Solid solution material, preparation method and application thereof, hard alloy cutter and manufacturing method

By using solid solution materials of TiCN, WC, Ta(Nb)C, Mo2C, Ni and Co to prepare cemented carbide cutting tools, the problems of W resource consumption, cost and performance of cemented carbide cutting tools are solved, and less Tungsten, low-cost, high-performance cutting blade with improved wear resistance and anti-stick properties.

CN118745544APending Publication Date: 2024-10-08四川圣才科技开发有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410810477.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing carbide cutting tools consume too much W resources in the manufacturing process, have high raw material costs, and have poor cutting performance, especially high friction resistance, insufficient wear resistance and toughness, and poor anti-stick properties, resulting in rapid damage to the tool.

Method used

A solid solution material is used, including TiCN, WC, Ta(Nb)C, Mo2C, Ni and Co, and a cemented carbide cutting tool is prepared through a specific ball milling and drying process to reduce the use of WC and increase the content of Mo2C to reduce friction. coefficient, and utilizes the inert nature of TiCN to reduce reactions with processed materials.

Benefits of technology

A tungsten-less, low-cost, high-performance cemented carbide cutting tool has been realized, saving 50-60% of WC resources, reducing raw material costs, improving the wear resistance and toughness of the cutting tool, enhancing anti-sticking properties, and reducing density More than 30%, the output rate per unit weight is increased by more than 30%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745544A_ABST
    Figure CN118745544A_ABST
Patent Text Reader

Abstract

The invention relates to a solid solution material, a preparation method and application thereof, a hard alloy cutter and a manufacturing method, and relates to the technical field of hard alloy preparation, the solid solution material comprises the following components by weight: 35-62% of TiCN, 10-20% of WC, 5-15% of Ta (Nb) C, 3-5% of Mo2C, 10-20% of Ni, and 0-5% of Co. The solid solution material is prepared by using the commercially available metal ceramic blank as the raw material, and is further applied to the preparation of the hard alloy cutting knife, so that the hard alloy cutting knife with less tungsten, low cost and high performance is obtained, and the problems of W resource consumption, high raw material cost, poor cutting performance and the like in the manufacturing of the existing hard alloy cutting knife are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cemented carbide preparation, and in particular to a solid solution material and a preparation method and application thereof, a cemented carbide cutting tool and a manufacturing method thereof. Background Art

[0002] Cemented carbide is an alloy material made of hard chemical of refractory metal and bonding metal through powder metallurgy process. Cemented carbide has a series of excellent properties such as high hardness, high wear resistance, high strength, good toughness, heat resistance and corrosion resistance, especially its high hardness and wear resistance, which makes it particularly suitable for use as a cutting tool.

[0003] Cemented carbide cutting tools are widely used in metal and non-metal cutting, hole processing, etc. They are also called industrial teeth and are mainly used for rotary milling cutters in CNC machining centers and CNC machine tool cutting blades. The existing technology uses WC-Co (or WC-TiC-Co) as the main chemical composition to produce cemented carbide cutting tools (currently a small number of domestic companies also use metal ceramic cutting tools). In order to improve the cutting performance of cemented carbide cutting tools, both KPM-type cemented carbide cutting tools are composite solid solutions as much as possible. The solid solution components are WC-Ta(Nb)C, WC-TiC, WC-Ta(Nb)C-TiC, etc. Even if the solid solutions of this type are composited, this type of conventional cemented carbide cutting tool still has the following disadvantages: (1) The WC content is high, reaching 80-95%, which consumes W resources; (2) The friction coefficient is large. Since no lubricant material similar to Mo2C is added to the composition, the friction resistance is large during the cutting process, which makes the cutting of the blade difficult. The force increases, making the wear resistance and toughness of the cutting tool worse; (3) Poor anti-sticking performance: Since WC and Co are materials with high chemical activity, high temperatures are generated during the cutting process, and they are easy to react or have affinity with certain chemical components or elements in the processed material, resulting in sticking or crescent pits, which quickly damage the tool; (4) Poor red hardness. In most cases, the composite solid solution of conventional cemented carbide cutting tools is WC-TiC. If the red hardness is to be improved, WC-Ta(Nb)C [its solid solution form is WC-Ta(Nb)C or WC-TiC-Ta(Nb)C] carbides need to be added. Since Ta(Nb)C is a type of extremely expensive chemical, in order to obtain high red hardness, the raw material cost of the prepared conventional cemented carbide cutting tools will be greatly increased. Summary of the invention

[0004] In order to solve the problems of existing cemented carbide cutting tools consuming W resources, high raw material costs, poor cutting performance, etc., the present invention provides a solid solution material and a preparation method and application thereof, a cemented carbide cutting tool and a manufacturing method thereof.

[0005] In a first aspect, the present invention provides a solid solution material, wherein the solid solution material comprises the following components in weight percentage:

[0006] TiCN: 35-62%, WC: 10-20%, Ta(Nb)C: 5-15%, Mo2C: 3-5%, Ni: 10-20%, Co: 0-5%.

[0007] In a second aspect, the present invention provides a method for preparing the solid solution material according to any one of the first aspects, the preparation method comprising the following steps:

[0008] crushing the metal ceramic blank to obtain metal ceramic particles;

[0009] The metal ceramic particles are subjected to a first ball milling, and then subjected to a first screening to obtain a metal ceramic wet material;

[0010] The metal ceramic wet material is dried for the first time to obtain the solid solution material.

[0011] In a third aspect, the present invention provides use of the solid solution material described in any one of the first aspect and the second aspect in preparing cemented carbide cutting tools.

[0012] In a fourth aspect, the present invention provides a method for preparing a cemented carbide cutting tool, the method comprising the following steps:

[0013] According to the use requirements, the required percentage content of WC, Co and the solid solution material described in claim 1 or 2 in the cemented carbide cutting tool formula is designed;

[0014] According to the required percentage content of WC, Co and the solid solution material according to claim 1 or 2 in the cemented carbide cutting tool formula, ingredients are prepared to obtain a mixture;

[0015] The mixed material is ball-milled for a second time, and then dried for a second time to obtain a dry mixed material;

[0016] The dry mixed material and the cemented carbide forming agent are mixed, and then sieved for a second time to obtain a cemented carbide cutting blade mixture;

[0017] The cemented carbide cutting blade mixture is pressed and then sintered to obtain the cemented carbide cutting blade.

[0018] Further, the cemented carbide cutting tool formula includes the following components in weight percentage:

[0019] TiCN: 44%, WC: 31.5%, Ta(Nb)C: 6%, Mo2C: 3%, Ni: 9.5%, Co: 6%; or,

[0020] The cemented carbide cutting tool formulation includes the following components in weight percentage:

[0021] TiCN: 13.5%, WC: 61%, Ta(Nb)C: 3.6%, Mo2C: 1.5%, Ni: 5.4%, Co: 15%.

[0022] Furthermore, the working condition parameters of the second ball mill include: a ball-to-material ratio of 4:1, a solid-liquid ratio of 1kg / 300ml, and ball milling at room temperature.

[0023] Furthermore, the cemented carbide forming agent includes at least one of SD-A and SD-B types in SD glue.

[0024] Furthermore, the amount of the cemented carbide forming agent added is 100-110 ml per 1 kg of the dry mixture.

[0025] Furthermore, the working condition parameters of the pressing include: the shrinkage coefficient of the pressed blank is 1.25-1.27, and the pressing method of the rod blank for the rotary milling cutter is: standard cutters use rod molding, small-size rods below ≤Φ6 use self-pressing, rods ≥100mm use extrusion, and rods with a diameter of ≥Φ16 use dry bag pressing.

[0026] Furthermore, the sintering working condition parameters include: a sintering temperature of 1450-1500° C. and a sintering time of 2-3 hours.

[0027] In a fifth aspect, the present invention provides a cemented carbide cutting tool, wherein the cemented carbide cutting tool is prepared by the method for preparing a cemented carbide cutting tool according to any one of the fourth aspects.

[0028] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:

[0029] The embodiment of the present invention provides a solid solution material and a preparation method and application thereof, a cemented carbide cutting tool and a manufacturing method thereof. The present invention uses commercially available metal ceramic blanks as raw materials to prepare a solid solution material, and further applies it to the preparation of cemented carbide cutting tools, thereby obtaining a low-tungsten, low-cost, high-performance cemented carbide cutting tool, which solves the problems of existing cemented carbide cutting tool manufacturing consuming W resources, high raw material costs, and poor cutting performance. Specifically:

[0030] 1. Compared with conventional solid solution of cemented carbide, the new solid solution contains a small amount of WC, generally less than 20%. The solid solution itself is a cemented carbide cutting tool material. Even if no or a small amount of conventional cemented carbide cutting tool material components (WC, Co) are added, it can be prepared into a cutting tool; under the condition that the toughness and bending strength are not required to be high, such as finishing and semi-finishing, a small amount of conventional cemented carbide material components (WC.Co) are added to the cutting tool to make its total WC percentage less than 30%, and its density is 8.0-9.0g / cm 3 It can save more than 50-60% of WC resources.

[0031] If the toughness and bending strength requirements are high, such as rough machining, the cutting material can appropriately increase the percentage of WC and Co, and the WC percentage is less than 60%; the density is 10.0-10.7g / cm 3 Between, more than 20-30% of WC resources can be saved.

[0032] 2. Compared with conventional solid solution, if the old metal ceramic blank is used as the new solid solution raw material, the direct raw material is greatly reduced, reduced by 2 / 3. In addition, the cutting tool of the present invention has a light density (8,0-10.7g / cm 3 ), compared with the density of conventional hard alloy cutting tools (12.0~15g / cm 3 ) is more than 30% lower, so the product output rate per unit weight is more than 30% higher, so its comprehensive cost is more than 60% lower than that of conventional cutting knives.

[0033] 3. Compared with conventional solid solutions, the new solid solution itself contains a high content of Ta(Nb)C. Therefore, there is no need to process the solid solution containing Ta(Nb)C. This can significantly increase the cost of raw materials and improve the red hardness of the hard alloy cutting tool at a low cost.

[0034] 4. Compared with the cutting blade containing TiC solid solution (PM type brand cutting blade), the new solid solution has TiCN as the main component, and its bending strength and toughness are much higher than TiC, and are close to WC type materials. When the production is properly controlled, the bending strength of the cutting blade prepared by this solid solution alone can reach more than 2400MPa, which is equivalent to the bending strength of WC-Co type cutting blades. Therefore, in addition to its high hardness, the toughness of the cutting blade prepared by the present invention is also improved. For example, the skinning knife described in Example 2 has a hardness of 90.3HRA and a fracture toughness of 12MPa√m after testing. The conventional brand YG8 in the national standard has a hardness of 89.5HRA and a fracture toughness of 10.5MPa√m.

[0035] 5. The new solid solution contains Mo2C-type lubricating components, which greatly reduce the friction coefficient during the processing and correspondingly improve the wear resistance and toughness of the cutting tool.

[0036] 6. The main component of the new solid solution TiCN is a kind of inert material (relative to WC), which is not easy to react with certain components or elements of the processed material during high-temperature processing, so the tool has good anti-sticking (or anti-crescent crater) performance. The WC added to the cutting tool material of the present invention is a Cr-added WC. This WC forms a chromium oxide protective film on the surface of the WC during high-temperature processing, which also makes the tool not easy to react with certain components or elements of the processed material, so the invented cutting tool has extremely high anti-sticking (or anti-crescent crater) performance.

[0037] In summary, the present invention is a low-tungsten, low-cost, high-performance cemented carbide cutting tool, which is a promising new type of cemented carbide, and its invention is an industry-disruptive technological innovation. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0040] Figure 1 Schematic diagram of a new solid solution cemented carbide Φ8 standard rod blank in an embodiment of the present invention.

[0041] Figure 2 Schematic diagram of a new solid solution cemented carbide Φ8 standard milling cutter in an embodiment of the present invention.

[0042] Figure 3 Schematic diagram of a new solid solution cemented carbide peeling knife in an embodiment of the present invention. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0045] In a first aspect, the present invention provides a solid solution material, wherein the solid solution material comprises the following components in weight percentage:

[0046] TiCN: 35-62%, WC: 10-20%, Ta(Nb)C: 5-15%, Mo2C: 3-5%, Ni: 10-20%, Co: 0-5%.

[0047] The embodiment of the present invention provides a solid solution material. The present invention uses commercially available metal ceramic blanks as raw materials to prepare the solid solution material, and further applies it to the preparation of cemented carbide cutting tools, thereby obtaining a low-tungsten, low-cost, high-performance cemented carbide cutting tool, which solves the problems of existing cemented carbide cutting tools consuming W resources, high raw material costs, and poor cutting performance. Specifically:

[0048] 1. Compared with conventional solid solution of cemented carbide, the new solid solution contains a small amount of WC, generally less than 20%. The solid solution itself is a cemented carbide cutting tool material. Even if no or a small amount of conventional cemented carbide cutting tool material components (WC, Co) are added, it can be prepared into a cutting tool; under the condition that the toughness and bending strength are not required to be high, such as finishing and semi-finishing, a small amount of conventional cemented carbide material components (WC.Co) are added to the cutting tool to make its total WC percentage less than 30%, and its density is 8.0-9.0g / cm 3 It can save more than 50-60% of WC resources.

[0049] If the toughness and bending strength requirements are high, such as rough machining, the cutting material can appropriately increase the percentage of WC and Co, and the WC percentage is less than 60%; the density is 10.0-10.7g / cm 3 Between, more than 20-30% of WC resources can be saved.

[0050] 2. Compared with conventional solid solution, if the old metal ceramic blank is used as the new solid solution raw material, the direct raw material is greatly reduced, reduced by 2 / 3. In addition, the cutting tool of the present invention has a light density (8,0-10.7g / cm 3 ), compared with the density of conventional hard alloy cutting tools (12.0~15g / cm 3 ) is more than 30% lower, so the product output rate per unit weight is more than 30% higher, so its comprehensive cost is more than 60% lower than that of conventional cutting knives.

[0051] 3. Compared with conventional solid solutions, the new solid solution itself contains a high content of Ta(Nb)C. Therefore, there is no need to process the solid solution containing Ta(Nb)C. This can significantly increase the cost of raw materials and improve the red hardness of the hard alloy cutting tool at a low cost.

[0052] 4. Compared with the cutting blade containing TiC solid solution (PM type brand cutting blade), the new solid solution has TiCN as the main component, and its bending strength and toughness are much higher than TiC, and are close to WC type materials. When the production is properly controlled, the bending strength of the cutting blade prepared by this solid solution alone can reach more than 2400MPa, which is equivalent to the bending strength of WC-Co type cutting blades. Therefore, in addition to its high hardness, the toughness of the cutting blade prepared by the present invention is also improved. For example, the skinning knife described in Example 2 has a hardness of 90.3HRA and a fracture toughness of 12MPa√m after testing. The conventional brand YG8 in the national standard has a hardness of 89.5HRA and a fracture toughness of 10.5MPa√m.

[0053] 5. The new solid solution contains Mo2C-type lubricating components, which greatly reduce the friction coefficient during the processing and correspondingly improve the wear resistance and toughness of the cutting tool.

[0054] 6. The main component of the new solid solution TiCN is a kind of inert material (relative to WC), which is not easy to react with certain components or elements of the processed material during high-temperature processing, so the tool has good anti-stickiness (or anti-crescent crater) performance. The WC added to the cutting tool material of the present invention is a Cr-added WC. This WC forms a chromium oxide protective film on the surface of the WC during high-temperature processing, which also makes the tool not easy to react with certain components or elements of the processed material, so the cutting tool of the invention has extremely high anti-stickiness (or anti-crescent crater).

[0055] In summary, the present invention is a low-tungsten, low-cost, high-performance cemented carbide cutting tool, which is a promising new type of cemented carbide, and its invention is an industry-disruptive technological innovation.

[0056] In a second aspect, the present invention provides a method for preparing the solid solution material according to any one of the first aspects, the preparation method comprising the following steps:

[0057] crushing the metal ceramic blank to obtain metal ceramic particles;

[0058] The metal ceramic particles are subjected to a first ball milling, and then subjected to a first screening to obtain a metal ceramic wet material;

[0059] The metal ceramic wet material is first dried to obtain the solid solution material.

[0060] In some specific embodiments, the metal ceramic blank can be a commercially available metal ceramic blank, whether new or old, and old blanks can be selected as much as possible to reduce costs, and the blank surface is cleaned with a special cemented carbide cleaning agent. Specifically, any model and specification of blades or any model and specification of milling cutters in commercially available metal ceramic blanks can be selected, or any model and specification of a mixed blank of blades and milling cutters can be selected.

[0061] In some specific embodiments, the method for preparing the solid solution material comprises the following process:

[0062] ①. Commercially available metal ceramic blanks, regardless of new or old, should be used as much as possible to reduce costs, and the surface of the blanks should be cleaned with a special cemented carbide cleaning agent;

[0063] ②. Manually or mechanically crush the briquettes into 1-2 mm particles;

[0064] ③. Load the crushed billet particles into a ball mill for ball milling. The ball material is YG8 hard alloy, and anhydrous alcohol is used as the wet grinding liquid. The process parameters are: ball milling time 18-24 hours, crushing ball diameter Φ12-Φ100mm, ball-to-material ratio 4:1, solid-liquid ratio 1kg / 300ml;

[0065] ④. Unload the material at the end of the time, and the wet-milled material will pass through a 120-mesh sieve;

[0066] ⑤. Send the sieved wet abrasive to a drying oven for drying to obtain dry powder;

[0067] ⑥ Send the dried powder for testing and determine the percentage of each component for future use.

[0068] In a third aspect, the present invention provides use of the solid solution material described in any one of the first aspect and the second aspect in preparing cemented carbide cutting tools.

[0069] In a fourth aspect, the present invention provides a method for preparing a cemented carbide cutting tool, the method comprising the following steps:

[0070] According to the use requirements, the required percentage content of WC, Co and the solid solution material described in claim 1 or 2 in the cemented carbide cutting tool formula is designed;

[0071] According to the required percentage content of WC, Co and the solid solution material according to claim 1 or 2 in the cemented carbide cutting tool formula, ingredients are prepared to obtain a mixture;

[0072] The mixed material is ball-milled for a second time, and then dried for a second time to obtain a dry mixed material;

[0073] The dry mixed material and the cemented carbide forming agent are mixed, and then sieved for a second time to obtain a cemented carbide cutting blade mixture;

[0074] The cemented carbide cutting blade mixture is pressed and then sintered to obtain the cemented carbide cutting blade.

[0075] In some specific embodiments, the cemented carbide cutting tool formulation includes the following components by weight percentage:

[0076] TiCN: 44%, WC: 31.5%, Ta(Nb)C: 6%, Mo2C: 3%, Ni: 9.5%, Co: 6%; or,

[0077] The cemented carbide cutting tool formulation includes the following components in weight percentage:

[0078] TiCN: 13.5%, WC: 61%, Ta(Nb)C: 3.6%, Mo2C: 1.5%, Ni: 5.4%, Co: 15%.

[0079] In some specific embodiments, the working condition parameters of the second ball mill include: a ball-to-material ratio of 4:1, a solid-liquid ratio of 1 kg / 300 ml, and ball milling at room temperature.

[0080] In some specific embodiments, the cemented carbide forming agent includes at least one of SD-A and SD-B types in SD glue.

[0081] In some specific embodiments, the amount of the cemented carbide forming agent added is 100-110 ml per 1 kg of the dry mixture.

[0082] In some specific embodiments, the working condition parameters of the pressing include: the shrinkage coefficient of the pressed blank is 1.25-1.27, and the pressing method of the rod blank for the rotary milling cutter is: the standard cutter adopts the rod molding method, the small-size rods below ≤Φ6 use self-pressing, the rods ≥100mm use extrusion, and the rods with a diameter ≥Φ16 use dry bag pressing.

[0083] In some specific embodiments, the sintering working condition parameters include: a sintering temperature of 1450-1500° C. and a sintering time of 2-3 hours.

[0084] In some specific embodiments, the method for preparing the cemented carbide cutting tool comprises the following steps:

[0085] 1. Prepare solid solution powder;

[0086] 2. Ingredients: According to the use requirements of the cutting tool, the required percentage content of each component (WC, Co, solid solution) is designed for the cutting tool formula, and then the weight of each component is calculated according to the percentage of each component, and then mixed and sent to the ball mill;

[0087] 3. Ball milling: The mixed material obtained in step 2 is placed in a ball mill for wet milling, with a ball-to-material ratio of 4:1 and a solid-liquid ratio of 1kg / 300ml. The mixed material is ball milled at room temperature for 36 hours to obtain a wet material.

[0088] 4. Drying: After the ground wet material obtained in step 3 is used to recover the alcohol in a vacuum dryer, it is dried in a steam drying oven to constant weight to obtain a dry powder;

[0089] 5. Adding glue: the dry powder obtained in step 4 is added with SD-B glue forming agent in a stirrer and stirred evenly for 2 minutes, the amount of glue added is 100-110 ml / lkg, and sieved through a 60-100 mesh sieve to obtain the composite new solid solution cemented carbide cutting tool mixture;

[0090] 6. Pressing: Press the mixture obtained in step 5. Design a mold according to the shape requirements of the cutting tool. The mold shrinkage coefficient is quite different from that of conventional cemented carbide cutting tools (the shrinkage coefficient of conventional cemented carbide cutting tools is generally 1.18-1.25). The shrinkage coefficient of the compact of the present invention is 1.25-1.27. The pressing method of the bar blank for the rotary milling cutter is: standard bar is pressed by die, small bar is pressed by self-pressing, long bar is ≥100mm or more by extrusion, and bar diameter is ≥16 or more by dry bag pressing. The obtained compact is sent for sintering;

[0091] 7. Sintering: The compact obtained in step 6 is sent to a low-pressure sintering furnace for sintering. The surface of the boat for placing the compact for sintering should be painted with high cobalt paint to prevent the contact surface with the boat from sticking to the boat, so that the product is carburized. The temperature in the furnace is controlled at 1450-1500°C and kept warm for 2-3 hours to obtain a sintered blank product, which is sent for testing. A qualified blank is obtained if it passes the test;

[0092] 8. Further processing: The qualified sintered blank obtained in step 7 is subjected to further processing such as fine grinding, passivation, surface treatment, grooving, etc. After the size inspection is qualified, the finished cutting knife is stored and packaged for sale.

[0093] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0094] Example 1

[0095] This embodiment provides a composite new solid solution cemented carbide cutting tool, including a new solid solution and a conventional cemented carbide cutting tool material (WC, Co), wherein the WC is WC with Cr added, and the new solid solution is a prefabricated alloy powder of a metal ceramic material. The implementation steps are as follows:

[0096] 1. Preparation of new solid solution: ① Use a special carbide cleaning agent to clean the old blank of commercially available metal ceramics; ② Manually or mechanically crush the blank into 1-2 mm particles; ③ Load the crushed blank particles into a ball mill for ball milling, and its process parameters are: ball milling time 18-24 hours, ball-to-material ratio 4:1, solid-liquid ratio 1kg / 300ml; ④ Unload the material at the time, and pass the wet material through a 120-mesh sieve;

[0097] ⑤ Send the sieved wet material to a drying oven for drying to obtain dry powder; ⑥ The dried and sieved wet material is sent for inspection, and a solid solution composition and percentage content are measured: TiCN: 58%, WC: 15%, Ta(Nb)C: 8%, Mo2C: 4%, Ni: 13%, Co: 2%. A dry solid solution powder is prepared for use.

[0098] 2. Ingredients: According to the use requirements of the cemented carbide cutting tool, the cemented carbide cutting tool is a milling cutter for aluminum alloy processing. The use requirements refer to finishing and semi-finishing. Then, the percentage of each component required for the invented cemented carbide cutting tool formula is designed. The formula and the required percentage of each component are: TiCN: 44%, WC: 31.5%, Ta (Nb) C: 6%, Mo2C3%, Ni: 9.5%, Co: 6%. According to the above component percentages, combined with the percentage data of the prepared solid solution powder, it is concluded that the ingredients need to add WC20% (WC contains 0.5% Cr), Co4.5%, and solid solution powder 75.5%. The ingredients weigh 20kg, and it is necessary to weigh WC4kg, Co0.9kg, and solid solution powder 15.1kg, that is, the mixture required by the formula is obtained.

[0099] 3. Ball milling: The mixed material obtained in step 2 is fed into a ball mill for wet grinding, with a ball-to-material ratio of 4:1 (i.e. 80:20), a solid-liquid ratio of 1kg / 300ml (i.e. 20kg / 6ooml), and ball milling at room temperature for 36 hours to obtain a wet material.

[0100] 4. Drying: After the ground wet material obtained in step 3 is used to recover the alcohol in a vacuum dryer, it is dried in a steam drying oven to obtain a dry powder.

[0101] 5. Adding glue: Add SD glue forming agent to the dry powder obtained in step 4 and stir evenly in a stirrer for 2 minutes. Add 105 ml / 1 kg of glue and sieve through a 60-100 mesh sieve to obtain the composite new solid solution cemented carbide cutting tool mixture of Experimental Example 1.

[0102] 6. Pressing: The mixture obtained in step 5 is pressed. The product of this embodiment is a Φ8 standard rod blank (see Figure 1), designed as a manual molding die, the die shrinkage coefficient is 1.27, the pressing is carried out by manual molding, the green compact weight = 4.4x4.4x3.14x61x0.0085 = 31.5g, where 4.4 is the rod radius, 61 is the rod length, 3.14 is the π value, and 0.0085 is the theoretical density of the product of the present invention. The obtained green compact is sent for sintering.

[0103] 7. Sintering: The compact obtained in step 6 is sent to a low-pressure sintering furnace for sintering. The surface of the boat for placing the compact for sintering should be painted with high cobalt paint to prevent the sintered blank from contacting the boat and sticking to the boat, resulting in carburization of the sintered blank. The temperature in the furnace is controlled at 1450-1500℃ and kept warm for 2-3 hours to obtain a sintered standard bar Φ8 blank product (see Figure 1 ).

[0104] 8. Further processing: The Φ8 standard rod blank obtained in step 7 was sent for inspection, and the inspection results were: ① Porosity A02B00C00, hardness 92.2HRA, density 8.45g / Cm 3 , fracture toughness 8.2MPa√m. Then the Φ8 rod blank is sent to the coreless grinder for fine grinding to make the size meet the requirements of fine grinding rod, and the Φ8 standard fine grinding rod is sent to the machining center for slotting and fine grinding to make its size, angle, cutting edge, finish, etc. meet the use requirements and become a finished milling cutter for aluminum alloy fine and semi-finishing (see Figure 2 ), pack the finished milling cutters and put them into storage.

[0105] Example 2

[0106] This embodiment provides a composite solid solution cemented carbide cutting tool, including a new solid solution and a conventional cemented carbide cutting tool material (WC, Co), wherein the WC is WC with Cr added, and the new solid solution is a metal ceramic pre-alloy powder. The implementation steps are as follows:

[0107] 1. Preparation of new solid solution: ① Use a special cemented carbide cleaning agent to clean the surface of the old metal ceramic blank on the market; ② Manually or mechanically break the blank into 1-2mm particles; ③ Load the crushed blank particles into a ball mill for ball milling, and its process parameters are: ball milling time 18-24 hours, ball-to-material ratio 4:1, solid-liquid ratio 1kg / 300ml; ④ Unload the material at the time, and pass the wet material through a 120-mesh sieve; ⑤ Send the sieved wet material to a drying oven for drying to obtain a dry powder; ⑥ Send the dried and sieved wet material for inspection, and measure a solid solution component and percentage content: TiCN: 47.9%, WC: 17.1%, Ta(Nb)C: 12%, Mo2C: 5%, Ni: 18%, Co: 0%. The prepared dry solid solution powder is ready for use.

[0108] 2. Ingredients: According to the use requirements of cemented carbide cutting tools, the cemented carbide cutting tools are peeling blades for processing 304 and 316 stainless steel bars. The use requirements are rough processing occasions that withstand strong impacts, in order to verify how much impact the product of the invention can withstand, so as to expand the application scope of the invention product. Then the cemented carbide cutting tool formula and the required percentage of each component are designed: TiCN: 13.5%, WC: 61%, Ta (Nb) C: 3.6%, Mo2C: 1.5%, Ni: 5.4%, Co: 15%. The ingredients weigh 50kg. According to the above ingredient percentages, combined with the percentage data of the prepared solid solution powder, it is concluded that the ingredients need to add WC27.5kg (WC contains Cr0.4%), Co7.5kg, and solid solution 15kg to obtain the mixture required by the formula.

[0109] 3. Ball milling: The mixed material obtained in step 2 is fed into a ball mill for wet grinding, with a ball-to-material ratio of 4=1 (i.e. 200:50), a solid-liquid ratio of 1kg / 300ml (i.e. 50kg / 15000ml), and ball milling at room temperature for 36 hours to obtain a wet material.

[0110] 4. Drying: After the ground wet material obtained in step 3 is used to recover the alcohol in a vacuum dryer, it is dried in a steam drying oven to obtain dry powder.

[0111] 5. Adding glue: Add SD glue forming agent to the dry powder obtained in step 4 and stir evenly in a stirrer for 2 minutes. Add glue in an amount of 100-110 ml / 1 kg (i.e. 5000-5500 ml / 50 kg). Sieve through a 60-100 mesh sieve to obtain a new solid-liquid cemented carbide cutting tool mixture of Example 2.

[0112] 6. Pressing: Press the mixture obtained in step 5. The product of this embodiment is a peeling blade (see Figure 3 ), the designed mold shrinkage coefficient is 1.26, and the unit weight of the pressed green sheet = (62 / 14.8) x 10.7 (g) = 45g, where: 62 is the unit weight of the skinning knife of the same model as YG8;

[0113] 10.7 is the theoretical calculated density of the product of the present invention; 14.8 is the theoretical density of YG8, and the obtained compact is sent for sintering.

[0114] 7. Sintering: The peeling knife blank obtained in step 6 is sent to a low-pressure sintering furnace for sintering. The surface of the boat where the blank is placed for sintering should be painted with high cobalt paint to prevent the sintered blank from contacting the boat and sticking to the boat, causing carburization of the sintered blank. The temperature in the furnace is controlled at 1450-1500℃; keep warm for 2-3 hours to obtain a sintered peeling knife blank product (see Figure 3 ).

[0115] 8. Inspection and further processing: The peeling knife blank obtained in step 7 is sent for inspection, and the inspection results are: a. Porosity A02B00C00, b. Hardness 90.2HRA, c. Density 10.7g / Cm3, d. Fracture toughness 12MPa√m. Then the surface of the peeling knife blank is passivated, and the peeling knife is packaged and stored.

[0116] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which are applicable regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0117] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A solid solution material, characterized in that: The solid solution material comprises the following components in weight percentage: TiCN: 35-62%, WC: 10-20%, Ta(Nb)C: 5-15%, Mo2C: 3-5%, Ni: 10-20%, Co: 0-5%.

2. A method for preparing the solid solution material according to claim 1, characterized in that: The preparation method comprises the following steps: crushing the metal ceramic blank to obtain metal ceramic particles; The metal ceramic particles are subjected to a first ball milling, and then subjected to a first screening to obtain a metal ceramic wet material; The metal ceramic wet material is dried for the first time to obtain the solid solution material.

3. Use of the solid solution material according to claim 1 or 2 in the preparation of cemented carbide cutting tools.

4. A method for preparing a cemented carbide cutting tool, characterized in that: The preparation method comprises the following steps: According to the use requirements, the required percentage content of WC, Co and the solid solution material described in claim 1 or 2 in the cemented carbide cutting tool formula is designed; According to the required percentage content of WC, Co and the solid solution material according to claim 1 or 2 in the cemented carbide cutting tool formula, ingredients are prepared to obtain a mixture; The mixed material is ball-milled for a second time, and then dried for a second time to obtain a dry mixed material; The dry mixed material and the cemented carbide forming agent are mixed, and then sieved for a second time to obtain a cemented carbide cutting blade mixture; The cemented carbide cutting blade mixture is pressed and then sintered to obtain the cemented carbide cutting blade.

5. The method for preparing a cemented carbide cutting tool according to claim 4, characterized in that: The cemented carbide cutting tool formulation includes the following components in weight percentage: TiCN: 44%, WC: 31.5%, Ta(Nb)C: 6%, Mo2C3%, Ni: 9.5%, Co: 6%; or, The cemented carbide cutting tool formulation includes the following components in weight percentage: TiCN: 13.5%, WC: 61%, Ta(Nb)C: 3.6%, Mo2C: 1.5%, Ni: 5.4%, Co: 15%.

6. The method for preparing a cemented carbide cutting tool according to claim 4, characterized in that: The working condition parameters of the second ball milling include: a ball-to-material ratio of 4:1, a solid-liquid ratio of 1kg / 300ml, and ball milling at room temperature.

7. The method for preparing a cemented carbide cutting tool according to claim 4, characterized in that: The cemented carbide forming agent includes at least one of SD-A and SD-B types in the SD glue series.

8. The method for preparing a cemented carbide cutting tool according to claim 4, characterized in that: The amount of the cemented carbide forming agent added is 100-110 ml per 1 kg of dry mixed material.

9. The method for preparing a cemented carbide cutting tool according to claim 4, characterized in that: The working condition parameters of the pressing include: the shrinkage coefficient of the pressed green sheet is 1.25-1.27, and the pressing method of the rod green sheet for the rotary milling cutter is: standard cutters use rod molding, small-size rods below ≤Φ6 use self-pressing, rods ≥100mm use extrusion, and rods with a diameter of ≥Φ16 use dry bag pressing; the working condition parameters of the sintering include: the sintering temperature is 1450-1500°C, and the time is 2-3 hours.

10. A cemented carbide cutting tool, characterized in that: The cemented carbide cutting tool is prepared by the preparation method of the cemented carbide cutting tool according to any one of claims 4 to 7.