
[0036] Example 2
[0037] A method for removing flotation reagents from ammonium tungstate solution comprises the following steps:
[0038] S1, tungstate ammonia solution is filtered to obtain ammonia slag and ammonium tungstate solution; the TOC content of the flotation reagent in the ammonium tungstate solution is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 384.6 mg / L and the thickness of the foam layer is 2 cm;
[0039] S2, the ammonium tungstate solution passes through an activated carbon mixture, the activated carbon mixture is composed of 10wt% of 40-60 mesh activated carbon, 40wt% of 90-110 mesh activated carbon, and 50wt% of 140-160 mesh activated carbon. The flow rate of the ammonium tungstate solution is controlled to be 1.5 times the volume of the activated carbon mixture per hour to obtain the ammonium tungstate solution with the flotation agent removed.
[0040] In this embodiment, the flotation reagent in the ammonium tungstate solution from which the flotation reagent is removed is measured by a TOC instrument to determine the TOC content, and the thickness of the foam layer is measured, wherein the TOC content is 7.3 mg / L, the flotation reagent removal rate is 98.1%, and the foam layer thickness is 0 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 20wt%, and its addition amount is 1.8vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 75wt%, and its addition amount is 1.8vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 40min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.6; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is less than 4ppm.
[0041] Comparative Example 1
[0042] The difference from Example 1 is that the activated carbon mixture in step S2 is formed by mixing 30wt% of 40-60 mesh activated carbon, 30wt% of 90-110 mesh activated carbon, and 40wt% of 140-160 mesh activated carbon.
[0043] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 82.7 mg / L, the flotation agent removal rate is 78.5%, and the foam layer thickness is 0 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 1h40min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.8; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 12ppm.
[0044] Comparative Example 2
[0045] The difference from Example 1 is that the activated carbon mixture in step S2 is replaced by activated carbon of 90-110 meshes of the same mass.
[0046] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 171.9 mg / L, the flotation agent removal rate is 55.3%, and the foam layer thickness is 0 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 3h10min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.5; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 18ppm.
[0047] Comparative Example 3
[0048] The difference from Example 1 is that the activated carbon mixture in step S2 is replaced by activated carbon of 40-60 mesh of the same mass.
[0049] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 274.2 mg / L, the flotation agent removal rate is 28.7%, and the foam layer thickness is 0 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 4h30min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.6; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 26ppm.
[0050] Comparative Example 4
[0051] The difference from Example 1 is that the activated carbon mixture in step S2 is replaced by D851 resin of the same mass.
[0052] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 39.6 mg / L, the flotation agent removal rate is 89.7%, and the foam layer thickness is 0 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 1h10min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.5; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 7ppm.
[0053] Comparative Example 5
[0054] The difference from Example 1 is that the activated carbon mixture in step S2 is replaced by 1 / 10 of the mass of polysilicate flocculant (PSAA), the adsorption reaction is carried out at room temperature for 1 hour, and the ammonium tungstate solution with the flotation agent removed is obtained by filtration and separation.
[0055] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 341.1 mg / L, the flotation agent removal rate is 11.3%, and the foam layer thickness is 2 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 5h40min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.6; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 31ppm.
[0056] Comparative Example 6
[0057] The difference from Example 1 is that the activated carbon mixture in step S2 is replaced by 1 / 5 of the mass of polysilicate flocculant (PSAA), the adsorption reaction is carried out at room temperature for 1 hour, and the ammonium tungstate solution with the flotation agent removed is obtained by filtration and separation.
[0058] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 338.1 mg / L, the flotation agent removal rate is 12.1%, and the foam layer thickness is 2 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 5h40min; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.6; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 30ppm.
[0059] Comparative Example 7
[0060] The difference from Example 1 is that the activated carbon mixture in step S2 is replaced by 1 / 10 of the mass of activated alumina, the adsorption reaction is carried out at room temperature for 1 hour, and the ammonium tungstate solution with the flotation agent removed is obtained by filtration and separation.
[0061] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 304.6 mg / L, the flotation agent removal rate is 20.8%, and the foam layer thickness is 2 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 5h; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.7; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 28ppm.
[0062] Comparative Example 8
[0063] The difference from Example 1 is that the activated carbon mixture in step S2 is replaced by 1 / 5 of the mass of activated alumina, the adsorption reaction is carried out at room temperature for 1 hour, and the ammonium tungstate solution with the flotation agent removed is obtained by filtration and separation.
[0064] In this comparative example, the TOC content of the ammonium tungstate solution from which the flotation agent is removed is determined by a TOC instrument, and the thickness of the foam layer is measured, wherein the TOC content is 298.8 mg / L, the flotation agent removal rate is 22.3%, and the foam layer thickness is 2 cm. The ammonium tungstate solution from which the flotation agent has been removed is subjected to impurity removal and aging, wherein the amount of magnesium sulfate added is 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, wherein the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, the solution is added to a container and the aging time is observed, and the aging time is 5h; after aging, the solution is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization end point is 6.7; then, the solution is filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 27ppm.
[0065] Comparative Example 9
[0066] The difference from Example 1 is that no activated carbon mixture is used in step S2.
[0067] The ammonium tungstate solution of this comparative example is subjected to impurity removal and aging, wherein magnesium sulfate is added in an amount of 1.5 times the molar amount of the P element, and then ammonium sulfide solution and copper sulfate solution are added, the concentration of the copper sulfate solution is 25wt%, and its addition amount is 1.5vol% of the volume of the ammonium tungstate solution; the concentration of the ammonium sulfate solution is 80wt%, and its addition amount is 1.6vol% of the volume of the ammonium tungstate solution; after stirring for 1h, it is added to a container and the aging time is observed, and the aging time is 6h; after aging, it is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95°C, and the pH value of the crystallization endpoint is 6.7, and then filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy, and the Ti element content in the ammonium paratungstate is 36ppm.
[0068] It can be seen from the above embodiments and comparative examples that the present invention passes the ammonium tungstate solution through the activated carbon mixture, which can not only effectively remove TOC in the ammonium tungstate solution, the TOC removal rate is ≥98%, and the foam in the solution is eliminated, but also the precipitation efficiency of the fine particle slag after impurity removal is greatly improved, the aging time is ≤40min, and the problem of excessive Ti element in ammonium paratungstate is solved (the Ti element content in ammonium paratungstate is <4ppm).
[0069] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for removing flotation reagents from ammonium tungstate solution, characterized in that: The steps include: S1, filtering the tungstate ammonia solution to obtain ammonia slag and ammonium tungstate solution; S2, the ammonium tungstate solution passes through an activated carbon mixture, the activated carbon mixture is composed of 10wt% of 40-60 mesh activated carbon, 30-40wt% of 90-110 mesh activated carbon, and 50-60wt% of 140-160 mesh activated carbon. The flow rate of the ammonium tungstate solution is controlled to be 1-1.5 times the volume of the activated carbon mixture per hour to obtain the ammonium tungstate solution with the flotation agent removed.
2. The method for removing flotation reagents from ammonium tungstate solution according to claim 1, characterized in that: In the step S1, tungstic acid is dissolved in ammonia water, wherein the concentration of ammonia water is 9-10wt%, the liquid-solid ratio of ammonia water to tungstic acid is (2-3)mL:1g, the reaction temperature is room temperature, the reaction time is 1-2h, and the ammonia slag and ammonium tungstate solution are obtained by filtration.
3. The method for removing flotation reagents from ammonium tungstate solution according to claim 2, characterized in that: In the step S1, a scheelite flotation concentrate having a WO3 content of 48 to 50 wt% is taken, and hydrochloric acid having a concentration of 24 to 25 wt% is added according to a liquid-solid ratio of hydrochloric acid to the scheelite flotation concentrate of (2 to 4) mL:1 g. The reaction temperature is 80 to 90° C., the reaction time is 4 to 6 hours, and tungstic acid is obtained by cooling and filtering.
4. The method for removing flotation reagents from ammonium tungstate solution according to claim 1, characterized in that: In the step S2, the TOC content in the ammonium tungstate solution from which the flotation agent is removed is ≤7.5 mg / L, and the TOC removal rate is ≥98%.
5. The method for removing flotation reagents from ammonium tungstate solution according to claim 1, characterized in that: The ammonium tungstate solution from which the flotation agent has been removed is subjected to decontamination and aging, wherein the amount of magnesium sulfate added is 1.5 to 2.0 times the molar amount of the P element, and then the ammonium sulfide solution and the copper sulfate solution are added, and the mixture is stirred for reaction for 1 to 1.5 hours and then added to a container to observe the aging time; after aging, the mixture is filtered, and then placed in a water bath for crystallization, the crystallization temperature is controlled to be 95 to 100°C, and the pH value of the crystallization endpoint is 6.4 to 6.9, and then filtered, washed, and dried to obtain ammonium paratungstate, and the Ti element content in the ammonium paratungstate is determined by spectroscopy.
6. The method for removing flotation reagents from ammonium tungstate solution according to claim 5, characterized in that: The concentration of the copper sulfate solution is 20-25wt%, and the amount thereof added is 1.5-1.8vol% of the volume of the ammonium tungstate solution. The concentration of the ammonium sulfate solution is 75-80wt%, and the amount thereof added is 1.6-1.8vol% of the volume of the ammonium tungstate solution.
7. The method for removing flotation reagents from ammonium tungstate solution according to claim 5, characterized in that: The aging time is ≤40min, and the Ti content in ammonium paratungstate is <4ppm.
8. The method for removing flotation reagents from ammonium tungstate solution according to claim 1, characterized in that: The flotation reagents are xanthate and pine oil.