Polyurethane fiber material as well as preparation method and application thereof
By using a combination of electrospinning and conductive carbon materials in the preparation of polyurethane fiber materials, a luffa-like network structure is formed, which solves the problems of sensor signal response lag and low sensitivity, and achieves polyurethane fiber materials with high sensitivity and stability. Improved sensor responsiveness and durability.
Patent Information
- Application Number
- CN202410919564.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The existing preparation methods of polyurethane fiber materials have problems such as delayed sensor signal response, low sensitivity and complicated preparation processes.
The polyurethane spinning solution is spun on the steel mesh receiving template using the electrospinning method to form a steel mesh structure, and a porogen is distributed on the fiber membrane. The spinning is repeated to form a luffa-like network structure, and then mixed with conductive carbon materials for adsorption. , remove the porogen and improve the sensitivity and stability of fiber materials.
By forming a multi-level luffa-like network structure, the effective contact area and conductive path of the fiber material are increased, the sensitivity and reliability of the sensor are improved, the sensor can respond quickly to smaller pressure changes, and its elasticity and durability are enhanced.
Smart Images

Figure CN118745604A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a polyurethane fiber material and a preparation method and application thereof. Background Art
[0002] With the continuous progress of materials science, the research and development of new composite materials has become a key factor in promoting technological innovation in many fields. Among them, network structure materials with bionic characteristics have attracted widespread attention due to their unique mechanical properties, excellent energy absorption capacity and good environmental adaptability. Multi-level fiber materials with loofah-like network structures, that is, complex fiber networks that imitate loofah vines in nature, are prepared by artificial synthesis methods.
[0003] However, the preparation methods in the related art have disadvantages such as delayed sensor signal response, low sensitivity, and complex preparation process.
[0004] Therefore, it is necessary to develop a new method for preparing polyurethane fiber material. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a method for preparing a polyurethane fiber material, which can effectively improve the sensitivity and stability of a sensor.
[0006] The second aspect of the present invention also provides a polyurethane fiber material.
[0007] The third aspect of the present invention also provides a flexible sensor.
[0008] According to a first aspect of the present invention, a method for preparing a polyurethane fiber material is provided, comprising the following steps:
[0009] S1, spinning the polyurethane spinning solution by electrostatic spinning, using a steel mesh as a receiving template, distributing a porogen on the surface of the polyurethane film formed by spinning during the spinning process, and then continuing to spin, and repeating the spinning process several times; thus obtaining an intermediate;
[0010] S2. Mix and adsorb the intermediate and the conductive carbon material solution under vacuum conditions to remove the porogen; the product is obtained.
[0011] The preparation method according to the embodiment of the present invention has at least the following beneficial effects:
[0012] The polyurethane fiber material prepared by the preparation method of the present invention has high sensitivity and stability. This is because a steel mesh receiving template is used to form a steel mesh structure on the fiber membrane, so that the fiber membrane has a micro-nano structure, which increases its effective contact area and improves its sensitivity. The micro-convex structure formed by the porogen is constructed on the steel mesh structure, so that the micro-nano structure on the fiber membrane is more abundant, and the formed loofah-like network structure has a larger effective contact area and more conductive paths, which can respond quickly to smaller pressure changes and has good elasticity, greatly improving its sensitivity.
[0013] Furthermore, its reliability is increased: the loofah-like network structure has a unique mesh structure, which is relatively dense and not easy to break when rubbed and stretched, so it can withstand larger deformation, thereby improving the reliability and durability of the sensor.
[0014] Furthermore, the combination of the steel mesh structure and the micro-convex structure on the electrospun fiber membrane forms a multi-level structure similar to a loofah network. The conductive network of this structure has richer levels and has a more sensitive and wide range of responses to different external stimuli, which can synergistically achieve high sensitivity and wide response.
[0015] According to some embodiments of the present invention, the mass concentration of the polyurethane spinning solution is 20% to 30%. Therefore, when the concentration of the polyurethane spinning solution is limited to the above range, it is conducive to the formation of long fibers.
[0016] According to some embodiments of the present invention, the polyurethane spinning solution is prepared by the following method:
[0017] The polyurethane particles are mixed with an organic solvent.
[0018] According to some embodiments of the present invention, the hardness of the polyurethane particles is 40 to 80 degrees. Thus, the rigidity and compressive stress of the prepared polyurethane fiber material are enhanced. The Shore hardness tester is used for testing.
[0019] According to some embodiments of the present invention, the mesh number of the steel mesh is 60 to 100 meshes. Thus, when the mesh number of the steel mesh is selected within the above range, it is conducive to the formation of a loofah-like network structure. Further, when the mesh number of the steel mesh is selected from 100 meshes, the sensitivity of the polyurethane fiber material can be provided.
[0020] According to some embodiments of the present invention, the mesh size of the porogen is 30 to 60. Therefore, when the mesh size of the porogen is selected within the above range, it is beneficial to form a micro-convex structure.
[0021] According to some embodiments of the present invention, the porogen is selected from at least one of sodium chloride particles, white sugar particles or monosodium glutamate particles.
[0022] According to some embodiments of the present invention, the mass concentration of the conductive carbon material solution is 0.01% to 0.05%.
[0023] According to some embodiments of the present invention, the conductive carbon material in the conductive carbon material solution is selected from at least one of carbon nanotubes, carbon black or graphene.
[0024] According to some embodiments of the present invention, the several times refers to greater than or equal to 1. Thus, the more times of repetition, the more layers of the loofah-like network structure formed, and the higher the sensitivity.
[0025] According to some embodiments of the present invention, the parameters of the electrospinning include: spinning voltage: 15-17KV, flow rate of 1-1.2mL / h; 100-120mm round-trip distance, winding speed of 100-120mm / s, collection speed of 100-120mm / s, receiving distance of 13-15cm, and ambient humidity of 45%-60%.
[0026] A polyurethane fiber material provided according to an embodiment of the second aspect of the present invention is prepared by the preparation method described in the first aspect of the present invention.
[0027] The third aspect of the present invention provides a flexible sensor, wherein the base material of the flexible sensor is selected from the polyurethane fiber material described in the second aspect of the present invention.
[0028] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0030] Figure 1 is a schematic diagram of the preparation process of an embodiment of the present invention;
[0031] Figure 2 It is the ultra-depth-of-field morphology image of the polyurethane fiber material prepared in Examples 1 to 3 of the present invention;
[0032] Figure 3 This is a sensitivity test diagram of the polyurethane fiber material prepared in Examples 1 to 3 of the present invention;
[0033] Figure 4 This is a finger bending test diagram of the polyurethane fiber material prepared in Example 1 of the present invention;
[0034] Figure 5 This is a wrist bending test diagram of the polyurethane fiber material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0036] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0037] Some of the raw materials of the present invention are as follows:
[0038] Preparation of polyurethane spinning solution: Use an electronic balance to weigh polyurethane particles with a hardness of 80 degrees, pour the weighed TPU particles into the organic solvent N,N-dimethylformamide (DMF) to prepare a solution with a TPU mass fraction of 25%, and then use a magnetic stirrer to fully stir it to obtain a spinning solution.
[0039] Porogenic agent: Use a grinder to grind the 60-mesh salt particles into fine salt particles for later use.
[0040] Preparation of conductive carbon material solution: Use 5% carbon nanotube dispersion from Suzhou Carbon Graphene Technology Co., Ltd. to prepare 500mL of 0.01% carbon nanotube dispersion. Use a 1L beaker to fill with deionized water, use a syringe to take out the dispersion and inject it into the deionized water to prepare 500mL of carbon nanotube dispersion diluted to 0.01%. Use ultrasonic equipment to ultrasonicate at 15 degrees Celsius for 10 minutes to make the carbon nanotube dispersion evenly dispersed.
[0041] Example 1
[0042] This example provides a method for preparing a polyurethane fiber material, and its flow diagram is as follows Figure 1 As shown, the following steps are included:
[0043] S1. Use an electrospinning machine for spinning. Add the prepared polyurethane spinning solution into a 10mL plastic syringe with a spinneret. Use conductive copper foil tape to make it into a horn shape to control the spinning range. Use a 100-mesh steel mesh to stick on the silicone oil paper, and then stick the silicone oil paper on the roller as a receiving template for electrospinning. During the spinning process, sprinkle a layer of porogen (7-8g) evenly on the formed polyurethane film every hour, and spin for 5 hours. Spinning voltage: 15KV, 1mL / h extrusion volume, 100mm round-trip distance, winding speed 120mm / s, collection speed 120mm / s, receiving distance 15cm, 45% humidity spinning.
[0044] S2. Divide the prepared 500mL 0.01% carbon nanotube dispersion into two parts for vacuum filtration of samples; during the filtration process, divide 250mL of the dispersion into two parts (125mL) for filtration twice for one sample. After one filtration, wash with anhydrous ethanol and deionized water and dry; after two filtrations, wash with anhydrous ethanol and deionized water and dry.
[0045] Example 2
[0046] This example provides a method for preparing a polyurethane fiber material, comprising the following steps:
[0047] S1. Use an electrospinning machine for spinning. Add the prepared polyurethane spinning solution into a 10mL plastic syringe with a spinneret. Use conductive copper foil tape to make it into a horn shape to control the spinning range. Use a 100-mesh steel mesh to stick on the silicone oil paper, and then stick the silicone oil paper on the roller as a receiving template for electrospinning. During the spinning process, sprinkle a layer of porogen evenly on the formed polyurethane film every hour, and spin for 2 hours. Spinning voltage: 15KV, 1mL / h extrusion volume, 100mm round-trip distance, winding speed 120mm / s, collection speed 120mm / s, receiving distance 15cm, 45% humidity spinning.
[0048] S2. Divide the prepared 500mL 0.01% carbon nanotube dispersion into two parts for vacuum filtration of samples; during the filtration process, divide 250mL of the dispersion into two parts (125mL) for filtration twice for one sample. After one filtration, wash with anhydrous ethanol and deionized water and dry; after two filtrations, wash with anhydrous ethanol and deionized water and dry.
[0049] Example 3
[0050] This example provides a method for preparing a polyurethane fiber material, comprising the following steps:
[0051] S1. Use an electrospinning machine for spinning. Add the prepared polyurethane spinning solution into a 10mL plastic syringe with a spinneret. Use conductive copper foil tape to make it into a horn shape to control the spinning range. Use a 100-mesh steel mesh to stick on the silicone oil paper, and then stick the silicone oil paper on the roller as a receiving template for electrospinning. During the spinning process, sprinkle a layer of porogen evenly on the formed polyurethane film every hour, and spin for 3 hours. Spinning voltage: 15KV, 1mL / h extrusion volume, 100mm round-trip distance, winding speed 120mm / s, collection speed 120mm / s, receiving distance 15cm, 45% humidity spinning.
[0052] S2. Divide the prepared 500mL 0.01% carbon nanotube dispersion into two parts for sample vacuum filtration; during the filtration process, divide 250mL of the dispersion into two parts (125ml) for one sample to be filtered twice. After one filtration, wash with anhydrous ethanol and deionized water and dry; after two filtrations, wash with anhydrous ethanol and deionized water and dry.
[0053] Comparative Example
[0054] The comparative example provides a method for preparing a polyurethane fiber material, and the steps thereof are substantially the same as those of Example 1, except that, in the comparative example, no porogen is added.
[0055] Performance Testing
[0056] The polyurethane fiber materials prepared in Examples 1 to 3 of the present invention were subjected to ultra-depth morphological observation, and the results are as follows: Figure 2 As shown, Figure 2 a is the morphology diagram of Example 2, Figure 2 b is the morphology of Example 3, Figure 2 c is the morphology diagram of Example 1. It can be seen from the figure that as the number of repeated spinning processes increases, the micro-nano structure on the fiber membrane gradually tends to be complex.
[0057] Sensitivity test:
[0058] Use a flexibility tester to test the resistance change rate under different strains, and then use the calculation formula to calculate the sensitivity coefficient to obtain experimental data. The calculation formula is:
[0059] GF = (ΔR / R0) / ε;
[0060] R represents the change in the dynamic resistance of the test, in ohms (Ω); R0 is the initial resistance of the flexible sensor, also in ohms (Ω); ε represents the strain rate of the material.
[0061] Use a digital multimeter to test the initial resistance of the polyurethane fiber material.
[0062] Before doing the tensile test, the left end of the test end needs to be returned to the origin to avoid errors in the test tension distance. Select samples that have passed the static conductivity test, paste copper foil tape on both ends, and then press the copper foil tape with a copper sheet to make the test data more accurate. The copper sheet is clamped at both ends with a test fixture. Compared with copper wire, copper sheet is usually thicker than copper wire, so it has a larger conductive cross-sectional area, which can accommodate more electron flow, thereby improving the conductivity. In addition, the contact area of the copper sheet is relatively large, which can completely cover the copper foil sticker, making the internal structure uniform enough, making the electron flow smoother and the conductivity better. After fixing the sample, first stretch 1mm as the pre-stretch length, the purpose is to put the sample in a horizontal pre-stretch state to reduce the measurement error, set 3mm and 5mm as the measurement stretch distance, and set the number of stretches to 20 times to intuitively display the test results. The moving speed is set to 1mm / s. In order to facilitate unified data statistics, the subsequent samples are set according to the above standards through the electronic flexibility tester (the tensile strain rate is 15% and 25% respectively).
[0063] Test results: The corresponding sensitivity coefficient can be calculated according to the sensitivity calculation formula and the data measured by the flexibility tester. Using pure TPU fiber membrane as a blank control, the sensitivity coefficients are 3.54 and 3.05 at the tensile strain rate of 15% and 25%, respectively. The sensitivity coefficients of the comparative fiber membrane at the tensile strain rate of 15% and 25% are 5.84 and 6.02, respectively.
[0064] The sensitivity of the polyurethane fiber materials prepared in Examples 1 to 3 of the present invention is as follows: Figure 3 As shown, from Figure 3 It can be seen that the sensitivity of the polyurethane fiber material of Example 1 when the stretching rate is 15% and 25% is 11.71 and 11.24 respectively. The sensitivity of the polyurethane fiber material of Example 2 when the stretching rate is 15% and 25% is 7.36 and 6.18 respectively. The sensitivity of the polyurethane fiber material of Example 3 when the stretching rate is 15% and 25% is 7.14 and 6.72 respectively.
[0065] Therefore, from the above, it can be seen that the multi-level fiber structure of the loofah network formed by the polyurethane fiber material prepared by the present invention can greatly improve the sensitivity coefficient of the sensor.
[0066] Application Testing
[0067] 1. Finger bending test: The finger is straightened as the initial state, and the sensor prepared in Example 1 of the present invention with polyurethane fiber material as the sensing element is placed on the finger joint, and the two ends are fixed with copper foil tape to test the response of finger bending. During the test, the finger is bent to the maximum angle and finally returns to the initial state of the finger straight, and this cycle is repeated. The results are shown in the figure. Figure 4 As shown, from Figure 4It can be seen that during the finger bending test, the motion signal can have a good response pattern, the finger bending and finger extension movement states can be identified from the peaks and valleys, and the signal is relatively smooth and has good stability.
[0068] 2. Wrist bending test: Place the sensor with polyurethane fiber material as the sensing element prepared in Example 1 of the present invention on the wrist joint, fix both ends with copper foil tape, and test the response of wrist bending in the same way as above. The results are as follows: Figure 5 As shown, from Figure 5 It can be seen that the resistance change rate is significantly improved compared with the finger bending test, and has good stability and repeatability, indicating that the wrist bending action can more easily be received by the flexible sensor The resistance value change information.
[0069] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A method for preparing a polyurethane fiber material, characterized in that: The steps include: S1, spinning the polyurethane spinning solution by electrostatic spinning, using a steel mesh as a receiving template, distributing a porogen on the surface of the polyurethane film formed by spinning during the spinning process, and then continuing to spin, and repeating the spinning process several times; thus obtaining an intermediate; S2. Mix and adsorb the intermediate and the conductive carbon material solution under vacuum conditions to remove the porogen; the product is obtained.
2. The method for preparing the polyurethane fiber material according to claim 1, characterized in that: The mass concentration of the polyurethane spinning solution is 20% to 30%.
3. The method for preparing the polyurethane fiber material according to claim 1, characterized in that: The polyurethane spinning solution is prepared by the following method: The polyurethane particles are mixed with an organic solvent.
4. The method for preparing the polyurethane fiber material according to claim 3, characterized in that: The hardness of the polyurethane particles is 40 to 80 degrees.
5. The method for preparing the polyurethane fiber material according to claim 1, characterized in that: The mesh number of the steel wire mesh is 60 to 100 meshes.
6. The method for preparing the polyurethane fiber material according to claim 1, characterized in that: The mesh number of the porogen is 30 to 60 meshes.
7. The method for preparing the polyurethane fiber material according to claim 1, characterized in that: The mass concentration of the conductive carbon material solution is 0.01% to 0.05%.
8. The method for preparing the polyurethane fiber material according to claim 1, characterized in that: The conductive carbon material in the conductive carbon material solution is selected from at least one of carbon nanotubes, carbon black or graphene.
9. A polyurethane fiber material, characterized in that: The preparation method is described in any one of claims 1 to 8.
10. A flexible sensor, characterized in that: The base material of the flexible sensor is selected from the polyurethane fiber material according to claim 9.
Citation Information
Patent Citations
Preparation method of high-bonding type composite mortar material with waste rubber powder
CN108689624A
Electrospun fiber with three-dimensional structure and preparation method thereof
CN111893585A
Preparation method of polyurethane nanofiber membrane
CN115573096A
Polymer fibre web mfg. device and method
CN1435515A
Filament Bundle Type Nano Fiber and Manufacturing Method Thereof
US20080241538A1