Preparation method of bonding type three-wavelength fluorescent anti-counterfeiting polymer fiber

By preparing bonded three-wavelength fluorescent anti-counterfeiting polymer fibers, we solve the anti-counterfeiting performance and anti-aggregation problems of existing fluorescent anti-counterfeiting fibers, achieve efficient three-color fluorescence effects, expand the scope of anti-counterfeiting applications and improve the performance of the fibers.

CN118745601APending Publication Date: 2024-10-08TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411089146.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing fluorescent anti-counterfeiting fibers have deficiencies in anti-counterfeiting performance and anti-aggregation, making it difficult to effectively deal with the circulation of counterfeit and shoddy products in the market.

Method used

Adopting the preparation method of bonded three-wavelength fluorescent anti-counterfeiting polymer fiber, by preparing reactive europium, terbium, and zinc complexes, and using free radical polymerization technology to copolymerize with methyl methacrylate to form three-color phosphor, and then through electrostatic Spinning technology is used to prepare fibers to achieve three-wavelength fluorescence effects.

Benefits of technology

It improves the anti-counterfeiting performance and anti-aggregation performance of the anti-counterfeiting fiber, and expands the scope of anti-counterfeiting applications. The fiber diameter is at the nanometer level, has excellent luminescence properties and fiber-forming properties, and can present bright green, orange-red, and blue under different wavelengths of light. Enhanced recognition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745601A_ABST
    Figure CN118745601A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a bonding type three-wavelength fluorescent anti-counterfeiting polymer fiber, and relates to the technical field of fluorescent anti-counterfeiting fibers. The method comprises the following steps: S1, preparing a reaction type europium complex, a reaction type terbium complex and a reaction type zinc complex; s2, preparing bonding type polymer fluorescent powder PMEuTbZn; and S3, preparing a fluorescent fiber FPMEuTbZn, namely the bonding type three-wavelength fluorescent anti-counterfeiting polymer fiber. According to the preparation method, the reaction process is simple, the problem of concentration quenching is effectively solved, finally, the application range of the anti-counterfeiting fiber is expanded to three-color rare earth polymer anti-counterfeiting, and the anti-counterfeiting performance is improved. The diameter of the three-wavelength fluorescent anti-counterfeiting polymer fiber prepared by the method disclosed by the invention is at a nanometer level, and the three-wavelength fluorescent anti-counterfeiting polymer fiber has excellent luminescence property and fiber forming property, and is bright green under the illumination of 254 nm, orange red under the illumination of 365 nm and blue under the illumination of 395 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorescent anti-counterfeiting fibers, in particular to a method for preparing a bonded three-wavelength fluorescent anti-counterfeiting polymer fiber. Background Art

[0002] As an anti-counterfeiting technology, anti-counterfeiting fiber can improve the advancement and effectiveness of anti-counterfeiting means and cope with the evolving counterfeiting technology. Rare earth inorganic / organic polymers have become a research hotspot for anti-counterfeiting fibers because they have both the excellent luminescence properties of rare earth complexes and the excellent fiber-forming properties of polymer matrices. However, due to problems such as low anti-counterfeiting performance and concentration quenching, their application in the field of anti-counterfeiting fibers is greatly limited. The method to enhance its anti-counterfeiting performance generally involves studying multi-wavelength anti-counterfeiting fibers. For example: Xu Yuanyuan et al. successfully prepared dual-wavelength fluorescent anti-counterfeiting fibers by melt spinning. The fibers can emit red fluorescence under the excitation of 254 nm ultraviolet light and green fluorescence under the excitation of 980 nm infrared light, with dual anti-counterfeiting effects. With the increase of the content of fluorescent powder, the fluorescence intensity of the dual-wavelength fluorescent anti-counterfeiting fiber continues to increase, but the agglomeration of the fluorescent powder is aggravated. Huang Suping et al. first modified polypropylene, then blended 7% dual-wavelength fluorescent compounds with modified polypropylene to obtain fluorescent polypropylene particles, and then melt-spun the fluorescent polypropylene to obtain dual-wavelength fluorescent fibers. Although these methods have improved the anti-counterfeiting performance of fluorescent fibers to a certain extent, they are still easy to be copied and prone to agglomeration, and cannot solve the problem of the circulation of counterfeit and shoddy products in the market. Summary of the invention

[0003] The purpose of the present invention is to improve the anti-counterfeiting level of fluorescent fibers and solve technical problems such as concentration quenching and agglomeration of fluorescent powders, and to provide a method for preparing a bonded three-wavelength fluorescent anti-counterfeiting polymer fiber.

[0004] The present invention is achieved by the following steps: A method for preparing a bonded three-wavelength fluorescent anti-counterfeiting polymer fiber comprises the following steps: S1. Preparation of reactive europium complexes, reactive terbium complexes, and reactive zinc complexes 1) Synthesis of reactive europium complexes: a. Weigh 10-undecenoic acid and o-phenanthroline, dissolve them in anhydrous ethanol solution in a three-necked flask, and fix it in a magnetic stirring constant temperature water bath.

[0005] b. Weigh EuCl 3 and α-thenoyltrifluoroacetone (TTA) were placed in a beaker, anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0006] c. First, add EuCl dropwise into the three-necked flask.3 anhydrous ethanol solution, and the pH of the reaction system was adjusted with a NaOH solution, followed by reaction.

[0007] d. Add anhydrous ethanol solution containing α-thiophenecarbonyltrifluoroacetone (TTA) dropwise into the three-necked flask, adjust the pH value of the solution with NaOH solution, and a large amount of white precipitate is produced, and then continue to react.

[0008] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven to obtain the reactive europium complex, which is recorded as Eu(TTA) 2 (Phen)(UA).

[0009] 2) Synthesis of reactive terbium complexes a. Weigh 10-undecenoic acid, dissolve it in anhydrous ethanol solution in a three-necked flask, and fix it in a magnetic stirring constant temperature water bath.

[0010] b. Weigh TbCl 3 and 4-benzoylbenzoic acid (p-BBA) were placed in a beaker, anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0011] c. First, add TbCl dropwise into the three-necked flask. 3 anhydrous ethanol solution, and the pH value of the reaction system is adjusted with a NaOH solution, and then the reaction is allowed to proceed.

[0012] d. Add anhydrous ethanol solution containing 4-benzoylbenzoic acid dropwise into the three-necked flask, adjust the pH value of the solution with NaOH solution, and a large amount of white precipitate is produced, and then continue to react.

[0013] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven to obtain the reactive terbium complex, which is recorded as Tb(p-BBA) 3 (UA).

[0014] 3) Synthesis of reactive zinc complexes a. Weigh 10-undecenoic acid, dissolve it in anhydrous methanol solution in a three-necked flask, and fix it in a magnetic stirring constant temperature water bath.

[0015] b. Weigh ZnCl 2 and 2-(2-hydroxyphenyl)benzothiazole (BTZ) were placed in a beaker, anhydrous methanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0016] c. First, add ZnCl dropwise into the three-necked flask.2 anhydrous methanol solution, and the pH value of the reaction system was adjusted with a NaOH solution, and then the reaction was allowed to proceed.

[0017] d. Add anhydrous methanol solution containing 2-(2-hydroxyphenyl)benzothiazole dropwise into the three-necked flask, adjust the pH value of the solution with NaOH solution, and a large amount of white precipitate is produced, and then continue to react.

[0018] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous methanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven to obtain the reactive zinc complex, which is recorded as Zn(BTZ)(UA).

[0019] S2. Preparation of bonded polymer phosphor PMEuTbZn 1) Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 (UA), Zn(BTZ)(UA) are placed in a beaker, and then methyl methacrylate (MMA) and azobisisobutyronitrile (AIBN) are weighed in the beaker, and then dimethyl sulfoxide (DMSO) solution is added, and ultrasonic vibration is performed until it is completely dissolved and then placed in a test tube with a support. The beaker is then rinsed with dimethyl sulfoxide (DMSO) solution and placed in a test tube. Nitrogen is introduced to deoxygenate, and the system is placed in a constant temperature water bath. Nitrogen is continued to be introduced. When the system becomes viscous, the introduction of nitrogen is stopped, and then the reaction is continued in a closed system.

[0020] 2) The product obtained by the reaction is poured into an anhydrous methanol solution to produce a white precipitate; the product is washed alternately with a dimethyl sulfoxide (DMSO) solution and an anhydrous methanol solution for 3 times to remove unreacted monomers and impurities in the product, and then vacuum dried to obtain the bonded polymer phosphor PMEuTbZn.

[0021] S3. Preparation of fluorescent fiber FPMEUuTbZn 1) Weigh the bonded polymer phosphor PMEuTbZn in a beaker and prepare a spinning solution using N,N-dimethylformamide (DMF) as solvent.

[0022] 2) The prepared spinning solution is sucked into a pipette, a needle is installed at the front end of the pipette, the propulsion speed, voltage and receiving distance of the spinning machine are set, and the fiber is deposited on a grounded roller wrapped with tin foil in advance. After the spinning is completed, the tin foil sprayed with the fiber is removed and dried in an oven to obtain the fluorescent fiber FPMEUtbZn, which is the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber.

[0023] As the preferred technical solution: In step S1-1), 10-undecenoic acid, o-phenanthroline, EuCl3 , α-thiophenecarboxylic acid trifluoroacetone (TTA) in a molar ratio of 1:1:1:2; in step S1-1)-a, the ratio of 10-undecenoic acid to anhydrous ethanol solution is 0.5 mmol:10 mL, and the temperature of the magnetic stirring constant temperature water bath is 50°C; in step S1-1)-b, EuCl 3 The ratio of anhydrous ethanol solution is 0.5mmol:10 mL; in step S1-1)-c, the pH value is adjusted to 6~7 and the reaction is carried out for 30min; in step S1-1)-d, the pH value is adjusted to 6~7 and the reaction is continued for 4h; in step S1-1)-e, the temperature of the vacuum drying oven is 60℃ and the drying time is 5h.

[0024] In step S1-2), 10-undecenoic acid, TbCl 3 , 4-benzoylbenzoic acid (p-BBA) in a molar ratio of 1:1:3; in step S1-2)-a, the ratio of 10-undecenoic acid to anhydrous ethanol solution is 0.5 mmol:10 mL, and the temperature of the magnetic stirring constant temperature water bath is 50°C; in step S1-2)-b, TbCl 3 The ratio of anhydrous ethanol solution is 0.5 mmol:10 mL; in step S1-2)-c, the pH value is adjusted to 6~7 and the reaction is carried out for 30 minutes; in step S1-2)-d, the pH value is adjusted to 6~7 and the reaction is continued for 4 hours; in step S1-2)-e, the temperature of the vacuum drying oven is 60°C and the drying time is 5 hours.

[0025] In step S1-3), 10-undecenoic acid, ZnCl 2 , 2-(2-hydroxyphenyl)benzothiazole (BTZ) in a molar ratio of 1:1:1; in step S1-3)-a, the ratio of 10-undecenoic acid to dimethyl sulfoxide solution is 0.5 mmol:10 mL, and the temperature of the magnetic stirring constant temperature water bath is 50°C; in step S1-3)-b, ZnCl 2 The ratio of dimethyl sulfoxide solution is 0.5 mmol:10 mL; in step S1-3)-c, the pH value is adjusted to 6~7 and the reaction is carried out for 30 minutes; in step S1-3)-d, the pH value is adjusted to 6~7 and the reaction is continued for 4 hours; in step S1-3)-e, the temperature of the vacuum drying oven is 60°C and the drying time is 5 hours.

[0026] As the preferred technical solution: In step S2-1), Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3The total amount of (UA), Zn(BTZ)(UA), the amount of methyl methacrylate (MMA), the amount of azobisisobutyronitrile (AIBN), the amount of the first dimethyl sulfoxide (DMSO) solution, and the amount of the second dimethyl sulfoxide (DMSO) solution are in the ratio of 9 g:150 g:1 g:350 ml:150 ml; the ultrasonic oscillation time is 1 h; the time for the first nitrogen introduction is 30 min; the temperature of the constant temperature water bath is 75°C; the time for the second nitrogen introduction is 2 h; and the reaction time in the closed system is 24 h.

[0027] In step S2-2), the vacuum drying temperature is 60° C. and the time is 12 h.

[0028] As the preferred technical solution: In step S3-1), the concentration of the prepared spinning solution is 16%.

[0029] In step S3-2), the capacity of the pipette is 5 mL, the upper outer diameter of the needle is 0.82 mm, the propulsion speed of the spinning machine is 2 mL / h, the voltage is 18 kV, and the receiving distance is 20 cm; the drying temperature of the oven is 60 ° C and the drying time is 2 h.

[0030] As the preferred technical solution: In step S2-1), Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 The mass ratio of (UA) and Zn(BTZ)(UA) is 1:(2~4):1.

[0031] As the preferred technical solution: In step S2-1), Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 The mass ratio of (UA) and Zn(BTZ) (UA) is 1:3:1.

[0032] The preparation method of the invention adopts a technical route of first coordination and then polymerization, firstly preparing reactive red, green and blue light coordination monomers of europium, terbium and zinc with double bonds, then copolymerizing the reactive three-color coordination monomers with methyl methacrylate by free radical polymerization technology to prepare three-color polymethyl methacrylate-europium terbium zinc polymer fluorescent powder, and then spinning polymer fluorescent fibers by electrostatic spinning technology.

[0033] The preparation method of the present invention has a simple reaction process and effectively overcomes the concentration quenching problem, and finally expands the application scope of anti-counterfeiting fiber to three-color rare earth polymer anti-counterfeiting, thereby improving the anti-counterfeiting performance. The three-wavelength fluorescent anti-counterfeiting polymer fiber prepared by the method of the present invention has a diameter at the nanometer level and has excellent luminescence performance and fiber-forming performance. It exhibits bright green under 254 nm light, orange-red under 365 nm light, and blue under 395 nm light. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments of the present invention are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 Complex Eu(TTA) 2 (Phen)(UA), complex Tb(p-BBA) 3 Infrared spectra of (UA), complex Zn(BTZ)(UA), homopolymer PMMA, bonded polymer phosphor PMEuTbZn and its fluorescent fiber FPMEUTbZn.

[0036] Figure 2 Complex Eu(TTA) 2 (Phen)(UA), complex Tb(p-BBA) 3 Ultraviolet absorption spectra of (UA), complex Zn(BTZ)(UA), homopolymer PMMA, bonded polymer phosphor PMEuTbZn and its fluorescent fiber FPMEUTbZn.

[0037] Figure 3 The microstructure and elemental composition of fluorescent fiber FPMEUuTbZn.

[0038] Figure 4 Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 Fluorescence spectrum of bonded polymer phosphor PMEuTbZn when the mass ratio of Zn(UA) and Zn(BTZ)(UA) is 1:2:1.

[0039] Figure 5 Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3Fluorescence spectrum of bonded polymer phosphor PMEuTbZn when the mass ratio of Zn(UA) and Zn(BTZ)(UA) is 1:3:1.

[0040] Figure 6 Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 Fluorescence spectrum of bonded polymer phosphor PMEuTbZn when the mass ratio of Zn(UA) and Zn(BTZ)(UA) is 1:4:1.

[0041] Figure 7 These are actual photos of the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber (fluorescent fiber FPM EuTbZn) prepared by the present invention under natural light and ultraviolet light of different wavelengths. DETAILED DESCRIPTION

[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention. Example 1

[0043] This embodiment provides a method for preparing a bonded three-wavelength fluorescent anti-counterfeiting polymer fiber, comprising the following steps: S1. Preparation of reactive europium complexes, reactive terbium complexes, and reactive zinc complexes 1) Synthesis of reactive europium complexes: a. Weigh 0.5 mmol of 10-undecenoic acid and 0.5 mmol of o-phenanthroline, dissolve them in 10 mL of anhydrous ethanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0044] b. Weigh 0.5 mmol of EuCl 3 and 1 mmol of α-thenoyltrifluoroacetone (TTA) were placed in a beaker, 10 mL of anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0045] c. First, add EuCl dropwise into the three-necked flask. 3 anhydrous ethanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0046] d. Add the anhydrous ethanol solution containing α-thiopheneyltrifluoroacetone dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0047] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive europium complex, which is recorded as Eu(TTA) 2 (Phen)(UA).

[0048] 2) Synthesis of reactive terbium complexes a. Weigh 0.5 mmol of 10-undecenoic acid, dissolve it in 10 mL of anhydrous ethanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0049] b. Weigh 0.5 mmol of TbCl 3 and 1.5 mmol of 4-benzoylbenzoic acid (p-BBA) were placed in a beaker, 10 mL of anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0050] c. First, add TbCl dropwise into the three-necked flask. 3 anhydrous ethanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0051] d. Add the anhydrous ethanol solution containing 4-benzoylbenzoic acid dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0052] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive terbium complex, which is recorded as Tb(p-BBA) 3 (UA).

[0053] 3) Synthesis of reactive zinc complexes a. Weigh 0.5 mmol of 10-undecenoic acid, dissolve it in 10 mL of anhydrous methanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0054] b. Weigh 0.5 mmol of ZnCl 2 and 0.5 mmol of 2-(2-hydroxyphenyl)benzothiazole (BTZ) were placed in a beaker, 10 mL of anhydrous methanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0055] c. First, add ZnCl dropwise into the three-necked flask. 2 anhydrous methanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0056] d. Add the anhydrous methanol solution containing 2-(2-hydroxyphenyl)benzothiazole dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0057] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous methanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive zinc complex, which is recorded as Zn(BTZ)(UA).

[0058] S2. Preparation of bonded polymer phosphor PMEuTbZn 1) Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 (UA), Zn(BTZ)(UA) totaling 0.18 g was placed in a beaker, of which Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 The mass ratio of (UA) and Zn(BTZ)(UA) is 1:2:1; then weigh 3 g of methyl methacrylate (MMA) and 0.02 g of azobisisobutyronitrile (AIBN) into a beaker, and then add 7 mL of dimethyl sulfoxide (DMSO) solution, ultrasonically shake for 1 h until completely dissolved, and then place it in a test tube with a support. Then rinse the beaker with 3 mL of dimethyl sulfoxide (DMSO) solution and place it in a test tube. Deoxygenate with nitrogen for 30 min, place it in a constant temperature water bath at 75°C, continue to pass nitrogen for 2 h, stop passing nitrogen when the system becomes viscous, and then continue to react in a closed system for 24 h.

[0059] 2) The product obtained by the reaction was poured into an anhydrous methanol solution to produce a white precipitate; the product was washed alternately with a dimethyl sulfoxide (DMSO) solution and an anhydrous methanol solution for 3 times to remove unreacted monomers and impurities in the product, and then vacuum dried at 60° C. for 12 h to obtain the bonded polymer phosphor PMEuTbZn.

[0060] S3. Preparation of fluorescent fiber FPMEUTbZn 1) Weigh the bonded polymer phosphor PMEuTbZn in a beaker and prepare a spinning solution with a concentration of 16% using N,N-dimethylformamide (DMF) as solvent.

[0061] 2) The prepared spinning solution was sucked into a 5 mL pipette, a needle with an outer diameter of 0.82 mm was installed at the front end of the pipette, the propulsion speed of the spinning machine was set to 2 mL / h, the voltage was set to 18 kV, and the receiving distance was set to 20 cm, and the fiber was deposited on a grounded roller wrapped with tin foil in advance. After the spinning was completed, the tin foil sprayed with the fiber was removed and dried in an oven at 60 °C for 2 h to obtain the fluorescent fiber FPMEUtbZn, which is the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber. Example 2

[0062] This embodiment provides a method for preparing a bonded three-wavelength fluorescent anti-counterfeiting polymer fiber, comprising the following steps: S1. Preparation of reactive europium complexes, reactive terbium complexes, and reactive zinc complexes 1) Synthesis of reactive europium complexes: a. Weigh 0.5 mmol of 10-undecenoic acid and 0.5 mmol of o-phenanthroline, dissolve them in 10 mL of anhydrous ethanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0063] b. Weigh 0.5 mmol of EuCl 3 and 1 mmol of α-thenoyltrifluoroacetone (TTA) were placed in a beaker, 10 mL of anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0064] c. First, add EuCl dropwise into the three-necked flask. 3 anhydrous ethanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0065] d. Add the anhydrous ethanol solution containing α-thiopheneyltrifluoroacetone dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0066] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive europium complex, which is recorded as Eu(TTA) 2 (Phen)(UA).

[0067] 2) Synthesis of reactive terbium complexes a. Weigh 0.5 mmol of 10-undecenoic acid, dissolve it in 10 mL of anhydrous ethanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0068] b. Weigh 0.5 mmol of TbCl3 and 1.5 mmol of 4-benzoylbenzoic acid (p-BBA) were placed in a beaker, 10 mL of anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0069] c. First, add TbCl dropwise into the three-necked flask. 3 anhydrous ethanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0070] d. Add the anhydrous ethanol solution containing 4-benzoylbenzoic acid dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0071] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive terbium complex, which is recorded as Tb(p-BBA) 3 (UA).

[0072] 3) Synthesis of reactive zinc complexes a. Weigh 0.5 mmol of 10-undecenoic acid, dissolve it in 10 mL of anhydrous methanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0073] b. Weigh 0.5 mmol of ZnCl 2 and 0.5 mmol of 2-(2-hydroxyphenyl)benzothiazole (BTZ) were placed in a beaker, 10 mL of anhydrous methanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0074] c. First, add ZnCl dropwise into the three-necked flask. 2 anhydrous methanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0075] d. Add the anhydrous methanol solution containing 2-(2-hydroxyphenyl)benzothiazole dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0076] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous methanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive zinc complex, which is recorded as Zn(BTZ)(UA).

[0077] S2. Preparation of bonded polymer phosphor PMEuTbZn 1) Eu(TTA)2 (Phen)(UA), Tb(p-BBA) 3 (UA), Zn(BTZ)(UA) totaling 0.18 g was placed in a beaker, of which Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 The mass ratio of (UA) and Zn(BTZ)(UA) is 1:3:1; then weigh 3 g of methyl methacrylate (MMA) and 0.02 g of azobisisobutyronitrile (AIBN) into a beaker, and then add 7 mL of dimethyl sulfoxide (DMSO) solution, ultrasonically shake for 1 h until completely dissolved, and then place it in a test tube with a support. Then rinse the beaker with 3 mL of dimethyl sulfoxide (DMSO) solution and place it in a test tube. Deoxygenate with nitrogen for 30 min, place it in a constant temperature water bath at 75°C, continue to pass nitrogen for 2 h, stop passing nitrogen when the system becomes viscous, and then continue to react in a closed system for 24 h.

[0078] 2) The product obtained by the reaction was poured into an anhydrous methanol solution to produce a white precipitate; the product was washed alternately with a dimethyl sulfoxide (DMSO) solution and an anhydrous methanol solution for 3 times to remove unreacted monomers and impurities in the product, and then vacuum dried at 60° C. for 12 h to obtain the bonded polymer phosphor PMEuTbZn.

[0079] S3. Preparation of fluorescent fiber FPMEUuTbZn 1) Weigh the bonded polymer phosphor PMEuTbZn in a beaker and prepare a spinning solution with a concentration of 16% using N,N-dimethylformamide (DMF) as solvent.

[0080] 2) The prepared spinning solution was sucked into a 5 mL pipette, a needle with an outer diameter of 0.82 mm was installed at the front end of the pipette, the propulsion speed of the spinning machine was set to 2 mL / h, the voltage was set to 18 kV, and the receiving distance was set to 20 cm, and the fiber was deposited on a grounded roller wrapped with tin foil in advance. After the spinning was completed, the tin foil sprayed with the fiber was removed and dried in an oven at 60 °C for 2 h to obtain the fluorescent fiber FPMEUtbZn, which is the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber. Example 3

[0081] This embodiment provides a method for preparing a bonded three-wavelength fluorescent anti-counterfeiting polymer fiber, comprising the following steps: S1. Preparation of reactive europium complexes, reactive terbium complexes, and reactive zinc complexes 1) Synthesis of reactive europium complexes: a. Weigh 0.5 mmol of 10-undecenoic acid and 0.5 mmol of o-phenanthroline, dissolve them in 10 mL of anhydrous ethanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0082] b. Weigh 0.5 mmol of EuCl 3 and 1 mmol of α-thenoyltrifluoroacetone (TTA) were placed in a beaker, 10 mL of anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0083] c. First, add EuCl dropwise into the three-necked flask. 3 anhydrous ethanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0084] d. Add the anhydrous ethanol solution containing α-thiopheneyltrifluoroacetone dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0085] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive europium complex, which is recorded as Eu(TTA) 2 (Phen)(UA).

[0086] 2) Synthesis of reactive terbium complexes a. Weigh 0.5 mmol of 10-undecenoic acid, dissolve it in 10 mL of anhydrous ethanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0087] b. Weigh 0.5 mmol of TbCl 3 and 1.5 mmol of 4-benzoylbenzoic acid (p-BBA) were placed in a beaker, 10 mL of anhydrous ethanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0088] c. First, add TbCl dropwise into the three-necked flask. 3 anhydrous ethanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0089] d. Add the anhydrous ethanol solution containing 4-benzoylbenzoic acid dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0090] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive terbium complex, which is recorded as Tb(p-BBA) 3 (UA).

[0091] 3) Synthesis of reactive zinc complexes a. Weigh 0.5 mmol of 10-undecenoic acid, dissolve it in 10 mL of anhydrous methanol solution in a three-necked flask, and fix it in a 50℃ magnetic stirring constant temperature water bath.

[0092] b. Weigh 0.5 mmol of ZnCl 2 and 0.5 mmol of 2-(2-hydroxyphenyl)benzothiazole (BTZ) were placed in a beaker, 10 mL of anhydrous methanol solution was added to each, and ultrasonic vibration was performed until they were completely dissolved.

[0093] c. First, add ZnCl dropwise into the three-necked flask. 2 anhydrous methanol solution, adjust the pH value of the reaction system to 6-7 with NaOH solution, and react for 30 minutes.

[0094] d. Add the anhydrous methanol solution containing 2-(2-hydroxyphenyl)benzothiazole dropwise into the three-necked flask, adjust the pH value of the solution to 6-7 with NaOH solution, and a large amount of white precipitate is produced. Continue the reaction for 4 h.

[0095] e. After the reaction is completed, filter to obtain a white precipitate, wash it alternately with anhydrous methanol solution and distilled water for 5 to 6 times, and dry the white precipitate in a vacuum drying oven at 60°C for 5 h to obtain the reactive zinc complex, which is recorded as Zn(BTZ)(UA).

[0096] S2. Preparation of bonded polymer phosphor PMEuTbZn 1) Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 (UA), Zn(BTZ)(UA) totaling 0.18 g was placed in a beaker, of which Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3The mass ratio of (UA) and Zn(BTZ)(UA) is 1:4:1; then weigh 3 g of methyl methacrylate (MMA) and 0.02 g of azobisisobutyronitrile (AIBN) into a beaker, and then add 7 mL of dimethyl sulfoxide (DMSO) solution, ultrasonically shake for 1 h until completely dissolved, and then place it in a test tube with a support. Then rinse the beaker with 3 mL of dimethyl sulfoxide (DMSO) solution and place it in a test tube. Deoxygenate with nitrogen for 30 min, place it in a constant temperature water bath at 75°C, continue to pass nitrogen for 2 h, stop passing nitrogen when the system becomes viscous, and then continue to react in a closed system for 24 h.

[0097] 2) The product obtained by the reaction was poured into an anhydrous methanol solution to produce a white precipitate; the product was washed alternately with a dimethyl sulfoxide (DMSO) solution and an anhydrous ethanol solution for 3 times to remove unreacted monomers and impurities in the product, and then vacuum dried at 60° C. for 12 h to obtain the bonded polymer phosphor PMEuTbZn.

[0098] S3. Preparation of fluorescent fiber FPMEUuTbZn 1) Weigh the bonded polymer phosphor PMEuTbZn in a beaker and prepare a spinning solution with a concentration of 16% using N,N-dimethylformamide (DMF) as solvent.

[0099] 2) The prepared spinning solution was sucked into a 5 mL pipette, a needle with an outer diameter of 0.82 mm was installed at the front end of the pipette, the propulsion speed of the spinning machine was set to 2 mL / h, the voltage was set to 18 kV, and the receiving distance was set to 20 cm, and the fiber was deposited on a grounded roller wrapped with tin foil in advance. After the spinning was completed, the tin foil sprayed with the fiber was removed and dried in an oven at 60 °C for 2 h to obtain the fluorescent fiber FPMEUtbZn, which is the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber.

[0100] Figure 1 For the complex Eu(TTA) 2 (Phen)(UA), complex Tb(p-BBA) 3 Infrared spectra of (UA), complex Zn(BTZ)(UA), homopolymer PMMA, bonded polymer phosphor PMEuTbZn and its fluorescent fiber FPMEUTbZn. As can be seen from the figure, the complexes are successfully coordinated and the three complexes are successfully polymerized with the polymer monomer.

[0101] Figure 2 For the complex Eu(TTA) 2 (Phen)(UA), complex Tb(p-BBA) 3(UA), complex Zn(BTZ)(UA), homopolymer PMMA, bonded polymer phosphor PMEuTbZn and its fluorescent fiber FPMeuTbZn UV absorption spectra. As can be seen from the figure, the bonded polymer phosphor PMEuTbZn shows a double peak absorption between 225~275nm, which is obviously the superposition of the absorption peaks of the complex in this area, indicating that the UV absorption spectrum of the copolymer is the result of their joint action, and the complex monomer and the polymer monomer are successfully polymerized.

[0102] Figure 3 The microstructure and elemental composition of fluorescent fiber FPMEUuTbZn.

[0103] Figures 4 to 6 Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 The fluorescence spectra of the bonded polymer phosphor PMEuTbZn when the mass ratio of (UA) and Zn(BTZ)(UA) is 1:2:1, 1:3:1, and 1:4:1. As can be seen from the figure, regardless of the red, green, and blue complex Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 When the feed ratio of (UA) and Zn(BTZ)(UA) is what, the bonded polymer phosphor PMEuTbZn and its fluorescent fiber FPMeuTbZn both show the characteristic emission peaks of the three-color complex; among them, when the red, green and blue complex Eu(TTA) 2 (Phen)(UA), Tb(p-BBA) 3 When the feed ratio of Zn(UA) and Zn(BTZ)(UA) is 1:3:1, the phosphor exhibits yellow-green, red and blue light emissions when excited at wavelengths of 254nm, 365nm and 395nm, with high recognition.

[0104] Figure 7 The following are photos of the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber (fluorescent fiber FPMEUtbZn) prepared by the present invention under natural light and different wavelengths of ultraviolet light. It can be seen from the figure that the green, orange-red, and blue fibers have good shape clarity and clearly show the details of the anti-counterfeiting mark, indicating that the prepared fluorescent fiber FPMEUtbZn has potential application value in anti-counterfeiting.

[0105] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a bonded three-wavelength fluorescent anti-counterfeiting polymer fiber, characterized in that: The steps include: S1. Preparation of reactive europium complexes, reactive terbium complexes, and reactive zinc complexes 1) Synthesis of reactive europium complexes: a weigh 10-undecenoic acid, o-phenanthroline, dissolved in anhydrous ethanol solution placed in a three-necked flask, and fixed in a magnetic stirring constant temperature water bath; b. Weigh EuCl3 and α-thenoyltrifluoroacetone separately into a beaker, add anhydrous ethanol solution to each, and ultrasonically oscillate until completely dissolved; c. First, an anhydrous ethanol solution containing EuCl3 was added dropwise to a three-necked flask, and the pH of the reaction system was adjusted with a NaOH solution, and then allowed to react; d. Then, an anhydrous ethanol solution containing α-thenoyltrifluoroacetone was added dropwise to the three-necked flask, and the pH value of the solution was adjusted with a NaOH solution. A large amount of white precipitate was produced, and then the reaction was continued; e. After the reaction is completed, a white precipitate is obtained by filtration, and the precipitate is washed alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and the white precipitate is dried in a vacuum drying oven to obtain the reactive europium complex, denoted as Eu(TTA)2(Phen)(UA); 2) Synthesis of reactive terbium complexes a weigh 10-undecenoic acid, dissolved in anhydrous ethanol solution placed in a three-necked flask, and fixed in a magnetic stirring constant temperature water bath; b. Weigh TbCl3 and 4-benzoylbenzoic acid separately into a beaker, add anhydrous ethanol solution to each, and ultrasonically oscillate until completely dissolved; c. First, an anhydrous ethanol solution containing TbCl3 was added dropwise to a three-necked flask, and the pH value of the reaction system was adjusted with a NaOH solution, and then allowed to react; d. Then, an anhydrous ethanol solution containing 4-benzoylbenzoic acid was added dropwise to the three-necked flask, and the pH value of the solution was adjusted with a NaOH solution. A large amount of white precipitate was produced, and then the reaction was continued; e. After the reaction is completed, a white precipitate is obtained by filtration, and the precipitate is washed alternately with anhydrous ethanol solution and distilled water for 5 to 6 times, and the white precipitate is placed in a vacuum drying oven to dry to obtain the reactive terbium complex, referred to as Tb(p-BBA)3(UA); 3) Synthesis of reactive zinc complexes a. Weigh 10-undecenoic acid, dissolve it in anhydrous methanol solution in a three-necked flask, and fix it in a magnetic stirring constant temperature water bath; b. Weigh ZnCl2 and 2-(2-hydroxyphenyl)benzothiazole separately into a beaker, add anhydrous methanol solution to each, and ultrasonically oscillate until completely dissolved; c. First, an anhydrous methanol solution containing ZnCl2 was added dropwise to a three-necked flask, and the pH value of the reaction system was adjusted with a NaOH solution, and then allowed to react; d. Then, an anhydrous methanol solution containing 2-(2-hydroxyphenyl)benzothiazole was added dropwise to the three-necked flask, and the pH value of the solution was adjusted with a NaOH solution. A large amount of white precipitate was produced, and then the reaction was continued; e. After the reaction is completed, a white precipitate is obtained by filtration, and the precipitate is washed alternately with anhydrous methanol solution and distilled water for 5 to 6 times, and the white precipitate is dried in a vacuum drying oven to obtain the reactive zinc complex, which is referred to as Zn(BTZ)(UA); S2. Preparation of bonded polymer phosphor PMEuTbZn 1) Place Eu(TTA)2(Phen)(UA), Tb(p-BBA)3(UA), and Zn(BTZ)(UA) in a beaker, weigh methyl methacrylate and azobisisobutyronitrile in the beaker, add dimethyl sulfoxide solution, ultrasonically shake until completely dissolved, place in a test tube, rinse the beaker with dimethyl sulfoxide solution and place in the test tube, pass nitrogen to deoxygenate, place in a constant temperature water bath, continue to pass nitrogen, stop passing nitrogen when the system becomes viscous, and then continue to react in a closed system; 2) pouring the product obtained by the reaction into an anhydrous methanol solution to produce a white precipitate; washing it with a dimethyl sulfoxide solution and an anhydrous methanol solution alternately for 3 times to remove unreacted monomers and impurities in the product, and then vacuum drying to obtain the bonded polymer phosphor PMEuTbZn; S3. Preparation of fluorescent fiber FPMEUuTbZn 1) Weigh the bonded polymer phosphor PMEuTbZn in a beaker and prepare a spinning solution using N,N-dimethylformamide as solvent; 2) The prepared spinning solution is sucked into a pipette, a needle is installed at the front end of the pipette, the propulsion speed, voltage and receiving distance of the spinning machine are set, and the fiber is deposited on a grounded roller wrapped with tin foil in advance. After the spinning is completed, the tin foil sprayed with the fiber is removed and dried in an oven to obtain the fluorescent fiber FPMEUtbZn, which is the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber.

2. The method for preparing the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber according to claim 1, characterized in that: In step S1-1), the molar ratio of 10-undecenoic acid, o-phenanthroline, EuCl3, and α-thiophenoyltrifluoroacetone is 1:1:1:2; in step S1-1)-a, the ratio of 10-undecenoic acid to anhydrous ethanol solution is 0.5 mmol:10 mL, and the temperature of the magnetic stirring constant temperature water bath is 50°C; in step S1-1)-b, the ratio of EuCl3 to anhydrous ethanol solution is 0.5 mmol:10 mL; in step S1-1)-c, the pH value is adjusted to 6-7 and the reaction is continued for 30 minutes; in step S1-1)-d, the pH value is adjusted to 6-7 and the reaction is continued for 4 hours; in step S1-1)-e, the temperature of the vacuum drying oven is 60°C and the drying time is 5 hours; In step S1-2), the molar ratio of 10-undecenoic acid, TbCl3, and 4-benzoylbenzoic acid is 1:1:3; in step S1-2)-a, the ratio of 10-undecenoic acid to anhydrous ethanol solution is 0.5 mmol:10 mL, and the temperature of the magnetic stirring constant temperature water bath is 50°C; in step S1-2)-b, the ratio of TbCl3 to anhydrous ethanol solution is 0.5 mmol:10 mL; in step S1-2)-c, the pH value is adjusted to 6-7 and the reaction is continued for 30 minutes; in step S1-2)-d, the pH value is adjusted to 6-7 and the reaction is continued for 4 hours; in step S1-2)-e, the temperature of the vacuum drying oven is 60°C and the drying time is 5 hours; In step S1-3), the molar ratio of 10-undecenoic acid, ZnCl2, and 2-(2-hydroxyphenyl)benzothiazole is 1:1:1; in step S1-3)-a, the ratio of 10-undecenoic acid to anhydrous methanol solution is 0.5 mmol:10 mL, and the temperature of the magnetic stirring constant temperature water bath is 50°C; in step S1-3)-b, the ratio of ZnCl2 to anhydrous methanol solution is 0.5 mmol:10 mL; in step S1-3)-c, the pH value is adjusted to 6~7 and the reaction is carried out for 30 minutes; in step S1-3)-d, the pH value is adjusted to 6~7 and the reaction is continued for 4 hours; in step S1-3)-e, the temperature of the vacuum drying oven is 60°C and the drying time is 5 hours.

3. The method for preparing the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber according to claim 1, characterized in that: In step S2-1), the total amount of Eu(TTA)2(Phen)(UA), Tb(p-BBA)3(UA), Zn(BTZ)(UA), the amount of methyl methacrylate, the amount of azobisisobutyronitrile, the amount of the first dimethyl sulfoxide solution, and the amount of the second dimethyl sulfoxide solution are in the ratio of 9 g:150 g:1 g:350 mL:150 mL; the ultrasonic oscillation time is 1 h; the time for the first nitrogen introduction is 30 min; the temperature of the constant temperature water bath is 75°C; the time for the second nitrogen introduction is 2 h; and the reaction time in the closed system is continued for 24 h; In step S2-2), the vacuum drying temperature is 60° C. and the time is 12 h.

4. The method for preparing the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber according to claim 1, characterized in that: In step S3-1), the concentration of the prepared spinning solution is 16%; In step S3-2), the capacity of the pipette is 5 mL, the upper outer diameter of the needle is 0.82 mm, the propulsion speed of the spinning machine is 2 mL / h, the voltage is 18 kV, and the receiving distance is 20 cm; the drying temperature of the oven is 60 ° C, and the drying time is 2 h.

5. The method for preparing the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber according to claim 3, characterized in that: In step S2-1), the mass ratio of Eu(TTA)2(Phen)(UA), Tb(p-BBA)3(UA), and Zn(BTZ)(UA) is 1:(2~4):

1.

6. The method for preparing the bonded three-wavelength fluorescent anti-counterfeiting polymer fiber according to claim 5, characterized in that: In step S2-1), the mass ratio of Eu(TTA)2(Phen)(UA), Tb(p-BBA)3(UA), and Zn(BTZ)(UA) is 1:3:1.