High-plasticity low-content rare earth magnesium alloy material and preparation method

By adding low contents of gadolinium, zinc and calcium elements to magnesium alloys, the mechanical properties and plasticity of magnesium alloys are improved, the problem of insufficient room temperature deformation ability of magnesium alloy materials is solved, and the preparation of high plasticity and low content rare earth magnesium alloy materials is achieved. Improved its application potential in the engineering field.

CN118745543APending Publication Date: 2024-10-08HUNAN CITY UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411074070.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The room temperature deformation ability of magnesium alloy materials is weak, which limits its application in the engineering field, especially in the preparation process of thin-walled and complex structural material parts.

Method used

By adding low contents of rare earth elements gadolinium (Gd), zinc (Zn) and calcium (Ca) to the magnesium alloy, controlling the sum of their mass percentages to be less than 2%, the mechanical properties and plasticity of the alloy are improved, and a simple preparation method is used Perform casting and extrusion processing with conventional equipment to prepare high plasticity and low content rare earth magnesium alloy materials.

Benefits of technology

It significantly increases the room temperature elongation of magnesium alloy materials to more than 40%, improves its plasticity and mechanical properties, reduces production costs, and expands its application scope in the engineering field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745543A_ABST
    Figure CN118745543A_ABST
Patent Text Reader

Abstract

The invention discloses a high-plasticity low-content rare earth magnesium alloy material and a preparation method, the high-plasticity low-content rare earth magnesium alloy material comprises the following components in percentage by mass: 0-1% of Gd, 0-1.5% of Zn, 0-0.8% of Ca and the balance of Mg and inevitable impurities, the content of Gd is not 0, and the sum of the mass percentages of Gd, Zn and Ca is less than or equal to 2%. The preparation method comprises the following steps: 1) selecting raw materials; 2) burdening; 3) smelting: after completely melting the pure magnesium ingot, adding the pure zinc ingot, the Mg-30Gd intermediate alloy and the Mg-20Ca intermediate alloy; after the raw materials are completely melted, stirring the melt for 3-5 minutes, and standing for 30-50 minutes; then cooling and pouring; (4) extruding: firstly performing homogenization treatment, and then performing water cooling; and extruding to obtain the magnesium alloy. The preparation method of the magnesium alloy material is simple and low in cost, the ductility of the prepared magnesium alloy material reaches 40% or above, and the plasticity of the magnesium alloy material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, and in particular to a high-plasticity and low-rare-earth-content magnesium alloy material and a preparation method thereof. Background Art

[0002] As the lightest metal structural material, magnesium alloy has the advantages of low density, high strength, high rigidity, good shock resistance, and good machining performance. Magnesium-aluminum alloy is the most widely used, followed by magnesium-manganese alloy and magnesium-zinc-zirconium alloy. It is mainly used in many fields such as aviation, aerospace, weapons and equipment, 3C, rail transportation, etc.

[0003] As magnesium alloys are increasingly used in the engineering field, the requirements for the deformation capacity and performance of magnesium alloy materials are becoming higher and higher, especially in the preparation process of thin-walled and complex structural parts. However, due to its close-packed hexagonal lattice structure, few room temperature slip systems, and generally low plasticity, its room temperature deformation capacity is relatively weak, which limits its further promotion and application in the engineering field.

[0004] In order to solve the problem of poor plasticity of magnesium alloy, patent application number CN201710021425.4 discloses a deformed magnesium alloy sheet with good room temperature formability and its preparation method, the chemical composition mass percentage is: 3-5% Al or 1-2% Zn, 0.2-2% Ca, 0-0.8% Gd, the balance is Mg, and does not contain Al and Zn elements at the same time. The preparation method is: the magnesium alloy is cast (semi-continuous water cooling or solid mold casting) and solution treated at 300-450℃ for 12-20 hours, and air-cooled to room temperature to form a slab. The slab is hot rolled at 400-450℃, and the total reduction rate is 90%. Among them, the reduction rate of the first two passes is within 10%, the reduction rate of the middle pass is 10-30%, and the last two passes are heated and rolled at 450-500℃, and the reduction rate is 10-15%. The rolled sheet is annealed at 350°C for 30-60 minutes.

[0005] The maximum elongation of the magnesium alloy sheet in the above patent at room temperature is only 24%, which is low in elongation and poor in plastic deformation ability. Therefore, providing a magnesium alloy with high plasticity has become an urgent problem to be solved. Summary of the invention

[0006] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide a high-plasticity, low-rare earth content magnesium alloy material and a preparation method thereof. The preparation method of the magnesium alloy material is simple and low-cost. The elongation of the prepared magnesium alloy material reaches more than 40%, which greatly improves the plasticity of the magnesium alloy material and has excellent comprehensive performance.

[0007] The technical solution adopted by the present invention to solve its technical problem is: a high-plasticity and low-rare-earth magnesium alloy material, the magnesium alloy material includes the following components and their mass percentages: Gd 0-1%, Zn 0-1.5%, Ca 0-0.8%, and the rest are Mg and inevitable impurities, wherein the present invention is to produce a high-plasticity and low-rare-earth magnesium alloy material, the content of the rare earth element Gd is not 0, and the sum of the mass percentages of the Gd, Zn and Ca elements is controlled to be ≤2%.

[0008] The addition of gadolinium can reduce the axial ratio of magnesium and promote the generation of non-basal slip during the extrusion process, thereby improving the mechanical properties of the alloy; zinc can effectively improve the mechanical properties of the alloy, increase the ignition point, and better ensure the safety of the alloy during the casting process; calcium can provide a strengthening effect and flame retardant effect similar to rare earth elements, and each element can also improve the overall performance of the material through the synergistic effect of grain boundary segregation. At the same time, the content of alloy elements added to metallic magnesium is low, which ensures the low production cost and high plasticity of the alloy; the inventor found that when the alloy elements are added too much, more coarse particle phases will be generated, which will deteriorate the plasticity of the alloy, so the sum of the mass percentages of Gd, Zn, and Ca elements is controlled below 2%.

[0009] Preferably, the magnesium alloy material includes the following components and their mass percentages: Gd 0.1-1%, Zn 0-1.5%, Ca 0-0.8%, the remainder being Mg and unavoidable impurities, and the sum of the mass percentages of Gd, Zn and Ca elements is 42%.

[0010] More preferably, the magnesium alloy material includes the following components and their mass percentages: Gd 0.3%, Zn 0.5%, Ca 0.25%, and the remainder being Mg and inevitable impurities.

[0011] More preferably, the magnesium alloy material includes the following components and their mass percentages: Gd 0.5%, Zn 1.0%, Ca 0.5%, and the rest being Mg and inevitable impurities.

[0012] Furthermore, the mass percentage of the unavoidable impurities is ≤0.2%.

[0013] The present invention also provides a method for preparing the high-plasticity and low-rare earth content magnesium alloy material as described above, comprising the following steps:

[0014] 1) Raw material selection: pure zinc ingot, pure magnesium ingot, Mg-30Gd master alloy and Mg-20Ca master alloy are selected as raw materials for preparing magnesium alloy materials;

[0015] 2) Ingredients: weigh pure zinc ingots, pure magnesium ingots, Mg-30Gd master alloy, and Mg-20Ca master alloy according to the mass percentage of each component in the magnesium alloy material;

[0016] 3) Melting: After heating the melting crucible to 400°C, add pure magnesium ingots. When the pure magnesium ingots are completely melted and heated to 730-750°C, add pure zinc ingots, Mg-30Gd master alloys, and Mg-20Ca master alloys in sequence. When the raw materials are completely melted, stir the melt for 3-5 minutes, salvage the scum on the surface of the melt, and let it stand for 30-50 minutes. Then cool it to 720-730°C and pour it into a metal mold to prepare an alloy ingot. The melting process is carried out under a protective atmosphere of CO2+SF6.

[0017] 4) Extrusion: firstly homogenize the alloy ingot obtained in step 3), and then water-cool it; and then extrude it to obtain the high-plasticity and low-rare-earth-content magnesium alloy material.

[0018] In the above step 3), after the pure magnesium ingot is completely melted, the Mg-30Gd master alloy, the pure zinc ingot, and the Mg-20Ca master alloy are added together for melting instead of being added in batches. This can not only greatly reduce the burn-out rate due to the addition of multiple batches of alloys, but also effectively reduce the mixing of impurities and improve the mechanical properties of the alloy.

[0019] Furthermore, the purity of the pure magnesium ingot is 99.99%, and the purity of the pure zinc ingot is 99.5%.

[0020] Furthermore, in step 4), the temperature of the homogenization treatment is 510-530° C., and the time of the homogenization treatment is 10-20 hours.

[0021] Furthermore, in step 4), the extrusion temperature is 400-420° C., and the extrusion ratio is 33:1.

[0022] The beneficial effects of the high-plasticity and low-rare-earth-content magnesium alloy material and the preparation method thereof of the present invention are as follows:

[0023] (1) The high-plasticity, low-rare-earth magnesium alloy provided by the present invention changes the magnesium matrix lattice structure through the alloying elements Gd, Zn and Ca, increases the room-temperature slip system, and at the same time, the addition of Gd, Zn and Ca, the co-segregation at the grain boundary will enhance the solid solution drag effect, inhibit the dynamic recrystallization during hot extrusion, hinder the grain growth, and achieve the effect of grain refinement, which can not only significantly improve the tensile strength and yield strength of the magnesium alloy material, but also make the elongation of the magnesium alloy material reach more than 40%, greatly improving the room-temperature plasticity of the magnesium alloy material and expanding its application range;

[0024] (2) The high-plasticity, low-rare earth magnesium alloy material provided by the present invention has a low degree of alloying and a low cost, and the equipment used is conventional general-purpose equipment, which is easy to industrialize and mass-produce, and is of great significance to the promotion of the application of magnesium alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 - is the stress-strain curve diagram of the magnesium alloy materials prepared in Example 1 and Example 2. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with the accompanying drawings and examples, but these specific implementation schemes do not limit the protection scope of the present invention in any way.

[0027] Example 1

[0028] A high-plasticity, low-content rare earth magnesium alloy material comprises the following components and their mass percentages: Gd 0.3%, Zn 0.5%, Ca 0.25%, and the balance is Mg and inevitable impurities. The mass percentage of inevitable impurities is ≤0.2%.

[0029] A method for preparing a high-plasticity and low-rare earth magnesium alloy material comprises the following steps:

[0030] 1) Raw material selection: pure zinc ingot (purity of 99.5%), pure magnesium ingot (purity of 99.99%), Mg-30Gd master alloy, and Mg-20Ca master alloy are selected as raw materials for preparing magnesium alloy materials;

[0031] 2) Ingredients: pure zinc ingots, pure magnesium ingots, Mg-30Gd master alloys, and Mg-20Ca master alloys are weighed according to the mass percentage of each component in the magnesium alloy material; wherein Zn is added in the form of pure zinc ingots, and Gd and Ca are added in the form of Mg-30Gd master alloys and Mg-20Ca master alloys, respectively;

[0032] 3) Melting: After heating the melting crucible to 400°C, add pure magnesium ingots. When the pure magnesium ingot is completely melted and heated to 740°C, add pure zinc ingots, Mg-30Gd master alloy, and Mg-20Ca master alloy in sequence. When the raw materials are completely melted, stir the melt for 4 minutes, salvage the slag on the surface of the melt, and let it stand for 40 minutes. Then cool it to 725°C and pour it into a metal mold to prepare an alloy ingot. The melting process is carried out under a protective atmosphere of CO2+SF6.

[0033] 4) Extrusion: firstly subject the alloy ingot obtained in step 3) to homogenization treatment at a temperature of 510° C. for 10 h, and then water-cooling; then subjecting the alloy ingot to extrusion at a temperature of 400° C. and an extrusion ratio of 33:1, to obtain the high-plasticity, low-rare-earth-content magnesium alloy material.

[0034] Example 2

[0035] A high-plasticity, low-rare-earth magnesium alloy material comprises the following components and their mass percentages: Gd 0.5%, Zn 1.0%, Ca 0.5%, and the balance is Mg and inevitable impurities. The mass percentage of inevitable impurities is ≤0.2%.

[0036] A method for preparing a high-plasticity and low-rare earth magnesium alloy material comprises the following steps:

[0037] 1) Raw material selection: pure zinc ingot (purity of 99.5%), pure magnesium ingot (purity of 99.99%), Mg-30Gd master alloy, and Mg-20Ca master alloy are selected as raw materials for preparing magnesium alloy materials;

[0038] 2) Ingredients: pure zinc ingots, pure magnesium ingots, Mg-30Gd master alloys, and Mg-20Ca master alloys are weighed according to the mass percentage of each component in the magnesium alloy material; wherein Zn is added in the form of pure zinc ingots, and Gd and Ca are added in the form of Mg-30Gd master alloys and Mg-20Ca master alloys, respectively;

[0039] 3) Melting: After heating the melting crucible to 400°C, add pure magnesium ingots. When the pure magnesium ingot is completely melted and heated to 730°C, add pure zinc ingots, Mg-30Gd master alloy, and Mg-20Ca master alloy in sequence. When the raw materials are completely melted, stir the melt for 3 minutes, salvage the slag on the surface of the melt, and let it stand for 30 minutes. Then cool it to 720°C and pour it into a metal mold to prepare an alloy ingot. The melting process is carried out under a protective atmosphere of CO2+SF6.

[0040] 4) Extrusion: firstly homogenize the alloy ingot obtained in step 3) at a temperature of 520° C. for 15 h, and then water-cool it; then extrude it at a temperature of 420° C. and an extrusion ratio of 33:1 to obtain the high-plasticity, low-rare-earth-content magnesium alloy material.

[0041] Example 3

[0042] The difference between this embodiment and embodiment 1 is that the mass percentages of the components are different, as shown in Table 1.

[0043] Example 4

[0044] The difference between this embodiment and embodiment 1 is that the mass percentages of the components are different, as shown in Table 1.

[0045] Example 5

[0046] The difference between this embodiment and embodiment 1 is that the mass percentages of the components are different, as shown in Table 1.

[0047] Example 6

[0048] The difference between this embodiment and embodiment 1 is that the mass percentages of the components are different, as shown in Table 1.

[0049] Comparative Example 1

[0050] The difference between this comparative example and Example 1 is that the mass percentages of the components are different, as shown in Table 1.

[0051] Comparative Example 2

[0052] The difference between this comparative example and Example 1 is that the mass percentages of the components are different, as shown in Table 1.

[0053] Table 1 Components and mass percentages in magnesium alloy materials prepared in Examples 1-6 and Comparative Examples 1-3

[0054]

[0055] Comparative Example 3

[0056] The difference between this comparative example and Example 1 lies in the different preparation methods, specifically: during the smelting process, the melting crucible is heated to 400°C and then a pure magnesium ingot is added; when the pure magnesium ingot is completely melted and the temperature is raised to 740°C, a Mg-30Gd intermediate alloy is added; after the pure magnesium ingot is completely melted, a pure zinc ingot and a Mg-20Ca intermediate alloy are added; when the raw materials are completely melted, the melt is stirred for 4 minutes, the scum on the surface of the melt is salvaged, and the melt is allowed to stand for 40 minutes; then the temperature is lowered to 725°C and poured into a metal mold to prepare an alloy ingot; the smelting process is carried out under a protective atmosphere of CO2+SF6.

[0057] The present invention has carried out the performance test of tensile strength, yield strength and elongation of the magnesium alloy materials prepared in Examples 1-6 and Comparative Examples 1-3 at room temperature. The stress-strain curves of Example 1 and Example 2 are shown in FIG. Figure 1 shown.

[0058] Table 2 Tensile strength, yield strength and elongation of magnesium alloy materials prepared in Examples 1-6 and Comparative Examples 1-4 at room temperature

[0059]

[0060]

[0061] As can be seen from the above table, the elongation of the magnesium alloy materials corresponding to Examples 1-6 is greater than 40%, and the Zn and Ca elements added in Comparative Examples 1-2 exceed the range specified in this application, and the corresponding elongation is less than 40%. Analysis shows that the present invention adopts the method of adding low-content Gd, Zn and Ca elements to the magnesium alloy, which significantly improves the elongation of the magnesium alloy material at room temperature, and can significantly improve the room temperature plasticity of the magnesium alloy material under the weakening texture and grain refinement of the low-content Gd, Zn and Ca elements. However, the addition of excessive Zn and Ca elements will not only be unfavorable to the improvement of the plasticity of the magnesium alloy material, but also increase the production cost of the magnesium alloy material.

[0062] In the preparation of magnesium alloy material, Comparative Example 3 adopts the method of adding Mg-30Gd master alloy, pure zinc ingot and Mg-20Ca master alloy in batches after the pure magnesium ingot is completely melted, while Example 1 of the present application adopts the method of adding Mg-30Gd master alloy, pure zinc ingot and Mg-20Ca master alloy together into the completely melted pure magnesium ingot for melting, and the elongation of the magnesium alloy material corresponding to Comparative Example 3 is also significantly lower than that of Example 1. It shows that the method of adding other raw materials simultaneously instead of adding them in batches after the pure magnesium ingot is completely melted in the present application can effectively reduce the mixing of impurities, effectively improve the elongation of the magnesium alloy material, significantly improve the plasticity of the magnesium alloy material, and improve the mechanical properties of the magnesium alloy material.

[0063] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A high plasticity and low rare earth content magnesium alloy material, characterized in that: The magnesium alloy material includes the following components and their mass percentages: Gd 0-1%, Zn 0-1.5%, Ca 0-0.8%, and the rest are Mg and inevitable impurities, wherein the content of Gd is not 0, and the sum of the mass percentages of Gd, Zn and Ca elements is 42%.

2. A high plasticity and low rare earth content magnesium alloy material as claimed in claim 1, characterized in that: The magnesium alloy material comprises the following components and their mass percentages: Gd 0.1-1%, Zn 0-1.5%, Ca 0-0.8%, the remainder being Mg and inevitable impurities, and the sum of the mass percentages of Gd, Zn and Ca elements is 42%.

3. A high plasticity and low rare earth content magnesium alloy material as claimed in claim 2, characterized in that: The magnesium alloy material includes the following components and their mass percentages: 0.3% Gd, 0.5% Zn, 0.25% Ca, and the rest being Mg and inevitable impurities.

4. A high plasticity and low rare earth content magnesium alloy material as claimed in claim 2, characterized in that: The magnesium alloy material includes the following components and their mass percentages: Gd 0.5%, Zn 1.0%, Ca 0.5%, and the rest is Mg and inevitable impurities.

5. A high plasticity and low rare earth content magnesium alloy material as claimed in any one of claims 1 to 4, characterized in that: The mass percentage of the unavoidable impurities is ≤0.2%.

6. A method for preparing a high-plasticity, low-rare-earth magnesium alloy material according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) Raw material selection: pure zinc ingot, pure magnesium ingot, Mg-30Gd master alloy and Mg-20Ca master alloy are selected as raw materials for preparing magnesium alloy materials; 2) Ingredients: weigh pure zinc ingots, pure magnesium ingots, Mg-30Gd master alloy, and Mg-20Ca master alloy according to the mass percentage of each component in the magnesium alloy material; 3) Melting: After heating the melting crucible to 400°C, add pure magnesium ingots. When the pure magnesium ingots are completely melted and heated to 730-750°C, add pure zinc ingots, Mg-30Gd master alloys, and Mg-20Ca master alloys in sequence. When the raw materials are completely melted, stir the melt for 3-5 minutes, salvage the scum on the surface of the melt, and let it stand for 30-50 minutes. Then cool it to 720-730°C and pour it into a metal mold to prepare an alloy ingot. The melting process is carried out under a protective atmosphere of CO2+SF6. 4) Extrusion: firstly homogenize the alloy ingot obtained in step 3), and then water-cool it; and then extrude it to obtain the high-plasticity and low-rare-earth-content magnesium alloy material.

7. A method for preparing a high-plasticity and low-rare earth magnesium alloy material as claimed in claim 6, characterized in that: The temperature of the homogenization treatment in step 4) is 510-530° C., and the time of the homogenization treatment is 10-20 hours.

8. The method for preparing a high-plasticity and low-rare-earth magnesium alloy material as claimed in claim 6, characterized in that: The extrusion temperature in step 4) is 400-420° C., and the extrusion ratio is 33:1.

Citation Information

Cited By

  • High-performance magnesium alloy and preparation method thereof

    CN121700215A