Method for preparing MnTe-coated MnO catalyst

By synthesizing the MnTe@MnO catalyst in the dopamine hydrochloride system, the problems of insufficient activity and poor stability of the MnTe@MnO catalyst are solved, and efficient HER and OER catalytic activity and long cycle stability are achieved, which is suitable for energy conversion and catalytic technology.

CN118745579APending Publication Date: 2024-10-08CHINA FAW CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410732476.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing MnTe@MnO catalyst has limited applications in energy conversion and catalytic technologies. Due to its insufficient HER and OER catalytic activities and poor cycle stability, it is difficult to be widely used.

Method used

By synthesizing MnTe and MnOOH nanorods in a dopamine hydrochloride system, the MnTe@MnO catalyst is prepared with specific mass ratios and processing conditions, including synthesis reactions in an autoclave, with high HER and OER catalytic activity and long cycle stability. sexual catalyst.

Benefits of technology

The HER and OER catalytic activity of the MnTe@MnO catalyst is significantly improved, achieving long cycle stability and efficient catalytic performance. It is suitable for preparing electrocatalysts and is widely used in energy conversion and catalytic technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004880912870000011
    Figure HDA0004880912870000011
  • Figure HDA0004880912870000012
    Figure HDA0004880912870000012
  • Figure HDA0004880912870000013
    Figure HDA0004880912870000013
Patent Text Reader

Abstract

The invention belongs to the field of catalyst materials, and particularly relates to a method for preparing a MnTe-coated MnO catalyst. Comprising the following steps: carrying out first mixing treatment on MnTe and MnOOH nanorods in water to obtain a first mixture; performing second mixing treatment on the first mixture and dopamine hydrochloride to obtain a second mixture; and carrying out a synthesis reaction on the second mixture in a high-pressure kettle to obtain the MnTe-coated MnO catalyst. According to the MnTe-coated MnO catalyst prepared by the method, the HER catalytic activity is remarkably improved, the OER catalytic activity is excellent, and the MnTe-coated MnO catalyst can be used for preparing an electrocatalyst, has long cycle stability and efficient catalytic activity, and can be widely applied to energy conversion and catalysis technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst materials and relates to a method for preparing a MnTe@MnO catalyst. Background Art

[0002] With the development of industry, energy and environmental issues are becoming increasingly prominent, and it is urgent to develop and utilize sustainable clean energy to replace modern fossil energy. Compared with the technical solution of using fossil fuels to produce hydrogen, electrolyte water technology has many advantages such as wide source of raw materials, high purity of hydrogen production, strong operability, no greenhouse gas emissions and high efficiency, and is considered to be one of the most promising hydrogen production methods.

[0003] MnTe@MnO catalyst is a nanocomposite composed of manganese telluride (MnTe) and manganese oxide (MnO), which exhibits excellent electrocatalytic performance in oxygen evolution reaction (OER). MnTe@MnO nanocomposite exhibits efficient OER performance in 1.0M alkaline solution, and its OER performance is as high as 10mAcm -2 Only 208 mV overpotential is required at the current density, which is significantly better than the individual MnTe and MnO electrode materials. Therefore, the MnTe@MnO catalyst shows potential as an electrocatalyst due to its efficient OER performance and good stability in alkaline media, and is expected to be further studied and applied in energy conversion and catalytic technology.

[0004] In order to promote the further application of MnTe@MnO catalysts in energy conversion and catalytic technology, it is urgent to develop a preparation method for MnTe@MnO catalysts with excellent performance. Summary of the invention

[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention proposes a method for preparing a MnTe@MnO catalyst. The MnTe@MnO catalyst prepared by the method has significantly improved HER catalytic activity and excellent OER catalytic activity, can be used to prepare an electrocatalyst, has long cycle stability and high catalytic activity, and can be widely used in energy conversion and catalytic technology.

[0006] It should be stated that the present invention is completed based on the following work of the inventor:

[0007] In the process of developing a highly catalytically active MnTe@MnO catalyst, the inventors found that the HER catalytic activity of the MnTe@MnO catalyst synthesized by using MnTe as the tellurium source, MnOOH as the manganese source, and MnOOH nanorods as the MnOOH precursor, and MnOOH nanorods and MnTe in a dopamine hydrochloride system was significantly improved. Further experimental results show that the MnTe@MnO catalyst obtained using the above precursor and reaction system has excellent overall performance in HER catalytic activity and OER catalytic activity, and has the advantages of long cycle stability and high catalytic activity, and can be used to prepare electrocatalysts and is widely used in energy conversion and catalytic technology.

[0008] In the first aspect of the present invention, the present invention proposes a method for preparing a MnTe@MnO catalyst. According to an embodiment of the present invention, the method comprises: performing a first mixing treatment on MnTe and MnOOH nanorods in water to obtain a first mixture; performing a second mixing treatment on the first mixture and dopamine hydrochloride to obtain a second mixture; and performing a synthesis reaction on the second mixture in an autoclave to obtain the MnTe@MnO catalyst. The MnTe@MnO catalyst prepared by the method of the embodiment of the present invention has significantly improved HER catalytic activity and excellent OER catalytic activity, can be used to prepare electrocatalysts, has long cycle stability and high efficiency catalytic activity, and can be widely used in energy conversion and catalytic technology.

[0009] According to an embodiment of the present invention, the mass ratio of the MnTe and MnOOH nanorods is (1-10):40.

[0010] According to an embodiment of the present invention, the mass ratio of the MnTe and MnOOH nanorods is (1-5):20, preferably (1-3):20. The inventors have determined through a large number of experiments that within this preferred mass ratio range, the prepared MnTe@MnO catalyst has excellent HER catalytic activity and presents a uniform nanosheet structure. Thus, the overall catalytic activity is further improved.

[0011] Exemplarily, the mass ratio of the MnTe to MnOOH nanorods may be 1:20, 2:20, 3:20, 4:20, or 5:20.

[0012] According to an embodiment of the present invention, the mass ratio of the MnOOH nanorods to dopamine hydrochloride is 4: (1-4), preferably 4: 1. The inventors have determined through a large number of experiments that within this mass ratio range, the prepared MnTe@MnO catalyst has excellent overall catalytic activity.

[0013] Exemplarily, the mass ratio of the MnOOH nanorods to dopamine hydrochloride may be 4:1, 2:1, 4:3, or 1:1.

[0014] According to an embodiment of the present invention, the mass ratio of the MnOOH nanorods to water is 1: (400-600), preferably 1: (450-550), and more preferably 1: 500. This facilitates obtaining a uniformly dispersed mixture of MnTe and MnOOH nanorods, which facilitates the next step.

[0015] According to an embodiment of the present invention, the water is deionized water.

[0016] According to an embodiment of the present invention, the MnOOH nanorods are prepared by the following method: anhydrous ethanol and potassium permanganate are mixed, and a chemical reaction is carried out at 180-220°C for 8-10 hours to obtain a crude product of MnOOH nanorods; the crude product of MnOOH nanorods is washed and dried to obtain the MnOOH nanorods. The MnOOH nanorods prepared by the above method are used to prepare MnTe@MnO catalysts, which can further improve their catalytic activity.

[0017] According to an embodiment of the present invention, the washing reagent of the washing treatment includes deionized water and ethanol, and the washing treatment includes: washing the MnOOH crude product with the deionized water and ethanol. The deionized water washing removes the unreacted reagents, and the ethanol washing removes water and other water-insoluble reagents. As known to those skilled in the art, the washing treatment can be repeated multiple times to obtain a pure product.

[0018] According to an embodiment of the present invention, the temperature of the drying process is 60-100° C., preferably 70-90° C. Exemplarily, the temperature of the drying process may be 60° C., 70° C., 80° C., 90° C., or 100° C.

[0019] According to an embodiment of the present invention, the drying time is 8 to 12 hours, preferably 9 to 11 hours. Exemplarily, the drying time can be 8 hours, 9 hours, 10 hours, 11 hours, or 12 hours.

[0020] According to an embodiment of the present invention, the drying process is performed under vacuum conditions.

[0021] According to an embodiment of the present invention, the synthesis reaction is carried out under normal pressure.

[0022] According to an embodiment of the present invention, the temperature of the synthesis reaction is 100-140° C., preferably 110-130° C., and more preferably 120° C. Thus, the efficiency of the MnTe@MnO synthesis reaction is further improved.

[0023] Illustratively, the temperature of the synthesis reaction can be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C.

[0024] According to an embodiment of the present invention, the synthesis reaction time is 4 to 12 hours, preferably 4 to 6 hours. The inventors have determined through a large number of experiments that within this reaction time, the synthesis reaction of MnTe@MnO is complete.

[0025] Illustratively, the synthesis reaction time can be 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, or 12 h.

[0026] According to an embodiment of the present invention, the second mixing process comprises: adding the acid dopamine to the first mixture by stirring, ultrasonically dispersing for 0.5 to 2 hours, and then stirring for 8 to 12 hours to obtain the second mixture. Thus, uniformly dispersed reaction raw materials are obtained, which is conducive to the MnTe@MnO synthesis reaction. Exemplarily, the ultrasonic dispersion time can be 0.5 hours, 1 hour, 1.5 hours, or 2 hours.

[0027] Illustratively, the stirring time may be 8 h, 9 h, 10 h, 11 h, or 12 h.

[0028] In the second aspect of the present invention, the present invention proposes a method for preparing a MnTe@MnO catalyst. According to an embodiment of the present invention, the method comprises: performing a first mixing treatment on MnTe and MnOOH nanorods in deionized water to obtain a first mixture; wherein the mass ratio of the MnTe, MnOOH nanorods and deionized water is 1:20:500, and the MnOOH nanorods are prepared by the following method: mixing anhydrous ethanol and potassium permanganate, and performing a chemical reaction at 180-220°C for 8-10 hours to obtain a crude product of MnOOH nanorods; and mixing the crude product of MnOOH nanorods. , after washing with deionized water and ethanol, drying at 70-90°C and vacuum conditions for 9-11 hours to obtain the MnOOH nanorods; stirring dopamine hydrochloride to the first mixture, ultrasonically dispersing for 0.5-2 hours, and then stirring for 10 hours to obtain a second mixture; wherein the mass ratio of the MnOOH nanorods to dopamine hydrochloride is 4:1, and the second mixture is subjected to a synthesis reaction in an autoclave at normal pressure and 120°C for 6 hours to obtain the MnTe@MnO catalyst. Contrary to the inventor's expectation, the MnTe@MnO catalyst prepared by the method of the embodiment of the present invention has significantly improved HER catalytic activity and OER catalytic activity, has long cycle stability and high catalytic activity, can be used to prepare electrocatalysts, and is widely used in energy conversion and catalytic technology.

[0029] In the third aspect of the present invention, the present invention provides a MnTe@MnO catalyst. According to an embodiment of the present invention, the catalyst is prepared according to the above method.

[0030] Those skilled in the art will appreciate that the features and advantages described above for the method for preparing the MnTe@MnO catalyst are also applicable to the MnTe@MnO catalyst, and will not be described in detail herein.

[0031] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0033] Figure 1 is a SEM image of the MnTe@MnO catalyst in Example 1 of the present invention;

[0034] Figure 2 HER hydrogen evolution half-reaction polarization curve diagram of the MnTe@MnO catalyst in Examples 1 to 4 of the present invention;

[0035] Figure 3 This is a polarization curve diagram of the OER oxygen evolution half-reaction of the MnTe@MnO catalyst in Examples 1 to 4 of the present invention. DETAILED DESCRIPTION

[0036] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.

[0037] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0038] In this document, the terms “include” or “comprising” are open expressions, that is, including the contents specified in the present invention but not excluding other contents.

[0039] As used herein, the terms "optionally", "optional" or "optionally" generally mean that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.

[0040] In the text, the term “HER@10mAcm -2" is used to describe the rate of hydrogen evolution reaction (HER) on the electrode surface. In HER, up to 10 mA cm -2 The overpotential required for the current density to reach a certain value is an important parameter to measure the activity of HER catalysts.

[0041] In the text, the term “OER@50mA cm -2 " is a specific indicator used to describe the performance of the oxygen evolution reaction (OER). OER is the anodic reaction in the water splitting process, involving the extraction of oxygen atoms from water and the ultimate production of oxygen. This process is critical for the electrolysis of water to produce hydrogen and many energy conversion and storage systems (such as lithium-air batteries). In OER, reaching 50mA cm -2 The required overpotential (the portion of the voltage that exceeds the theoretical value) is an important indicator of the activity of OER catalysts.

[0042] In this text, the term "overpotential" is the additional voltage applied to the electrode to drive the electrochemical reaction under thermodynamically non-spontaneous conditions. A lower overpotential means that the catalyst is more efficient in lowering the energy barrier of the reaction, thereby achieving a higher current density at a lower voltage. Therefore, a lower overpotential means that the catalyst has a higher efficiency.

[0043] In an embodiment of the present invention, MnTe (MnTe precursor) was synthesized by the following method: (0.091 g) 0.02 M MnCl2 and (0.25 g) 0.02 M tellurium powder were dissolved in 50 mL of deionized water. The above solution was then mixed with 2.0 mL of hydrazine hydrate at ambient temperature for 2 h. Thereafter, the corresponding mixture was heated at 160 ° C for 24 h in a stainless steel autoclave to obtain a gray precipitate. The resulting gray precipitate was modified, collected and repeatedly centrifuged using deionized water and ethanol, and the product was dehydrated in an oven at 70 ° C the next day. The MnTe precipitate was extracted and stored for later use.

[0044] In an embodiment of the present invention, MnOOH nanorods (MnOOH precursor) were synthesized by the following method: 30 mL of dehydrated ethanol was added to 0.20 g of potassium permanganate to produce a uniform mixture while stirring. For this purpose, a stainless steel autoclave (40 mL) with a Teflon coating was used. The autoclave was heated at 200° C. for 9 hours in an oven. After cooling to room temperature, the produced material was repeatedly washed with deionized water and ethanol, and then vacuum dried at 80° C. for 10 hours to obtain MnOOH nanorods.

[0045] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.

[0046] Example 1

[0047] In this example, the MnTe@MnO nanocatalyst was prepared by the following method:

[0048] 4 mg MnTe and 80 mg prepared MnOOH nanorods were added to 40.0 mL deionized water, and 0.2 g dopamine hydrochloride was added while stirring. The mixture was then dispersed by ultrasound for 0.5 h, and then vigorously stirred for 10 h. The mixture was transferred to a Teflon-coated stainless steel autoclave and reacted at 120 ° C for 6 h. After cooling naturally to room temperature, the sample was centrifuged and then dried at 60 ° C.

[0049] The SEM image of the MnTe@MnO catalyst prepared in this example is shown in Figure 1 shown.

[0050] The results show that the MnTe@MnO catalyst has a uniform nanosheet structure.

[0051] Example 2

[0052] The difference between this embodiment and embodiment 1 is that the added amount of MnTe is 8 mg.

[0053] Example 3

[0054] The difference between this embodiment and embodiment 1 is that the added amount of MnTe is 12 mg.

[0055] Example 4

[0056] Compared with Example 1, this embodiment is different in that the mixture is dispersed by ultrasound for 0.5 h and then vigorously stirred for 8 h.

[0057] Example 5

[0058] Compared with Example 1, this embodiment is different in that the mixture is dispersed by ultrasound for 0.5 h and then vigorously stirred for 12 h.

[0059] Example 6

[0060] Compared with Example 1, this example is different in that the reaction time in the stainless steel autoclave is 4 hours.

[0061] Example 7

[0062] Compared with Example 1, this example is different in that the amount of MnTe added is 10 mg; and the holding time at 120° C. in the stainless steel autoclave is 10 h.

[0063] The catalysts prepared in Examples 1 to 7 were tested for producing hydrogen by electrolyzing water to test the long-cycle stability of the materials.

[0064] The test method is: at room temperature, using a saturated calomel electrode as a reference electrode, in 1M KOH solution, and the test time is 12 hours.

[0065] The test results are shown in Table 1.

[0066] Table 1: Long cycle stability test results of MnTe@MnO catalysts of Examples 1 to 7

[0067] Example <![CDATA[Overpotential mV (HER @ 10 mA cm -2 )]]> <![CDATA[Overpotential mV (OER @ 50 mA cm -2 )]]> Example 1 145 148 Example 2 188 343 Example 3 157 352 Example 4 159 366 Example 5 155 346 Example 6 145 374 Example 7 167 389

[0068] The above results show that: (1) the MnTe@MnO nanocomposite material disclosed in the prior art has a reference current density of 10 mA cm 2 When the overpotential is 208 mV, the current density of the MnTe@MnO catalyst of the present invention reaches 10 mA cm -2 The overpotential required can be as low as 145-188 mV. This result shows that the HER catalytic activity of the MnTe@MnO catalyst of the present invention is significantly improved. (2) Contrary to the inventors' expectations, the current density of the MnTe@MnO catalyst prepared in Example 1 of the present invention reaches 10 mA cm -2 The required overpotential is as low as 145mV and the current density reaches 50mAcm -2 The overpotential required is as low as 148 mV. The HER catalytic activity of the MnTe@MnO catalyst prepared in Example 1 of the present invention is significantly improved, and the OER catalytic activity is significantly improved.

[0069] The inventors further investigated the HER hydrogen evolution half-reaction polarization curve and the OER oxygen evolution half-reaction polarization curve of the MnTe@MnO catalysts prepared in Examples 1 to 4. The specific test methods and results are as follows:

[0070] HER hydrogen evolution half-reaction polarization test: At room temperature, a saturated calomel electrode was used as a reference electrode, and the MnTe@MnO catalysts prepared in Examples 1 to 4 were subjected to a HER hydrogen evolution half-reaction polarization test in 1M KOH solution.

[0071] OER oxygen evolution half-reaction polarization test: Using a saturated calomel electrode as a reference electrode, the MnTe@MnO catalysts prepared in Examples 1 to 4 were subjected to an OER oxygen evolution half-reaction polarization test in 1 M KOH solution.

[0072] The results of the HER hydrogen evolution half-reaction polarization test are as follows: Figure 2 shown.

[0073] The results of the polarization test of the OER oxygen evolution half-reaction are as follows Figure 3 shown.

[0074] The results show that: (1) the MnTe@MnO catalyst of Example 1 has a vertical axis of 10 mA / cm -2 The absolute value of the horizontal axis is the smallest. (2) The MnTe@MnO catalyst of Example 1 has a vertical axis of 50 mA / cm -2 The absolute value of the horizontal axis is the smallest.

[0075] The above test results further verified and confirmed that the HER catalytic activity and OER catalytic activity of the MnTe@MnO catalyst prepared by the method of Example 1 were significantly improved, and it had long cycle stability and high catalytic activity.

[0076] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a MnTe@MnO catalyst, characterized in that: include: Performing a first mixing process on MnTe and MnOOH nanorods in water to obtain a first mixture; Performing a second mixing process on the first mixture and dopamine hydrochloride to obtain a second mixture; The second mixture is subjected to a synthesis reaction in an autoclave to obtain the MnTe@MnO catalyst.

2. The method according to claim 1, characterized in that The mass ratio of the MnTe and MnOOH nanorods is (1-10):40; Optionally, the mass ratio of the MnTe to MnOOH nanorods is (1-5):20, preferably (1-3):

20.

3. The method according to any one of claims 1 or 2, characterized in that: The mass ratio of the MnOOH nanorods to dopamine hydrochloride is 4:(1-4), preferably 4:

1.

4. The method according to any one of claims 1 to 3, characterized in that: The mass ratio of the MnOOH nanorods to water is 1:(400-600), preferably 1:(450-550), and more preferably 1:

500.

5. The method according to claim 1, characterized in that The water is deionized water.

6. The method according to claim 1, characterized in that The MnOOH nanorods are prepared by the following method: After mixing anhydrous ethanol and potassium permanganate, a chemical reaction is carried out at 180-220° C. for 8-10 hours to obtain a crude product of MnOOH nanorods; The MnOOH nanorods are obtained by washing and drying the crude MnOOH nanorods; Optionally, the washing reagent of the washing treatment includes deionized water and ethanol, and the washing treatment includes: washing the MnOOH crude product with the deionized water and ethanol; Optionally, the drying temperature is 60 to 100°C, preferably 70 to 90°C; Optionally, the drying time is 8 to 12 hours, preferably 9 to 11 hours; Optionally, the drying process is performed under vacuum conditions.

7. The method according to claim 1, characterized in that The synthesis reaction is carried out under normal pressure; Optionally, the temperature of the synthesis reaction is 100 to 140°C, preferably 110 to 130°C, more preferably 120°C; Optionally, the synthesis reaction time is 4 to 12 hours, preferably 4 to 6 hours.

8. The method according to claim 1, characterized in that The second mixing process comprises: The acid dopamine is added to the first mixture with stirring, ultrasonically dispersed for 0.5 to 2 hours, and then stirred for 8 to 12 hours to obtain the second mixture.

9. A method for preparing a MnTe@MnO catalyst, characterized in that: include: The MnTe and MnOOH nanorods are first mixed in deionized water to obtain a first mixture; wherein the mass ratio of the MnTe, MnOOH nanorods and deionized water is 1:20:500, and the MnOOH nanorods are prepared by the following method: anhydrous ethanol and potassium permanganate are mixed, and chemically reacted at 180-220° C. for 8-10 hours to obtain a crude product of MnOOH nanorods; the crude product of MnOOH nanorods is washed with deionized water and ethanol, and then dried at 70-90° C. under vacuum conditions for 9-11 hours to obtain the MnOOH nanorods; Dopamine hydrochloride is added to the first mixture with stirring, ultrasonically dispersed for 0.5 to 2 hours, and then stirred for 10 hours to obtain a second mixture; wherein the mass ratio of the MnOOH nanorods to dopamine hydrochloride is 4:1, The second mixture was subjected to a synthesis reaction in an autoclave at normal pressure and 120° C. for 6 hours to obtain the MnTe@MnO catalyst.

10. A MnTe@MnO catalyst, characterized in that: The catalyst is prepared according to the method according to any one of claims 1 to 8 or the method according to claim 9.

Citation Information

Cited By

  • Cobalt-doped NiS-coated MoS2 catalyst and preparation method and application thereof

    CN117512665A