Preparation method of flame-retardant antibacterial ecological fiber

High-performance flame-retardant and antibacterial Lyocell fiber is prepared through bio-based flame retardants such as pyridoxine phosphate ammonium salt and process steps, which solves the problem of insufficient flammability and antibacterial properties of Lyocell fiber and achieves its flame retardant performance. and significant improvements in antibacterial properties, improving safety and scope of application.

CN118745661APending Publication Date: 2024-10-08HEYE HEALTH TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411097379.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The flammability of Lyocell fiber leads to fire risks and affects the safety of human life and property, and it is difficult to effectively improve its flame retardant performance and antibacterial properties with existing technology.

Method used

Ammonium pyridoxine phosphate ester (ASPPEA) is used as a bio-based flame retardant, and a high-performance flame retardant and antibacterial product is prepared through a series of process steps including pretreatment, oxidation, flame retardant finishing, antibacterial modification and carboxymethylation. Lyocell fiber, including FR-Ag-O-Lyocell and FR-Ag-Cm-Cu-O-Lyocell.

Benefits of technology

Significantly improves the flame retardant performance and antibacterial durability of Lyocell fiber, reduces the release of flammable gases, enhances its thermal stability and carbon-forming properties during the combustion process, reduces the amount of residual carbon, and improves the adsorption capacity of copper ions , significantly improving the safety and application scope of the fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745661A_ABST
    Figure CN118745661A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a flame-retardant antibacterial ecological fiber, which comprises the following steps: preparation of pyridoxine ammonium phosphate (ASPPEA), pretreatment of a Lyocell fiber, preparation of an oxidized Lyocell fiber, preparation of a flame-retardant Lyocell fiber (FR-O-Lyocell), preparation of a flame-retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell), preparation of a carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell), and preparation of a flame-retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell). According to the invention, a novel bio-based flame retardant ASPPE is creatively compounded with a plurality of materials such as O, AG, Cm, Cu and the like and Lyocell fibers, so that the material is endowed with durable, flame-retardant and ecological antibacterial effects; in the preparation process, a padding curing method, a chemical grafting method, an oxidation method and a dry spraying wet method are creatively used for preparing the material, and the material has the outstanding characteristics of being green, non-toxic, naturally degradable, soft in hand feeling, high in flame retardance, excellent in thermal stability and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing flame-retardant and antibacterial ecological fiber, and belongs to the technical field of new materials. Background Art

[0002] As a new type of regenerated cellulose fiber, Lyocell fiber overcomes the disadvantage of viscose fiber causing ecological pollution during the production process. It has the advantages of being green, environmentally friendly, naturally degradable, biocompatible and wearable, and is known as the green fiber of the 21st century. Lyocell fiber is widely used in the textile industry due to its excellent mechanical properties, good drape, smooth feel and good hygroscopicity. In addition, Lyocell fiber has high dry strength and wet strength. Its dry strength is close to that of polyester fiber, which means that it is more able to withstand mechanical action and chemical treatment and has strong processing applicability; its wet modulus is very high, indicating that its dimensional stability is very good; due to its strong and stretching characteristics, it is also very suitable for blending with other fibers. The various excellent properties of Lyocell fiber have made it widely developed and used in various fields, such as clothing, non-woven fabrics, conveyor belts, industrial filter materials, and the medical field; however, Lyocell fiber is highly flammable and easy to cause fire, which brings great harm to human life and property safety. Therefore, it is of great significance to modify Lyocell fiber to improve its safety and expand its application range. Summary of the invention

[0003] In view of the above problems, the present invention provides a flame retardant and antibacterial ecological fiber.

[0004] The first technical purpose of the present invention is to provide an oxidative antibacterial Lyocell fiber with good thermal stability, high release of active oxygen and low release of combustible gas.

[0005] The second technical purpose of the present invention is to provide a method for preparing flame-retardant antibacterial Lyocell fiber II (FR-Ag-O-Lyocell) with good antibacterial durability, excellent flame retardant performance and high charring ability.

[0006] The third technical objective of the present invention is to provide a preparation process using the flame retardant and antibacterial Lyocell fiber three (FR-Ag-Cm-Cu-O-Lyocell).

[0007] The present invention provides a method for preparing a flame-retardant and antibacterial ecological fiber, comprising the following steps: characterized in that it includes the preparation of pyridoxine phosphate ammonium salt (ASPPEA), pretreatment of Lyocell fiber, preparation of oxidized Lyocell fiber, preparation of flame-retardant Lyocell fiber (FR-O-Lyocell), preparation of flame-retardant and antibacterial Lyocell fiber (FR-Ag-O-Lyocell), preparation of flame-retardant and antibacterial (FR-Ag-O-Lyocell) fiber, preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell), and preparation of flame-retardant and antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell).

[0008] Preferably, step (1) preparation of pyridoxine phosphate ammonium salt (ASPPEA) First, VB6 and phosphoric acid are added into a round-bottom flask equipped with a reflux condenser, and magnetic stirring is turned on to heat up to obtain a light yellow ester liquid. Then, a certain proportion of urea is added and distilled water is added to heat up to obtain a bright orange liquid. Secondly, the bright orange liquid is dropped into hot anhydrous ethanol to precipitate a white precipitate. Finally, a white solid is filtered to precipitate again, washed, and vacuum dried to a constant weight to obtain pyridoxine phosphate ammonium salt (ASPPEA). Preferably, step (2) pretreatment of antibacterial Lyocell fibers First, weigh N-methylmorpholine-N-oxide (NMMO) in a beaker, add deionized water, then add PG and HA, heat and stir until it becomes a clear and transparent yellow liquid, then weigh cellulose fiber and add it, heat and stir until it becomes a transparent yellow-brown viscous state, then add 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) and stir until the color of the spinning solution returns to its original state, finally, transfer the spinning solution into a syringe, extrude the spinning solution through a needle, coagulate and stretch, and wind to obtain antibacterial Lyocell fiber, and soak and dry naturally; Preferably, step (3) preparation of oxidative antibacterial Lyocell fiber First, prepare a buffer solution of disodium hydrogen phosphate and sodium dihydrogen phosphate, place the buffer solution and the antibacterial Lyocell fiber prepared in step (2) in a three-necked flask, add 2,2,6,6-tetramethylpiperidinium nitrogen oxide (TEMPO) and sodium chlorite (NaClO2), stir in a sealed manner, add sodium hypochlorite (NaClO), immediately stop the reaction, then add anhydrous ethanol to terminate the reaction, take out the fiber, wash with anhydrous ethanol, and finally obtain the oxidized antibacterial Lyocell fiber; Preferably, step (4) preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) First, the pyridoxine phosphate ammonium salt prepared in step (1) is added to ionized water, heated to dissolve, and dicyandiamide is added as a catalyst. After the solution is uniform and transparent, Lyocell fiber is added, taken out after a period of time, then baked and washed, and finally dried and weighed to obtain flame retardant antibacterial Lyocell fiber (FR-O-Lyocell); Preferably, step (5) preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell) First, the FR-O-Lyocell fiber prepared in step (4) is immersed in a silver nitrate solution, taken out and washed with deionized water, then immersed in a sodium borohydride solution for reduction, and finally washed with deionized water and dried to obtain a flame retardant and antibacterial Lyocell fiber (FR-Ag-O-Lyocell); Preferably, step (6) preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) The FR-Ag-O-Lyocell fiber prepared in step (5), sodium chloroacetate and ethanol aqueous solution are placed in a three-necked flask, heated in a water bath, then ethanol aqueous solution and sodium hydroxide are added, heated in a water bath, and finally washed with anhydrous ethanol to obtain carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell); Preferably, step (7) preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) is immersed in a copper sulfate solution, taken out and washed with deionization, then a sodium borohydride (NaBH4) solution is prepared, and the pH value is adjusted with sodium hydroxide (NaOH), immersed in reduction, and finally washed and dried at room temperature to obtain a flame retardant and antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell); The first technical purpose of the present invention is achieved through the following technical solutions: Preferably, step (1) preparation of pyridoxine phosphate ammonium salt (ASPPEA) 1-6g of VB6 and 3-10g of phosphoric acid are added to a round-bottom flask equipped with a reflux condenser, magnetic stirring is turned on, the temperature is raised to 100-150°C, and the temperature is maintained for reaction for 1-5h to finally obtain a light yellow ester liquid, and then 10-20g of urea is added to the above liquid, and then 100-200mL of distilled water is added, and the temperature is maintained at 100-150°C for reaction for 1-5h, and then the system is heated to 100-150°C for reaction for 1-5h, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid is obtained by suction filtration. The white solid is dissolved in 100-200mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid is the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA).

[0009] The invention has the advantages of utilizing the structural characteristics of pyridoxine to modify it, synthesizing a novel bio-based flame retardant ASPPEA, and applying it to lyocell fibers to give the lyocell fibers a durable flame retardant effect.

[0010] Preferably, step (2) pretreatment of antibacterial Lyocell fibers Weigh 10-20mL NMMO in a beaker, add deionized water to make its water content 10-15%, then add 1-5% PG and 1-5% HA of the total solution, place in a 50-100℃ water bath and heat with stirring, add the prepared NMMO aqueous solution into a round-bottom flask while hot, weigh cellulose fiber and add, heat in an oil bath at 100-150℃, put into a stirrer and stir (speed 100-500r / min), wait until the cellulose is completely dissolved, then add BTDA and continue stirring, transfer the prepared but not yet cooled spinning solution into a syringe, prepare it by dry-wet spray method, extrude the spinning solution through a needle, enter into a coagulation bath and coagulate and stretch, wind it by a winder to obtain antibacterial Lyocell fiber, soak it in water for 24-48 hours and then dry it naturally.

[0011] The invention has the advantages that the NMMO aqueous solution is non-toxic and non-biogenic, and the Lyocell fiber prepared by dissolving cellulose in the NMMO aqueous solution has good performance. The fiber is prepared by esterification reaction between the hydroxyl group of cellulose and the carboxyl group of BTDA, and BTDA can release active oxygen under light conditions, thereby achieving an antibacterial effect.

[0012] Preferably, step (3) preparation of oxidative antibacterial Lyocell fiber First, prepare 0-5mL of disodium hydrogen phosphate and 50-100mL of sodium dihydrogen phosphate buffer, strictly control the pH to 6-7, place the buffer and 1-6g of the pretreated antibacterial Lyocell fiber obtained in step (2) in a three-necked flask, add 0.01-0.10g of TEMPO and 1.70-1.80g of NaClO2, stir in a closed manner at 50-100°C for 0-30min, then add 0-5g of NaClO, keep the reaction at 50-100°C for 6-12h; then add 0-20mL of anhydrous ethanol to terminate the reaction; wash the fiber with anhydrous ethanol for 1-6 times, and finally obtain O-Lyocell.

[0013] The advantage of the present invention is that the Lyocell fiber is oxidized by using the TEMPO / NaClO2 / NaClO oxidation system, the primary hydroxyl groups on the cellulose structural units are successfully oxidized into carboxyl groups, and the obtained oxidized fiber has good thermal stability and carbonization properties.

[0014] The second technical purpose of the present invention is achieved through the following technical solutions: Preferably, step (4) preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) The ASPPEA flame retardant prepared in step (1) is added to deionized water, heated at 50-100°C to completely dissolve it, and a flame retardant liquid with a concentration of 10-50wt% is prepared. Subsequently, dicyandiamide (about 5-10wt% of the flame retardant liquid) is added as a catalyst. After the solution is uniform and transparent, weighed lyocell fibers (ratio of 1:10-1:20) are added. After 1-5 hours, the Lyocell fibers are taken out and then placed in an oven at 150-200°C for baking for 1-10 minutes. The finished fibers are washed with deionized water to remove the flame retardant that has not participated in the reaction. Finally, they are dried at 50-100°C and weighed to obtain FR-O-Lyocell fibers.

[0015] The advantage of the present invention is that the flame retardant finishing of Lyocell fiber is carried out through the padding and baking process. During the finishing process, the ammonium phosphonate group will be decomposed into the phosphonic acid group, and react with the hydroxyl group on the Lyocell fiber under the catalytic action of dicyandiamide to form a covalent bond, thereby imparting good flame retardant properties.

[0016] Preferably, step (5) preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell) First, immerse the FR-O-Lyocell fiber prepared in step (4) in a 0.1-0.6 mol / L silver nitrate solution for 1-10 min, then wash off the excess silver nitrate solution with deionized water, and then immerse the fabric in a 0.01-0.10 mol / L sodium borohydride solution for reduction for 1-6 min. The color of the fabric gradually changes from light yellow to black. Finally, wash the modified fabric with deionized water and dry it at 50-100°C to obtain FR-Ag-O-Lyocell.

[0017] The invention has the advantages that the flame-retardant modified fiber is immersed in a silver nitrate solution, the phosphonic acid group in the flame retardant is used to adsorb silver ions on the surface of the fabric, nano silver is synthesized in situ, and the generation of metal oxides at high temperature can increase the carbon residue of the modified fabric. Since the carbon residue will be further oxidized and decomposed in an aerobic environment, the carbon residue of the fabric is significantly reduced compared with that in a nitrogen atmosphere, and a large amount of non-combustible gas is released during the combustion process, so the flame retardant effect is exerted in the gas phase.

[0018] The third technical objective of the present invention is achieved through the following technical solutions: Preferably, step (6) preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) 1-5 g of the FR-Ag-O-Lyocell fiber prepared in step (5), 1-5 g of sodium chloroacetate and a 50-100 wt% ethanol aqueous solution are placed in a three-necked flask, and heated in a water bath at 50-100° C. for 1-5 h to allow the fiber and the sodium chloroacetate to be fully mixed, and then 50-100 wt% ethanol aqueous solution and 1-5 g of sodium hydroxide are added thereto, and then the water bath temperature is raised to 50-100° C. and maintained for 1-5 h. Finally, the reacted fiber is washed 1-6 times with anhydrous ethanol until it is neutral to obtain FR-Ag-Cm-O-Lyocell.

[0019] The advantage of the present invention is that a highly graphitized carbon layer protective cover is generated on the surface of the carboxymethylated Lyocell fiber during combustion, which effectively interrupts the transfer of heat, mass and oxygen, and has a flame retardant effect in the condensed phase. The amount of residual carbon left by the flame retardant fiber is high, indicating that the flame retardant fiber has excellent thermal stability and carbon forming properties.

[0020] Preferably, step (7) preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) is immersed in a 0-1 mol / L copper sulfate solution for 5-15 minutes, and then the excess copper sulfate solution is washed off with deionized water. Then, a 0.01-0.10 mol / L NaBH4 solution is prepared, and the pH value of the solution is adjusted to 5-10 with NaOH. The fabric is then immersed in the solution for reduction for 1-6 minutes, and the color of the fiber gradually changes from light blue to copper brown. Finally, the fabric is washed in deionized water and dried at room temperature to obtain FR-Ag-Cm-Cu-O-Lyocell.

[0021] The advantages of the present invention are that covalent bonding with Lyocell fibers is achieved, flame retardancy and durability are improved, and the adsorption capacity of the fabric to copper ions is enhanced, thereby stabilizing more reduced nanoparticles on the fabric surface, so as to prepare Lyocell fibers with excellent flame retardancy and antibacterial properties.

[0022] In summary, the present invention has the following beneficial effects: 1. The present invention has the advantages of utilizing the structural characteristics of pyridoxine to modify it, synthesizing a new type of bio-based flame retardant ASPPEA, and applying it to lyocell fiber to give the lyocell fiber a durable flame retardant effect; 2. The advantages of the present invention are that the NMMO aqueous solution is non-toxic and non-biogenic, and the Lyocell fiber prepared by dissolving cellulose therein has good performance. It is prepared by esterification reaction between the hydroxyl group of cellulose and the carboxyl group of BTDA. BTDA can release active oxygen under light conditions, thereby playing an antibacterial effect; 3. The present invention has the advantage that the Lyocell fiber is oxidized by using the TEMPO / NaClO2 / NaClO oxidation system, and the primary hydroxyl groups on the cellulose structural units are successfully oxidized into carboxyl groups, and the oxidized fiber obtained has good thermal stability and carbonization properties; 4. The present invention has the advantage that the flame retardant finishing of Lyocell fiber is carried out by padding and baking process, during which the ammonium phosphonate groups are decomposed into phosphonic acid groups, and react with the hydroxyl groups on the Lyocell fiber under the catalytic action of dicyandiamide to form covalent bonds, thereby imparting good flame retardant properties; 5. The advantages of the present invention are that the flame-retardant modified fiber is immersed in a silver nitrate solution, the phosphonic acid group in the flame retardant is used to adsorb silver ions on the surface of the fabric, nanosilver is synthesized in situ, and the generation of metal oxides at high temperature can increase the carbon residue of the modified fabric. Since the carbon residue will be further oxidized and decomposed in an aerobic environment, the carbon residue of the fabric is significantly reduced compared with that in a nitrogen atmosphere, and a large amount of non-combustible gas is released during the combustion process, and the flame retardant effect is exerted in the gas phase; 6. The present invention has the advantage that a highly graphitized carbon layer protective cover is generated on the surface of the carboxymethylated Lyocell fiber during combustion, which effectively interrupts the transfer of heat, mass and oxygen, and has a flame retardant effect in the condensed phase. The amount of residual carbon left by the flame retardant fiber is high, indicating that the flame retardant fiber has excellent thermal stability and carbon forming properties; 7. The advantages of the present invention are that it can achieve covalent bonding with Lyocell fibers, improve flame retardancy and durability, and enhance the fabric's ability to adsorb copper ions, thereby allowing more reduced nanoparticles to be firmly attached to the fabric surface, in order to prepare Lyocell fibers with excellent flame retardancy and antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a flow chart of a method for preparing flame-retardant and antibacterial ecological fiber. DETAILED DESCRIPTION

[0024] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and substance of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.

[0025] If not specifically stated, the technical means used in the examples are conventional means known to those skilled in the art. In addition, all the raw materials used in the examples are known commercial products. Example 1

[0026] like Figure 1 As shown, a method for preparing a flame retardant and antibacterial ecological fiber comprises:

[0027] Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) 1g of VB6 and 3g of phosphoric acid were added to a round-bottom flask equipped with a reflux condenser, magnetic stirring was turned on, the temperature was raised to 130°C, and the temperature was maintained for 2h to finally obtain a light yellow ester liquid, and then 12g of urea was added to the above liquid, and then 100mL of distilled water was added, and the temperature was maintained at 110°C for 3h, and then the system was heated to 120°C for 2h, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid was obtained by suction filtration. The white solid was dissolved in 100mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid was the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA); Step (2) Pretreatment of antibacterial Lyocell fibers Weigh 15 mL of NMMO in a beaker, add deionized water to make its water content 13.3%, then add 1% of the total solution of PG and 1% of the total solution of HA, place in a 75°C water bath for heating and stirring, add the prepared NMMO aqueous solution to a round-bottom flask while hot, weigh cellulose fiber and add, heat in an oil bath at 105°C, put in a stirrer for stirring (speed 400r / min), wait until the cellulose is completely dissolved, then add BTDA and continue stirring, transfer the prepared but not yet cooled spinning solution into a syringe, prepare by dry-wet spray method, extrude the spinning solution through a needle, enter into a coagulation bath for coagulation and stretching, wind up by a winder to obtain antibacterial Lyocell fiber, soak in water for 24-48 hours and then dry naturally; Step (3) Preparation of oxidative antibacterial Lyocell fibers First, prepare 0.5 mL of disodium hydrogen phosphate and 90 mL of sodium dihydrogen phosphate buffer, strictly control the pH to 6.8, put the buffer and 1 g of the pretreated antibacterial Lyocell fiber obtained in step (2) into a three-necked flask, add 0.04 g of TEMPO and 1.73 g of NaClO2, stir at 60 ° C for 10 min, then add 1 g of NaClO, keep the reaction at 60 ° C for 12 h; then add 5 mL of anhydrous ethanol to terminate the reaction; wash the fiber with anhydrous ethanol for 6 times, and finally obtain O-Lyocell; Step (4) Preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) The ASPPEA flame retardant prepared in step (1) is added to deionized water, heated at 70°C to completely dissolve it, and a flame retardant liquid with a concentration of 30wt% is prepared. Subsequently, dicyandiamide (about 7wt% of the flame retardant liquid) is added as a catalyst. After the solution becomes uniform and transparent, weighed Lyocell fibers (at a ratio of 1:20) are added. After 2 hours, the Lyocell fibers are taken out and then placed in an oven at 200°C for 10 minutes. The finished fibers are washed with deionized water to remove the flame retardant that has not participated in the reaction. Finally, they are dried at 60°C and weighed to obtain FR-O-Lyocell fibers. Step (5) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell) First, the FR-O-Lyocell fiber prepared in step (4) is immersed in a 0.1 mol / L silver nitrate solution for 10 minutes, and then the excess silver nitrate solution is washed off with deionized water. Then, the fabric is immersed in a 0.03 mol / L sodium borohydride solution for reduction for 1 minute, and the color of the fabric gradually changes from light yellow to black. Finally, the modified fabric is washed with deionized water and then dried at 60°C to obtain FR-Ag-O-Lyocell. Step (6) Preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) 2 g of the FR-Ag-O-Lyocell fiber prepared in step (5), 2.5 g of sodium chloroacetate and 85 wt % ethanol aqueous solution were placed in a three-necked flask, and heated in a water bath at 60° C. for 2 h to allow the fiber and the sodium chloroacetate to be fully mixed, and then 85 wt % ethanol aqueous solution and 1.5 g of sodium hydroxide were added thereto, and then the water bath temperature was raised to 70° C. and maintained for 3 h. Finally, the reacted fiber was washed 1-6 times with anhydrous ethanol until it was neutral, to obtain FR-Ag-Cm-O-Lyocell; Step (7) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) was immersed in a 0.1 mol / L copper sulfate solution for 10 min, and then the excess copper sulfate solution was washed off with deionized water. Then, a 0.08 mol / L NaBH4 solution was prepared, and the pH value of the solution was adjusted to 10 with NaOH. The fabric was then immersed in this solution for reduction for 1 min, and the color of the fiber gradually changed from light blue to copper brown. Finally, the fabric was washed in deionized water and dried at room temperature to obtain FR-Ag-Cm-Cu-O-Lyocell. Example 2

[0028] Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) 2g of VB6 and 4g of phosphoric acid were added to a round-bottom flask equipped with a reflux condenser, magnetic stirring was turned on, the temperature was raised to 120°C, and the temperature was maintained for 1h to finally obtain a light yellow ester liquid, and then 11g of urea was added to the above liquid, and then 100mL of distilled water was added, and the temperature was maintained at 100°C for 2h, and then the system was heated to 110°C for 3h, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid was obtained by suction filtration. The white solid was dissolved in 110mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid was the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA); Step (2) Pretreatment of antibacterial Lyocell fibers Weigh 14 mL of NMMO in a beaker, add deionized water to make its water content 12%, then add 2% of the total solution of PG and 2% of the total solution of HA, place in a 70°C water bath for heating and stirring, add the prepared NMMO aqueous solution to a round-bottom flask while hot, weigh cellulose fiber and add, heat in an oil bath at 100°C, put in a stirrer for stirring (speed 450r / min), wait until the cellulose is completely dissolved, then add BTDA and continue stirring, transfer the prepared but not yet cooled spinning solution into a syringe, prepare by dry-wet spray method, extrude the spinning solution through a needle, enter into a coagulation bath for coagulation and stretching, wind up by a winder to obtain antibacterial Lyocell fiber, soak in water for 40 hours and then dry naturally; Step (3) Preparation of oxidative antibacterial Lyocell fibers First, prepare 1 mL of disodium hydrogen phosphate and 50 mL of sodium dihydrogen phosphate buffer, strictly control the pH to 6, place the buffer and 1.5 g of the pretreated antibacterial Lyocell fiber obtained in step (2) in a three-necked flask, add 0.03 g of TEMPO and 1.72 g of NaClO2, stir at 65 ° C for 17 min, then add 2 g of NaClO, keep the reaction at 65 ° C for 11 h, and then add 7 mL of anhydrous ethanol to terminate the reaction; wash the fiber with anhydrous ethanol 5 times, and finally obtain O-Lyocell; Step (4) Preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) Add the ASPPEA flame retardant prepared in step (1) to deionized water, heat it at 65°C to completely dissolve it, and prepare a flame retardant liquid with a concentration of 25wt%, then add dicyandiamide (about 6wt% of the flame retardant liquid) as a catalyst. After the solution is uniform and transparent, add weighed lyocell fiber (ratio of 1:15). After 3 hours, take out the Lyocell fiber, and then bake the fiber in a 165°C oven for 9 minutes. The finished fiber is washed with deionized water to remove the flame retardant that has not participated in the reaction, and finally dried at 65°C and weighed to obtain FR-O-Lyocell fiber; Step (5) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell) First, immerse the FR-O-Lyocell fiber prepared in step (4) in a 0.2 mol / L silver nitrate solution for 9 minutes, and then wash off the excess silver nitrate solution with deionized water. Then, immerse the fabric in a 0.02 mol / L sodium borohydride solution for 2 minutes, and the color of the fabric gradually changes from light yellow to black. Finally, wash the modified fabric with deionized water and dry it at 65°C to obtain FR-Ag-O-Lyocell; Step (6) Preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) 1 g of the FR-Ag-O-Lyocell fiber prepared in step (5), 2 g of sodium chloroacetate and 80 wt % ethanol aqueous solution were placed in a three-necked flask and heated in a water bath at 65 ° C for 1 h to fully mix the fiber and the sodium chloroacetate, and then 80 wt % ethanol aqueous solution and 2 g of sodium hydroxide were added thereto, and then the water bath temperature was raised to 75 ° C and maintained for 2 h. Finally, the reacted fiber was washed 5 times with anhydrous ethanol until it was neutral to obtain FR-Ag-Cm-O-Lyocell; Step (7) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) was soaked in a 0.2 mol / L copper sulfate solution for 11 minutes, and then the excess copper sulfate solution was washed off with deionized water. Then, a 0.07 mol / L NaBH4 solution was prepared, and the pH value of the solution was adjusted to 9 with NaOH. The fabric was then immersed in this solution for 2 minutes for reduction, and the color of the fiber gradually changed from light blue to copper brown. Finally, the fabric was washed in deionized water and dried at room temperature to obtain FR-Ag-Cm-Cu-O-Lyocell. Example 3

[0029] Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) 3 g of VB6 and 6 g of phosphoric acid were added to a round-bottom flask equipped with a reflux condenser, magnetic stirring was turned on, the temperature was raised to 120°C, and the temperature was maintained for 3 hours to finally obtain a light yellow ester liquid, and then 19 g of urea was added to the above liquid, and then 110 mL of distilled water was added, and the temperature was maintained at 115°C for 2.5 hours, and then the system was heated to 125°C for 2.5 hours, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid was obtained by suction filtration. The white solid was dissolved in 110 mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid was the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA); Step (2) Pretreatment of antibacterial Lyocell fibers Weigh 17mL NMMO in a beaker, add deionized water to make its water content 13.5%, then add 2% PG and 3% HA, heat and stir in a water bath at 80°C, add the prepared NMMO aqueous solution to a round-bottom flask while hot, weigh cellulose fiber and add, heat in an oil bath at 110°C, put in a stirrer and stir (speed 480r / min), wait until the cellulose is completely dissolved, then add BTDA and continue stirring, transfer the prepared but not yet cooled spinning solution into a syringe, prepare it by dry-wet spray method, extrude the spinning solution through a needle, enter the coagulation bath and coagulate and stretch, wind it by a winder to obtain antibacterial Lyocell fiber, soak it in water for 45 hours and dry it naturally; Step (3) Preparation of oxidative antibacterial Lyocell fibers First, prepare 1.5 mL of disodium hydrogen phosphate and 95 mL of sodium dihydrogen phosphate buffer, strictly control the pH to 6.5, put the buffer and 1.5 g of the pretreated antibacterial Lyocell fiber obtained in step (2) into a three-necked flask, add 0.03 g of TEMPO and 1.75 g of NaClO2, stir at 70 ° C for 15 min, then add 2 g of NaClO, keep the reaction at 70 ° C for 11 h, then add 7 mL of anhydrous ethanol to terminate the reaction, wash the fiber 5 times with anhydrous ethanol, and finally obtain O-Lyocell; Step (4) Preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) Add the ASPPEA flame retardant prepared in step (1) to deionized water, heat it at 75°C to completely dissolve it, and prepare a flame retardant liquid with a concentration of 40wt%, then add dicyandiamide (about 8wt% of the flame retardant liquid) as a catalyst. After the solution is uniform and transparent, add weighed lyocell fiber (ratio is 1:15), take out the Lyocell fiber after 2.5 hours, and then bake the fiber in an oven at 180°C for 8 minutes. The finished fiber is washed with deionized water to remove the flame retardant that has not participated in the reaction, and finally dried at 65°C and weighed to obtain FR-O-Lyocell fiber; Step (5) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell) First, immerse the FR-O-Lyocell fiber prepared in step (4) in a 0.2 mol / L silver nitrate solution for 10 minutes, and then wash off the excess silver nitrate solution with deionized water. Then, immerse the fabric in a 0.05 mol / L sodium borohydride solution for 3 minutes, and the color of the fabric gradually changes from light yellow to black. Finally, wash the modified fabric with deionized water and dry it at 80°C to obtain FR-Ag-O-Lyocell. Step (6) Preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) 3 g of the FR-Ag-O-Lyocell fiber prepared in step (5), 3 g of sodium chloroacetate and a 90 wt % ethanol aqueous solution were placed in a three-necked flask and heated in a water bath at 75° C. for 1 h to fully mix the fiber and the sodium chloroacetate. Then, a 90 wt % ethanol aqueous solution and 2 g of sodium hydroxide were added thereto. The water bath temperature was then raised to 75° C. and maintained for 1-5 h. Finally, the reacted fiber was washed 5 times with anhydrous ethanol until it was neutral to obtain FR-Ag-Cm-O-Lyocell. Step (7) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) is immersed in a 0.3 mol / L copper sulfate solution for 12 minutes, and then the excess copper sulfate solution is washed off with deionized water. Then, a 0.06 mol / L NaBH4 solution is prepared, and the pH value of the solution is adjusted to 9 with NaOH. The fabric is then immersed in this solution for reduction for 2 minutes, and the color of the fiber gradually changes from light blue to copper brown. Finally, the fabric is washed in deionized water and dried at room temperature to obtain FR-Ag-Cm-Cu-O-Lyocell. Example 4

[0030] Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) 2g of VB6 and 6g of phosphoric acid were added to a round-bottom flask equipped with a reflux condenser, magnetic stirring was turned on, the temperature was raised to 140°C, and the temperature was maintained for 3h to finally obtain a light yellow ester liquid, and then 15g of urea was added to the above liquid, and then 130mL of distilled water was added, and the reaction was maintained at 140°C for 3.5h, and then the system was heated to 110°C for 3.5h, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid was obtained by suction filtration. The white solid was dissolved in 140mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid was the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA); Step (2) Pretreatment of antibacterial Lyocell fibers Weigh 16mL NMMO in a beaker, add deionized water to make its water content 14%, then add 3% of the total solution of PG and 4% of the total solution of HA, place in a 85℃ water bath for heating and stirring, add the prepared NMMO aqueous solution to a round-bottom flask while hot, weigh cellulose fiber and add, heat in an oil bath at 125℃, put in a stirrer for stirring (speed 350r / min), wait until the cellulose is completely dissolved, then add BTDA and continue stirring, transfer the prepared but not yet cooled spinning solution into a syringe, prepare by dry-wet spray method, extrude the spinning solution through a needle, enter into a coagulation bath for coagulation and stretching, wind up by a winder to obtain antibacterial Lyocell fiber, soak in water for 42 hours and dry naturally; Step (3) Preparation of oxidative antibacterial Lyocell fibers First, prepare 3 mL of disodium hydrogen phosphate and 100 mL of sodium dihydrogen phosphate buffer, strictly control the pH to 6.6, put the buffer and 2 g of the pretreated antibacterial Lyocell fiber obtained in step (2) into a three-necked flask, add 0.05 g of TEMPO and 1.76 g of NaClO2, stir at 80 ° C for 15 min, then add 3 g of NaClO, keep the reaction at 80 ° C for 8 h, then add 10 mL of anhydrous ethanol to terminate the reaction, wash the fiber 3 times with anhydrous ethanol, and finally obtain O-Lyocell; Step (4) Preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) The ASPPEA flame retardant prepared in step (1) is added to deionized water, heated at 80°C to completely dissolve it, and a flame retardant liquid with a concentration of 40wt% is prepared. Then dicyandiamide (about 8wt% of the flame retardant liquid) is added as a catalyst. When the solution is uniform and transparent, weighed lyocell fiber (ratio is 1:12) is added. After 3 hours, the Lyocell fiber is taken out and then placed in a 140°C oven for 8 minutes. The finished fiber is washed with deionized water to remove the flame retardant that has not participated in the reaction. Finally, it is dried at 70°C and weighed to obtain FR-O-Lyocell fiber; Step (5) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell) First, the FR-O-Lyocell fiber prepared in step (4) was immersed in a 0.2 mol / L silver nitrate solution for 8 minutes, and then the excess silver nitrate solution was washed off with deionized water. The fabric was then immersed in a 0.06 mol / L sodium borohydride solution for reduction for 3 minutes. The color of the fabric gradually changed from light yellow to black. Finally, the modified fabric was washed with deionized water and then dried at 75°C to obtain FR-Ag-O-Lyocell; Step (6) Preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) 3 g of the FR-Ag-O-Lyocell fiber prepared in step (5), 5 g of sodium chloroacetate and a 95 wt% ethanol aqueous solution were placed in a three-necked flask and heated in a water bath at 80°C for 1-5 h to allow the fiber and the sodium chloroacetate to be fully mixed, and then 50-100 wt% ethanol aqueous solution and 3 g of sodium hydroxide were added thereto, and then the water bath temperature was raised to 80°C and maintained for 2 h. Finally, the reacted fiber was washed three times with anhydrous ethanol until it was neutral to obtain FR-Ag-Cm-O-Lyocell; Step (7) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) is soaked in a 0.3 mol / L copper sulfate solution for 10 minutes, and then the excess copper sulfate solution is washed off with deionized water. Then, a 0.05 mol / L NaBH4 solution is prepared, and the pH value of the solution is adjusted to 7 with NaOH. Then, the fabric is soaked in this solution for reduction for 3 minutes, and the color of the fiber gradually changes from light blue to copper brown. Finally, the fabric is washed in deionized water and dried at room temperature to obtain FR-Ag-Cm-Cu-O-Lyocell. Comparative Example 1

[0031] Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) 6 g of VB6 and 10 g of phosphoric acid were added to a round-bottom flask equipped with a reflux condenser, magnetic stirring was turned on, the temperature was raised to 145°C, and the temperature was maintained for 5 hours to finally obtain a light yellow ester liquid, and then 20 g of urea was added to the above liquid, and then 200 mL of distilled water was added, and the temperature was maintained at 150°C for 5 hours, and then the system was heated to 150°C for 5 hours, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid was obtained by suction filtration. The white solid was dissolved in 200 mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid was the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA); Step (2) Lyocell fiber pretreatment Take an appropriate amount of Lyocell fiber and place it in a beaker filled with deionized water, and add a small amount of anhydrous ethanol. Wash it at room temperature for 30 minutes, then take it out, wash it several times with deionized water, and put it in a 60°C oven to dry for use.

[0032] Step (3) Preparation of flame retardant antibacterial Lyocell fiber (FR-Lyocell) Add the ASPPEA flame retardant prepared in step (1) to deionized water, heat it at 100°C to completely dissolve it, and prepare a flame retardant liquid with a concentration of 50wt%, then add dicyandiamide (about 10wt% of the flame retardant liquid) as a catalyst. After the solution is uniform and transparent, add weighed lyocell fiber (ratio is 1:10), take out the Lyocell fiber after 1-5 hours, and then bake the fiber in an oven at 150-200°C for 10 minutes. The finished fiber is washed with deionized water to remove the flame retardant that has not participated in the reaction, and finally dried at 50-100°C and weighed to obtain FR-Lyocell fiber; Step (4) Preparation of flame retardant Lyocell fiber (FR-Ag-Lyocell) First, the FR-Lyocell fiber prepared in step (3) was immersed in a 0.6mol / L silver nitrate solution for 10min, and then the excess silver nitrate solution was washed off with deionized water. The fabric was then immersed in a 0.10mol / L sodium borohydride solution for reduction for 5min, and the color of the fabric gradually changed from light yellow to black. Finally, the modified fabric was washed with deionized water and then dried at 50-100°C to obtain FR-Ag-Lyocell; Step (5) Preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-Lyocell) 4.5 g of the FR-Ag-Lyocell fiber prepared in step (4), 4.5 g of sodium chloroacetate and a 95 wt % ethanol aqueous solution were placed in a three-necked flask and heated in a water bath at 95° C. for 4.5 h to fully mix the fiber and the sodium chloroacetate. Then, 85 wt % ethanol aqueous solution and 4.5 g of sodium hydroxide were added thereto. The water bath temperature was then raised to 95° C. and maintained for 4.5 h. Finally, the reacted fiber was washed twice with anhydrous ethanol until it was neutral to obtain FR-Ag-Cm-Lyocell; Step (6) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cm-Cu-Lyocell) First, the FR-Ag-Cm-Lyocell fiber prepared in step (5) was immersed in a 0.9 mol / L copper sulfate solution for 14 minutes, and then the excess copper sulfate solution was washed off with deionized water. Then, a 0.09 mol / L NaBH4 solution was prepared, and the pH value of the solution was adjusted to 6 with NaOH. The fabric was then immersed in this solution for reduction for 5 minutes, and the color of the fiber gradually changed from light blue to copper brown. Finally, the fabric was washed in deionized water and dried at room temperature to obtain FR-Ag-Cm-Cu-Lyocell. Comparative Example 2

[0033] Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) 3 g of VB6 and 10 g of phosphoric acid were added to a round-bottom flask equipped with a reflux condenser, magnetic stirring was turned on, the temperature was raised to 150°C, and the temperature was maintained for 5 hours to finally obtain a light yellow ester liquid, and then 20 g of urea was added to the above liquid, and then 200 mL of distilled water was added, and the temperature was maintained at 150°C for 5 hours, and then the system was heated to 150°C for 5 hours, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid was obtained by suction filtration. The white solid was dissolved in 200 mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid was the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA); Step (2) Pretreatment of antibacterial Lyocell fibers Weigh 20mL NMMO in a beaker, add deionized water to make its water content 15%, then add 5% of the total solution of PG and 5% of the total solution of HA, place in a 100°C water bath for heating and stirring, add the prepared NMMO aqueous solution to a round-bottom flask while hot, weigh cellulose fiber and add, heat in an oil bath at 150°C, put in a stirrer for stirring (speed 500r / min), wait until the cellulose is completely dissolved, then add BTDA and continue stirring, transfer the prepared but not yet cooled spinning solution into a syringe, prepare by dry-wet spray method, extrude the spinning solution through a needle, enter into a coagulation bath for coagulation and stretching, wind up by a winder to obtain antibacterial Lyocell fiber, soak in water for 24 hours and then dry naturally; Step (3) Preparation of oxidative antibacterial Lyocell fibers First, prepare 5 mL of disodium hydrogen phosphate and 100 mL of sodium dihydrogen phosphate buffer, strictly control the pH to 7, put the buffer and 6 g of the pretreated antibacterial Lyocell fiber obtained in step (2) into a three-necked flask, add 0.10 g of TEMPO and 1.80 g of NaClO2, stir at 100 ° C for 30 min, then add 5 g of NaClO, keep the reaction at 100 ° C for 12 h, then add 20 mL of anhydrous ethanol to terminate the reaction, wash the fiber once with anhydrous ethanol, and finally obtain O-Lyocell; Step (4) Preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) The ASPPEA flame retardant prepared in step (1) is added to deionized water, heated at 100°C to completely dissolve it, and a flame retardant liquid with a concentration of 50wt% is prepared. Then, dicyandiamide (about 10wt% of the flame retardant liquid) is added as a catalyst. After the solution is uniform and transparent, weighed lyocell fiber (ratio of 1:10) is added. After 1 hour, the Lyocell fiber is taken out and then placed in an oven at 200°C for 1 minute. The finished fiber is washed with deionized water to remove the flame retardant that has not participated in the reaction, and finally it is dried at 100°C and weighed to obtain FR-O-Lyocell fiber; Step (5) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-O-Lyocell) First, the FR-O-Lyocell fiber prepared in step (4) was immersed in a 0.6 mol / L silver nitrate solution for 10 min, and then the excess silver nitrate solution was washed off with deionized water. The fabric was then immersed in a 0.10 mol / L sodium borohydride solution for reduction for 6 min, and the color of the fabric gradually changed from light yellow to black. Finally, the modified fabric was washed with deionized water and then dried at 100 ° C to obtain FR-Ag-O-Lyocell; Step (6) Preparation of flame retardant antibacterial Lyocell fiber (FR-Ag-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (5) is immersed in a 1 mol / L copper sulfate solution for 15 minutes, and then the excess copper sulfate solution is washed off with deionized water. Then, a 0.10 mol / L NaBH4 solution is prepared, and the pH value of the solution is adjusted to 5 with NaOH. The fabric is then immersed in this solution for 6 minutes for reduction, and the color of the fiber gradually changes from light blue to copper brown. Finally, the fabric is washed in deionized water and dried at room temperature to obtain FR-Ag-Cu-O-Lyocell.

[0034] Comparison of detection experiments: The fibers obtained in Examples 1 to 4 and Comparative Example Products 1 and 2 were tested. The specific testing methods are as follows: Thermogravimetric analysis (TG) The thermal stability of the modified Lyocell fiber in air was characterized by a thermogravimetric analyzer. The temperature range was set at 40-800°C and the temperature was increased at a rate of 10°C / min.

[0035] Vertical burning test The vertical combustion performance of lyocell fabrics before and after modification and after washing was characterized by a vertical combustion tester. The combustion parameters of lyocell fabrics before and after modification and after washing were mainly tested after a 60 s ignition experiment. The size of the sample to be tested was 300 mm×80 mm×2 mm.

[0036] Analysis of fiber antibacterial properties Weigh 0.75 g of the dried antibacterial fiber and control group fiber, wrap them in tin foil and sterilize them, put them in a wide-mouth bottle containing two bacteria, and expose them to sunlight. Every 60 minutes, take out the liquid in the wide-mouth bottle for dilution and application. Expose for a total of 240 minutes to obtain the inactivation effect of antibacterial nanocellulose on bacteria with increasing illumination time.

[0037]

[0038] As can be seen from Table 1, Example 1 is the best and Comparative Example 2 is the worst. The comparative example data is significantly smaller than that of the example, indicating that the carbon residue is less and easier to burn at 800°C. The generation of high-temperature FR-Ag-Cm-Cu-O-Lyocell fibers can increase the carbon residue of the modified fabric. Since the carbon residue will be further oxidized and decomposed in an aerobic environment, the carbon residue of the fiber is significantly increased compared with that in the air atmosphere, which has the advantage of high carbonization.

[0039]

[0040] As can be seen from Table 2, Example 1 is the best, while Comparative Example 2 is the worst. The data of the comparative example is obviously larger, and the longer the carbonization length, the worse the flame retardant effect. However, the FR-Ag-Cm-Cu-O-Lyocell fiber was not ignited during the experiment, but the carbonization length gradually increased, indicating that the introduction of the flame retardant improved the carbonization effect of the fiber, endowed the fiber with flame retardant properties, and had better flame retardant properties.

[0041]

[0042] As shown in Table 3, Example 1 is the best and Comparative Example 2 is the worst. The data of the comparative example is obviously lower than that of the example, indicating that the antibacterial performance of the fiber of the comparative example against the two bacteria is greatly reduced. However, with the addition of BTDA in the example, the antibacterial Lyocell fiber has antibacterial properties, indicating that the introduction of BTDA improves the antibacterial effect of the fiber, gives the fiber antibacterial ability, and has good antibacterial ability.

[0043] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to the present embodiment as needed, but they are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A method for preparing flame-retardant and antibacterial ecological fiber, characterized in that: include: Preparation of pyridoxine ammonium phosphate, pretreatment of Lyocell fiber, preparation of oxidized Lyocell fiber, preparation of flame retardant Lyocell fiber 1, preparation of flame retardant and antibacterial Lyocell fiber 2 (FR-Ag-O-Lyocell), preparation of carboxymethylated Lyocell fiber, preparation of flame retardant and antibacterial Lyocell fiber 3 (FR-Ag-Cm-Cu-O-Lyocell).

2. A method for preparing a flame retardant and antibacterial ecological fiber according to claim 1, characterized in that: Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) First, VB6 and phosphoric acid are added into a round-bottom flask equipped with a reflux condenser, and magnetic stirring is turned on to heat up to obtain a light yellow ester liquid. Then, a certain proportion of urea is added and distilled water is added to heat up to obtain a bright orange liquid. Secondly, the bright orange liquid is dropped into hot anhydrous ethanol to precipitate a white precipitate. Finally, a white solid is filtered to precipitate again, washed, and vacuum dried to a constant weight to obtain pyridoxine phosphate ammonium salt (ASPPEA). Step (2) Pretreatment of antibacterial Lyocell fibers First, weigh N-methylmorpholine-N-oxide (NMMO) in a beaker, add deionized water, then add PG and HA, heat and stir until it becomes a clear and transparent yellow liquid, then weigh cellulose fiber and add it, heat and stir until it becomes a transparent yellow-brown viscous state, then add 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) and stir until the color of the spinning solution returns to its original state, finally, transfer the spinning solution into a syringe, extrude the spinning solution through a needle, coagulate and stretch, and wind to obtain antibacterial Lyocell fiber, and soak and dry naturally; Step (3) Preparation of oxidative antibacterial Lyocell fibers First, prepare a buffer solution of disodium hydrogen phosphate and sodium dihydrogen phosphate, place the buffer solution and the antibacterial Lyocell fiber prepared in step (2) in a three-necked flask, add 2,2,6,6-tetramethylpiperidinium nitrogen oxide (TEMPO) and sodium chlorite (NaClO2), stir in a sealed manner, add sodium hypochlorite (NaClO), immediately stop the reaction, then add anhydrous ethanol to terminate the reaction, take out the fiber, wash with anhydrous ethanol, and finally obtain the oxidized antibacterial Lyocell fiber; Step (4) Preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) First, the pyridoxine phosphate ammonium salt prepared in step (1) is added to ionized water, heated to dissolve, and dicyandiamide is added as a catalyst. After the solution becomes uniform and transparent, Lyocell fiber is added, taken out after a period of time, then baked and washed, and finally dried and weighed to obtain flame retardant antibacterial Lyocell fiber (FR-O-Lyocell); Step (5) Preparation of flame retardant antibacterial Lyocell fiber II (FR-Ag-O-Lyocell) First, the FR-O-Lyocell fiber prepared in step (4) is immersed in a silver nitrate solution, taken out and washed with deionized water, then immersed in a sodium borohydride solution for reduction, and finally washed with deionized water and dried to obtain a flame retardant and antibacterial Lyocell fiber (FR-Ag-O-Lyocell); Step (6) Preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) The FR-Ag-O-Lyocell fiber prepared in step (5), sodium chloroacetate and ethanol aqueous solution are placed in a three-necked flask, heated in a water bath, then ethanol aqueous solution and sodium hydroxide are added, heated in a water bath, and finally washed with anhydrous ethanol to obtain carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell); Step (7) Preparation of flame retardant antibacterial Lyocell fiber 3 (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) is immersed in a copper sulfate solution, taken out and washed with deionizer, then a sodium borohydride (NaBH4) solution is prepared, and the pH value is adjusted with sodium hydroxide (NaOH), and then immersed in reduction, and finally, washed and dried at room temperature to obtain a flame retardant and antibacterial Lyocell fiber (FR-Ag-Cm-Cu-O-Lyocell).

3. The method for preparing a flame retardant and antibacterial ecological fiber according to claim 2, characterized in that: Step (1) Preparation of pyridoxine phosphate ammonium salt (ASPPEA) 1-6g of VB6 and 3-10g of phosphoric acid are added to a round-bottom flask equipped with a reflux condenser, magnetic stirring is turned on, the temperature is raised to 100-150°C, and the temperature is maintained for reaction for 1-5h to finally obtain a light yellow ester liquid, and then 10-20g of urea is added to the above liquid, and then 100-200mL of distilled water is added, and the temperature is maintained at 100-150°C for reaction for 1-5h, and then the system is heated to 100-150°C for reaction for 1-5h, and then dropped into hot anhydrous ethanol to obtain a white precipitate, and a white solid is obtained by suction filtration. The white solid is dissolved in 100-200mL of distilled water and precipitated again with hot anhydrous ethanol, washed, and vacuum dried to constant weight. The white solid is the prepared flame retardant pyridoxine phosphate ammonium salt (ASPPEA).

4. The method for preparing a flame retardant and antibacterial ecological fiber according to claim 3, characterized in that: Step (2) Pretreatment of antibacterial Lyocell fibers Weigh 10-20mL NMMO in a beaker, add deionized water to make its water content 10-15%, then add 1-5% PG and 1-5% HA of the total solution, place in a 50-100℃ water bath and heat with stirring, add the prepared NMMO aqueous solution into a round-bottom flask while hot, weigh cellulose fiber and add, heat in an oil bath at 100-150℃, put into a stirrer and stir at a speed of 100-500r / min, wait until the cellulose is completely dissolved, then add BTDA and continue stirring, transfer the prepared but not yet cooled spinning solution into a syringe, prepare it by dry-wet spray method, extrude the spinning solution through a needle, enter into a coagulation bath and coagulate and stretch, wind it by a winder to obtain antibacterial Lyocell fiber, soak it in water for 24-48 hours and then dry it naturally.

5. The method for preparing a flame retardant and antibacterial ecological fiber according to claim 4, characterized in that: Step (3) Preparation of oxidative antibacterial Lyocell fibers First, prepare 0-5 mL of disodium hydrogen phosphate and 50-100 mL of sodium dihydrogen phosphate buffer, strictly control the pH to 6-7, place the buffer and 1-6 g of the pretreated antibacterial Lyocell fiber obtained in step (2) in a three-necked flask, add 0.01-0.10 g of TEMPO and 1.70-1.80 g of NaClO2, stir in a sealed container at 50-100°C for 0-30 min, then add 0-5 g of NaClO, keep the reaction at 50-100°C for 6-12 h; then add 0-20 mL of anhydrous ethanol to terminate the reaction; The fiber is washed with anhydrous ethanol for 1-6 times to finally obtain O-Lyocell.

6. The method for preparing a flame retardant and antibacterial ecological fiber according to claim 3, characterized in that: Step (4) Preparation of flame retardant antibacterial Lyocell fiber (FR-O-Lyocell) The ASPPEA flame retardant prepared in step (1) is added to deionized water, heated at 50-100°C to completely dissolve it, and a flame retardant liquid with a concentration of 10-50wt% is prepared. Subsequently, 5-10wt% of dicyandiamide is added as a catalyst to the flame retardant liquid. After the solution is uniform and transparent, weighed lyocell fibers are added in a ratio of 1:10-1:

20. After 1-5 hours, the Lyocell fibers are taken out and then placed in an oven at 150-200°C for baking for 1-10 minutes. The finished fibers are washed with deionized water to remove the flame retardant that has not participated in the reaction. Finally, they are dried at 50-100°C and weighed to obtain FR-O-Lyocell fibers.

7. The method for preparing a flame retardant and antibacterial ecological fiber according to claim 6, characterized in that: Step (5) Preparation of flame retardant antibacterial Lyocell fiber II (FR-Ag-O-Lyocell) First, immerse the FR-O-Lyocell fiber prepared in step (4) in a 0.1-0.6 mol / L silver nitrate solution for 1-10 min, then wash off the excess silver nitrate solution with deionized water, and then immerse the fabric in a 0.01-0.10 mol / L sodium borohydride solution for reduction for 1-6 min. The color of the fabric gradually changes from light yellow to black. Finally, wash the modified fabric with deionized water and dry it at 50-100°C to obtain FR-Ag-O-Lyocell.

8. The method for preparing a flame retardant and antibacterial ecological fiber according to claim 7, characterized in that: Step (6) Preparation of carboxymethylated Lyocell fiber (FR-Ag-Cm-O-Lyocell) 1-5 g of the FR-Ag-O-Lyocell fiber prepared in step (5), 1-5 g of sodium chloroacetate and a 50-100 wt% ethanol aqueous solution are placed in a three-necked flask, and heated in a water bath at 50-100° C. for 1-5 h to allow the fiber and the sodium chloroacetate to be fully mixed, and then 50-100 wt% ethanol aqueous solution and 1-5 g of sodium hydroxide are added thereto, and then the water bath temperature is raised to 50-100° C. and maintained for 1-5 h. Finally, the reacted fiber is washed 1-6 times with anhydrous ethanol until it is neutral to obtain FR-Ag-Cm-O-Lyocell.

9. The method for preparing a flame retardant and antibacterial ecological fiber according to claim 8, characterized in that: Step (7) Preparation of flame retardant antibacterial Lyocell fiber 3 (FR-Ag-Cm-Cu-O-Lyocell) First, the FR-Ag-Cm-O-Lyocell fiber prepared in step (6) is immersed in a 0-1 mol / L copper sulfate solution for 5-15 min, and then the excess copper sulfate solution is washed off with deionized water. Then, a 0.01-0.10 mol / L NaBH4 solution is prepared, and the pH value of the solution is adjusted to 5-10 with NaOH. The fabric is then immersed in the solution for reduction for 1-6 min, and the color of the fiber gradually changes from light blue to copper brown. Finally, the fabric is washed in deionized water and dried at room temperature to obtain FR-Ag-Cm-Cu-O-Lyocell.