Electric leakage testing device, semiconductor wafer and electric leakage testing method
By setting the source, drain and field plate electrodes in the cell area of the gallium nitride device, and using the leakage test device to apply voltage, the problem of inability to provide timely feedback on performance and dielectric quality in the gallium nitride device manufacturing process is solved, and the device can be measured accurate monitoring and cost savings.
Patent Information
- Application Number
- CN202410635829.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-05-21
AI Technical Summary
During the manufacturing process of gallium nitride devices, timely feedback on device performance and media quality cannot be provided, resulting in increased production costs.
Provide a leakage testing device and method, which includes a cell area of a gallium nitride device, setting source, drain and field plate electrodes, applying voltage through the drain pad and field plate pad for leakage testing, and monitoring the electrical properties of the device performance and media quality.
The leakage test device can accurately determine the main leakage sources of gallium nitride devices, monitor the reliability and dielectric defects of the devices, screen out degraded devices in advance, and reduce production costs.
Smart Images

Figure CN118748153A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a leakage test device, a semiconductor wafer and a leakage test method. Background Art
[0002] Gallium nitride (GaN) devices have high breakdown electric field strength, high current density and withstand voltage, and wide band gap and large forbidden band width, which greatly reduce the leakage problem of the device. In addition, due to its large band gap width, it has good high-voltage performance and can work under high temperature, high pressure and high frequency, which can improve the efficiency of the device, reduce consumption and reduce costs; it also has high thermal conductivity and excellent heat dissipation performance, which can make it more integrated and power density than conventional components, so GaN devices are widely used in the field of power electronics.
[0003] The field plate of GaN devices mainly plays the role of modulating the channel distribution of the device, thereby significantly improving the breakdown voltage of the device, and can also effectively improve the problem that the low on-resistance of the device is restricted under high speed and high voltage. In addition, the introduction of the field plate structure can also effectively suppress reliability issues such as current collapse, inverse piezoelectric effect, and stress-related degradation, further improving the power characteristics of GaN devices.
[0004] At present, during the manufacturing process of GaN devices, due to the changes in process technology and fluctuations in machine equipment, the product will have the problem of unstable yield during the process. However, the existing gallium nitride device structure cannot timely feedback the performance of the device and the quality of the medium during the process, and it is impossible to screen out degraded devices in advance, which increases production costs. Summary of the invention
[0005] The present application mainly provides a leakage test device, a semiconductor wafer and a leakage test method to solve the problem in the prior art that device performance and dielectric quality cannot be fed back in time during the manufacturing process of gallium nitride devices.
[0006] In order to solve the above technical problems, a technical solution adopted by the present application is to provide a leakage test device, comprising:
[0007] A first gallium nitride device includes a cell region, wherein a plurality of cells are arranged in the cell region, and each of the cells includes a semiconductor stack and a source electrode, a drain electrode, and a field plate electrode arranged at intervals on one side of the semiconductor stack;
[0008] A drain pad is disposed outside the cell region and electrically connected to the drain of each of the cells;
[0009] A source pad, disposed outside the cell region and electrically connected to the source of each of the cells;
[0010] A field plate pad is disposed outside the cell region and connected to the field plate electrode of each cell;
[0011] The source pad and the field plate pad are arranged on the same side of the cell, and a projection of the source pad on the plane where the field plate pad is located at least partially overlaps with the field plate pad.
[0012] Wherein, along the direction away from the cell, the source electrode includes a source metal layer, a first metal layer and a second metal layer which are stacked, and the drain electrode includes a drain metal layer, the first metal layer and the second metal layer which are stacked; the first metal layer and the second metal layer of the source electrode are disconnected from the first metal layer and the second metal layer of the drain electrode;
[0013] The field plate electrode includes a field plate metal layer, the field plate pad includes the field plate metal layer, and the field plate metal layer of the field plate electrode is connected to the field plate metal layer of the field plate pad;
[0014] The source pad includes the second metal layer, the second metal layer of the source is connected to the second metal layer of the source pad, and the second metal layer of the drain is disconnected from the second metal layer of the source pad;
[0015] The drain pad includes the first metal layer. The first metal layer of the drain is connected to the first metal layer of the drain pad, and the first metal layer of the source is disconnected from the first metal layer of the drain pad.
[0016] Wherein, an insulating dielectric layer is arranged between the field plate pad and the source pad.
[0017] The source pad further includes a first metal layer, and the drain pad further includes the second metal layer and the field plate metal layer.
[0018] Wherein, the leakage test device also includes:
[0019] A gate, the gate being disposed between the source and the field plate electrode, and the field plate electrode being disposed between the gate and the drain;
[0020] A gate pad is disposed outside the cell region and is electrically connected to the gate of each of the cells;
[0021] The gate and the gate pad both include the field plate metal layer, the gate and the field plate metal layer of the gate pad are connected, and the gate and the field plate metal layer of the gate pad are disconnected from the field plate electrode and the field plate metal layer of the field plate pad.
[0022] Wherein, the drain pad is connected to the drain electrodes in each cell in the cell region;
[0023] The gate pad is connected to the gates in each cell in the cell region;
[0024] The source pad is connected to the source electrodes in each cell in the cell area;
[0025] The field plate pad is connected to each of the field plate electrodes in each cell.
[0026] Wherein, the field plate electrode is connected to the field plate pad through a first wire formed by the field plate metal layer;
[0027] The source electrode is connected to the source electrode pad through a second wire formed by the second metal layer;
[0028] The drain electrode is connected to the drain pad through a third wire formed by the first metal layer;
[0029] Projections of the first conductive line and the second conductive line on the plane where the field plate pad is located are arranged at an interval.
[0030] Each of the cells further comprises: a passivation layer disposed on the semiconductor stack, wherein the passivation layer is used to insulate the source, the gate, the field plate electrode and the drain in the cell region.
[0031] The semiconductor stack includes a substrate, a buffer layer arranged on the substrate, a first semiconductor layer arranged on the buffer layer, and a second semiconductor layer on the first semiconductor layer, and a heterojunction structure is formed between the first semiconductor layer and the second semiconductor layer.
[0032] In order to solve the above technical problems, another technical solution adopted by the present application is: to provide a semiconductor wafer, comprising:
[0033] A plurality of device regions, each of which has a second gallium nitride device;
[0034] A plurality of test areas, each of which is provided with at least one leakage test device, wherein the leakage test device is any one of the leakage test devices described above, and the leakage test device is used to test whether the second gallium nitride device has leakage and determine the source of the leakage.
[0035] In order to solve the above technical problems, another technical solution adopted by the present application is to provide a leakage test method, comprising:
[0036] Obtain a first gallium nitride preform; the first gallium nitride preform comprises: a cell region, a plurality of cells are arranged in the cell region, each of the cells comprises a semiconductor stack and a source electrode and a drain electrode spaced apart and arranged on one side of the semiconductor stack; the source electrode comprises a source metal layer, and the drain electrode comprises a drain metal layer;
[0037] A field plate electrode and a field plate pad are fabricated on one side of the first gallium nitride preform where the source metal layer and the drain metal layer are disposed, wherein the field plate electrode is connected to the field plate pad;
[0038] The source electrode, the drain electrode and the drain pad are continuously manufactured on the side of the first gallium nitride preform provided with the source metal layer and the drain metal layer, and the drain electrode is connected to the drain pad;
[0039] A voltage is applied to the drain pad and the field plate pad to perform a leakage test.
[0040] Wherein, the leakage test method further includes:
[0041] After the field plate pad is manufactured, before the drain electrode and the drain pad are connected to each other, an insulating dielectric layer is manufactured on the surface of the field plate pad.
[0042] Wherein, the leakage test method further includes:
[0043] After the leakage test is performed, a source pad is manufactured and the source electrode and the drain electrode are manufactured, and the source electrode is connected to the source pad;
[0044] The source pad and the field plate pad are arranged on the same side of the cell, and a projection of the source pad on the plane where the field plate pad is located at least partially overlaps with the field plate pad.
[0045] The step of manufacturing a field plate electrode and a field plate pad on a side of the first gallium nitride preform provided with the source metal layer and the drain metal layer, and connecting the field plate electrode and the field plate pad comprises:
[0046] A field plate metal layer is fabricated on one side of the first gallium nitride preform provided with the source metal layer and the drain metal layer to form the field plate electrode and the field plate pad, wherein the field plate electrode and the field plate pad are connected via a first wire formed by the field plate metal layer;
[0047] The source electrode, the drain electrode and the drain pad are continuously manufactured on the side of the first gallium nitride preform provided with the source metal layer and the drain metal layer, and the step of connecting the drain electrode and the drain pad comprises:
[0048] A first metal layer is formed on the surface of the first gallium nitride preform provided with the field plate electrode to form the source electrode, the drain electrode and the drain pad, wherein the drain electrode and the drain pad are connected via a third wire formed by the first metal layer;
[0049] After the leakage test is performed, the source pad is manufactured and the source and the drain are manufactured, and the steps of connecting the source and the source pad include:
[0050] A second metal layer is formed on the surface of the first gallium nitride preform provided with the first metal layer to form the source electrode, the drain electrode and the source electrode pad. The source electrode and the source electrode pad are connected through a second wire formed by the second metal layer.
[0051] The beneficial effects of the present application are as follows: Different from the prior art, the present application discloses a leakage test device, a semiconductor wafer and a leakage test method, wherein the leakage test device comprises a first gallium nitride device, comprising a cell region, a plurality of cells are arranged in the cell region, each cell comprises a semiconductor stack and a source, a drain and a field plate electrode arranged at intervals on one side of the semiconductor stack; a drain pad is arranged outside the cell region and electrically connected to the drain of each cell; a source pad is arranged outside the cell region and electrically connected to the source of each cell; a field plate pad is arranged outside the cell region and electrically connected to the field plate electrode of each cell; wherein the source pad and the field plate pad are arranged on the same side of the cell, and the projection of the source pad on the plane where the field plate pad is located at least partially overlaps with the field plate pad. Through the above arrangement, the problem that the performance of the device and the quality of the medium cannot be fed back in time in the process of the gallium nitride device can be solved, and the cost can be saved. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0053] Figure 1 It is a structural schematic diagram of an embodiment of a leakage test device provided by the present application;
[0054] Figure 2 yes Figure 1 A cross-sectional schematic diagram of a first gallium nitride device of a leakage test device provided;
[0055] Figure 3 It is a flow chart of the first embodiment of the leakage test method provided by the present application;
[0056] Figure 4 It is a flow chart of the second embodiment of the leakage testing method provided by the present application;
[0057] Figure 5 It is a structural schematic diagram of an embodiment of a semiconductor wafer provided in the present application. DETAILED DESCRIPTION
[0058] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0059] The terms "first", "second", "third" in the embodiments of the present application are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second", "third" can expressly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.
[0060] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0061] See also Figure 1 to Figure 2 , Figure 1 is a structural schematic diagram of an embodiment of a leakage test device provided by the present application, Figure 2 yes Figure 1 A schematic cross-sectional view of a first gallium nitride device of a leakage test device is provided.
[0062] See also Figure 1 and Figure 2The present application provides a leakage test device 100, which includes a first gallium nitride device 1, a drain pad 2, a source pad 3 and a field plate pad 4. The first gallium nitride device 1 includes a cell region A, in which a plurality of cells are arranged, and each cell includes a semiconductor stack 5 and a source 6, a drain 7 and a field plate electrode 8 arranged at intervals on one side of the semiconductor stack 5. The drain pad 2, the source pad 3 and the field plate pad 4 are all arranged outside the cell region A, and the drain pad 2 is electrically connected to the drain 7 of each cell, the source pad 3 is electrically connected to the source 6 of each cell, and the field plate pad 4 is electrically connected to the field plate electrode 8 of each cell.
[0063] In this embodiment, the source pad 3 and the field plate pad 4 are arranged on the same side of the cell, and the projection of the source pad 3 on the plane where the field plate pad 4 is located at least partially overlaps with the field plate pad 4 . The projection of the source pad 3 on the plane where the field plate pad 4 is located is set to at least partially overlap with the field plate pad 4, and the source pad 3 is electrically connected to the source 6 of each cell, the field plate pad 4 is electrically connected to the field plate electrode 8 of each cell, and the drain pad 2 is electrically connected to the drain 7 of each cell. A voltage is applied to the field plate pad 4 and the drain pad 2. A leakage test can be performed using a test instrument to test the BV electrical curve (breakdown curve). According to the leakage data obtained from the test, the quality of the field plate electrode 8 and the leakage channel can be monitored, and the main leakage source of the first gallium nitride device 1 can be more accurately determined, the failure point can be confirmed, and the electrical performance of the device structure, the reliability of the device, the dielectric defects and the defects between the dielectric contact surfaces can be accurately fed back. Degraded devices can be screened out in advance, thereby reducing costs. At the same time, it does not affect the use of the first gallium nitride device 1, and effectively solves the problem that the performance of the device and the quality of the dielectric cannot be fed back in time in the manufacturing process of the gallium nitride device in the prior art.
[0064] In some embodiments, the first gallium nitride device 1 is an E-HEMT (Enhancement-Mode High Electron Mobility Transistor) device, which is completely consistent with a normal gallium nitride device in structure. Using an E-HEMT device to replace a real gallium nitride device can avoid problems such as device damage that may occur when directly testing a real gallium nitride device. Further, the presence of several pads in the leakage test device 100 can effectively increase the breakdown voltage of the E-HEMT device. In other embodiments, the E-HEMT device is composed of several gallium nitride devices, which are also called cells. The number of cells is determined according to actual conditions and is not limited here.
[0065] like Figure 1 and Figure 2As shown, in some embodiments, the cell region A has a first side and a second side relative to each other, the direction from the first side to the second side is the extension direction of the cell, the drain pad 2 is arranged on the first side of the cell, the source pad 3 and the field plate pad 4 are both arranged on the second side of the cell, and the projection of the source pad 3 on the plane where the field plate pad 4 is located completely overlaps with the field plate pad 4.
[0066] In other embodiments, the source pad 3 and the field plate pad 4 may also be simultaneously arranged on the first side of the cell, and the drain pad 2 may be arranged on the second side of the cell, or the source pad 3 and the field plate pad 4 may also be arranged at any other position, and the projection of the source pad 3 on the plane where the field plate pad 4 is located may also only partially overlap with the field plate pad 4.
[0067] Specifically, Figure 2 As shown, the semiconductor stack 5 includes a substrate 51, a buffer layer 52 arranged on the substrate 51, a first semiconductor layer 53 arranged on the buffer layer 52, and a second semiconductor layer 54 arranged on the first semiconductor layer 53, which are stacked in sequence. The first semiconductor layer 53 and the second semiconductor layer 54 have a heterojunction structure, and the heterojunction between the first semiconductor layer 53 and the second semiconductor layer 54 can form a two-dimensional electron gas (2DEG) with high mobility, high density and high conductivity. When a voltage is applied to the drain 7 and the source 6, the two-dimensional electron gas can effectively conduct electrons, so that the first gallium nitride device 1 can have excellent performance.
[0068] In a specific embodiment, the material of the substrate 51 includes but is not limited to Si, SiC, etc. The material of the first semiconductor layer 53 includes GaN, and the material of the second semiconductor layer 54 includes AlGaN, and an AlGaN / GaN heterojunction structure is formed between the first semiconductor layer 53 and the second semiconductor layer 54 .
[0069] like Figure 2 As shown, in some embodiments, along the direction away from the cell, the source 6 includes a source metal layer 61, a first metal layer M1 and a second metal layer M2 which are stacked, the drain 7 includes a drain metal layer 71, a first metal layer M1 and a second metal layer M2 which are stacked, the first metal layer M1 of the source 6 is disconnected from the first metal layer M1 of the drain 7, and the second metal layer M2 of the source 6 is disconnected from the second metal layer M2 of the drain 7, that is, the first metal layer M1 of the source 6 and the first metal layer M1 of the drain 7 are the same metal layer, but are spaced apart from each other, and the second metal layer M2 of the source 6 and the second metal layer M2 of the drain 7 are the same metal layer, but are spaced apart from each other.
[0070] The field plate electrode 8 includes a field plate metal layer M3, and the field plate pad 4 includes a field plate metal layer M3. The field plate metal layer M3 of the field plate electrode 8 is connected to the field plate metal layer M3 of the field plate pad 4, that is, the field plate metal layer M3 of the field plate electrode 8 and the field plate metal layer M3 of the field plate pad 4 are the same metal layer, but the field plate metal layer M3 of the field plate electrode 8 is located in the cell area A, and the field plate metal layer M3 of the field plate pad 4 is located outside the cell area A, and the field plate metal layer M3 of the field plate electrode 8 and the field plate metal layer M3 of the field plate pad 4 are connected to each other.
[0071] In this embodiment, the field plate pad 4 only includes the field plate metal layer M3, and does not include the first metal layer M1 or the second metal layer M2. The field plate electrode 8 only includes the field plate metal layer M3, and does not include the first metal layer M1 and the second metal layer M2. The field plate metal layer M3 of the field plate pad 4 is connected to the field plate metal layer M3 of the field plate electrode 8 to realize the electrical connection between the field plate pad 4 and the field plate electrode 8.
[0072] In a specific embodiment, the field plate electrode 8 is connected to the field plate pad 4 through the first wire L1 formed by the field plate metal layer M3, that is, the field plate electrode 8, the first wire L1 and the field plate pad 4 are formed by the same field plate metal layer M3. In other embodiments, the field plate metal layer M3 of the field plate electrode 8 can also be electrically connected to the field plate metal layer M3 of the field plate pad 4 by other means.
[0073] In some embodiments, the source pad 3 includes a second metal layer M2, the second metal layer M2 of the source 6 is connected to the second metal layer M2 of the source pad 3, and the second metal layer M2 of the drain 7 is disconnected from the second metal layer M2 of the source pad 3, that is, the second metal layer M2 of the source pad 3 and the second metal layer M2 of the source 6 and the second metal layer M2 of the drain 7 are all the same metal layer, but the second metal layer M2 of the source pad 3 and the second metal layer M2 of the source 6 are connected to each other, and the second metal layer M2 of the drain 7 is separated from the second metal layer M2 of the source pad 3 and the second metal layer M2 of the source 6.
[0074] In a specific embodiment, the source 6 is connected to the source pad 3 through the second wire L2 formed by the second metal layer M2, that is, the second metal layer M2 of the source 6, the first wire L1 and the second metal layer M2 of the field plate pad 4 are formed by the same metal layer. Figure 1 As shown, the first wire L1 and the second wire L2 are both located on the same side of the cell region A, and the projections of the first wire L1 and the second wire L2 on the plane where the field plate pad 4 is located are spaced apart. In other embodiments, the source 6 may also be electrically connected to the source pad 3 through other metal layers or wires or other methods.
[0075] In some embodiments, the drain pad 2 includes a first metal layer M1, the first metal layer M1 of the drain 7 is connected to the first metal layer M1 of the drain pad 2, and the first metal layer M1 of the source 6 is disconnected from the first metal layer M1 of the drain pad 2. That is, the first metal layer M1 of the drain pad 2, the first metal layer M1 of the drain 7, and the first metal layer M1 of the source 6 are the same metal layer, except that the first metal layer M1 of the drain pad 2 is located outside the cell region A, the first metal layer M1 of the drain 7 and the first metal layer M1 of the source 6 are located in the cell region A and are spaced and disconnected from each other, and the first metal layer M1 of the drain 7 and the first metal layer M1 of the drain pad 2 are connected to each other.
[0076] In a specific embodiment, the drain electrode 7 is connected to the drain pad 2 through the third wire L3 formed by the first metal layer M1, that is, the first metal layer M1 of the drain electrode 7, the third wire L3, and the first metal layer M1 of the drain pad 2 are formed by the same metal layer. Figure 1 As shown, the third wire L3 is located at the first side of the cell area A, and the first wire L1 and the second wire L2 are both located at the second side of the cell area A. In other embodiments, the first metal layer M1 of the drain 7 may also be electrically connected to the first metal layer M1 of the drain pad 2 through other wires or methods.
[0077] Specifically, the source metal layer 61 is in ohmic contact with the semiconductor stack 5, and the drain metal layer 71 is in ohmic contact with the semiconductor stack 5. In some embodiments, the source metal layer 61 may be a single substance, alloy or compound including any one of Ti, Al, Ni, Au, and Ta, and the drain metal layer 71 may be a single substance, alloy or compound including any one of Ti, Al, Ni, Au, and Ta. The field plate metal layer M3 may be a single substance, alloy or compound including any one of Ti, Al, Ni, Au, and Ta, and the first metal layer M1 and the second metal layer M2 may also be a single substance, alloy or compound including any one of Ti, Al, Ni, Au, and Ta.
[0078] Since the source pad 3 and the field plate pad 4 are arranged on the same side of the cell, and the projection of the source pad 3 on the plane where the field plate pad 4 is located at least partially overlaps with the field plate pad 4, therefore, Figure 2 As shown, an insulating dielectric layer 9 is disposed between the field plate pad 4 and the source pad 3 so that the source pad 3 and the field plate pad 4 are insulated from each other to avoid mutual influence between the source pad 3 and the field plate pad 4 during testing.
[0079] In some embodiments, Figure 2As shown, the source pad 3 also includes a first metal layer M1, and the drain pad 2 also includes a second metal layer M2 and a field plate metal layer M3. That is, the source pad 3 includes the first metal layer M1 and the second metal layer M2 stacked in sequence, and the second metal layer M2 of the source pad 3 is connected to the second metal layer M2 of the source 6. The drain pad 2 also includes the field plate metal layer M3, the first metal layer M1 and the field plate metal layer M3 stacked in sequence, and the first metal layer M1 of the drain pad 2 is connected to the first metal layer M1 of the drain 7.
[0080] In other embodiments, the source pad 3 may include only the second metal layer M2 but not the first metal layer M1, the drain pad 2 may include only the first metal layer M1, or may include both the first metal layer M1 and the field plate metal layer M3 but not the second metal layer M2, or the drain pad 2 may include both the first metal layer M1 and the second metal layer M2 but not the field plate metal layer M3. The design may be performed as needed, as long as the second metal layer M2 of the source pad 3 and the second metal layer M2 of the source 6 are interconnected to achieve electrical connection between the source pad 3 and the source 6, and the first metal layer M1 of the drain pad 2 and the first metal layer M1 of the drain 7 are interconnected to achieve electrical connection between the drain pad 2 and the drain 7.
[0081] See also Figure 1 and Figure 2 The leakage test device 100 also includes a gate 10 and a gate pad 11. The gate 10 is located in the cell area A and is arranged between the source 6 and the field plate electrode 8. The field plate electrode 8 is arranged between the gate 10 and the drain 7. The gate pad 11 is arranged outside the cell area A and is electrically connected to the gate 10 of each cell.
[0082] like Figure 2 As shown, in some embodiments, the gate pad 11 is located on the second side of the cell region A, that is, the gate pad 11 and the source pad 3 and the field plate pad 4 are located on the same side of the cell region A, and the gate pad 11 and the source pad 3 and the field plate pad 4 are spaced apart. In other embodiments, the gate pad 11 can also be disposed at any position outside the cell region A.
[0083] like Figure 2 As shown, in some embodiments, the gate 10 and the gate pad 11 both include a field plate metal layer M3, the field plate metal layer M3 of the gate 10 is connected to the field plate metal layer M3 of the gate pad 11, the field plate metal layer M3 of the gate 10 is disconnected from the field plate metal layer M3 of the field plate electrode 8, and the field plate metal layer M3 of the gate pad 11 is disconnected from the field plate metal layer M3 of the field plate pad 4 and the field plate metal layer M3 of the field plate electrode 8. That is, the field plate metal layer M3 of the gate 10, the field plate metal layer M3 of the gate pad 11, the field plate metal layer M3 of the field plate electrode 8, and the field plate metal layer M3 of the field plate pad 4 are the same metal layer.
[0084] In a specific embodiment, the gate 10 may be connected to the gate pad 11 through another conductive line formed by the field plate metal layer M3. In other embodiments, the gate 10 may also be electrically connected to the field plate metal layer M3 of the gate pad 11 through other means.
[0085] In other embodiments, the gate pad 11 may also include a first metal layer M1 and / or a second metal layer M2, that is, the gate pad 11 may include a field plate metal layer M3, a first metal layer M1 and a second metal layer M2 which are stacked in sequence, or may only include a stacked field plate metal layer M3 and a first metal layer M1, or may only include a stacked field plate metal layer M3 and a second metal layer M2, or may only include a stacked field plate metal layer M3 and a second metal layer M2, or may only include a field plate metal layer M3. It can be designed as needed, as long as the field plate metal layer M3 of the gate pad 11 and the field plate metal layer M3 of the gate 10 are interconnected to achieve electrical connection between the gate 10 and the gate pad 11.
[0086] In some embodiments, a cap layer (not shown) may be provided on the side of the field plate metal layer M3 of the gate 10 close to the semiconductor stack 5. The cap layer may be a P-GaN layer, which may improve the energy band at the AlGaN / GaN heterojunction interface.
[0087] In some embodiments, Figure 1 As shown, the drain pad 2 is connected to the drains 7 in each cell in the cell region A, the gate pad 11 is connected to the gates 10 in each cell in the cell region A, and the field plate pad 4 is connected to each field plate electrode 8 in each cell. The drains 7, gates 10, and field plate electrodes 8 in multiple cells can be connected to the corresponding pads after being collected, which can simplify the structure and reduce costs.
[0088] See also Figure 2 In some embodiments, each cell further includes a passivation layer 12 disposed on the semiconductor stack 5, and the passivation layer 12 is used to insulate the source 6, the gate 10, the field plate electrode 8, and the drain 7 in the cell region A to avoid mutual influence.
[0089] In some embodiments, Figure 2As shown, the passivation layer 12 includes a first passivation layer 121, a second passivation layer 122 and a third passivation layer 123. The first passivation layer 121 is arranged on the surface of the semiconductor stack 5 close to the gate 10 and between the field plate electrode 8 and the drain metal layer 71. The first passivation layer 121 directly contacts the AlGaN surface; the second passivation layer 122 is arranged on the side of the gate 10 away from the semiconductor stack 5 and covers the gate 10, the field plate electrode 8, the first passivation layer 121 and the semiconductor stack 5. The second passivation layer 122 is located between the source 6 and the drain 7; the third passivation layer 123 covers the side of the second passivation layer 122 away from the semiconductor stack 5 and is located between the source 6 and the drain 7. The main constituent elements of the first passivation layer 121, and / or the second passivation layer 122, and / or the third passivation layer 123 include any one or more of Si, O, Al, and N.
[0090] In a specific embodiment, Figure 2 As shown, the field plate electrode 8 includes a main body portion 81 and a lap portion 82 which are connected to each other. The main body portion 81 is arranged on the surface of the semiconductor stack 5 close to the gate 10 and the side of the main body portion 81 is arranged in contact with the side of the first passivation layer 121. The lap portion 82 partially covers the surface of the first passivation layer 121 away from the semiconductor stack 5.
[0091] In the embodiment of the present application, the leakage test device 100 provided by the present application is used. During the manufacturing process of the first gallium nitride device 1, a voltage is applied to the field plate pad 4 and the drain pad 2, and a test instrument, such as a B1500 tester, is used to perform a BV electrical curve (breakdown curve) test on the first gallium nitride device 1. According to the test results or leakage data, such as the magnitude of the leakage current, the quality of the field plate electrode 8 and the leakage channel can be monitored, and the main leakage source of the first gallium nitride device 1 can be more accurately determined. The quality and defects of the first passivation layer 121 and the contact surface between the first passivation layer 121 and AlGaN are monitored to confirm the failure point. For example, when the B1500 tester is used to perform a BV electrical curve test on the first gallium nitride device 1, the voltage will be limited to 200V during the test, and the normal current during the test is at the nA level. If the leakage current is large, the current value will reach the mA level or even directly break down.
[0092] The above arrangement can accurately feedback the electrical performance of the device structure, the reliability of the device, the dielectric defects, and the defects between the dielectric contact surfaces. At the same time, the design of the field plate electrode 8 can be integrated into the E-HEMT device without affecting the use of the first gallium nitride device 1. The design of the field plate electrode 8 can detect the deficiencies of the process in advance, and the degraded devices can be screened out in advance, thereby reducing costs and effectively solving the problem of the inability to timely feedback the device performance and dielectric quality in the process of gallium nitride devices in the prior art. In the embodiment of the present application, since the E-HEMT device is completely consistent with the normal gallium nitride device in structure, leakage data can be obtained from the test pattern monitoring, and the main leakage source of the device can be more accurately determined, saving costs.
[0093] See also Figure 3 to Figure 4 , Figure 3 is a flow chart of the first embodiment of the leakage test method provided by the present application, Figure 4 It is a flow chart of the second embodiment of the leakage testing method provided by the present application.
[0094] See also Figure 3 The present application also provides a leakage test method, which can be used to detect the leakage of the first gallium nitride device 1. Specifically, the leakage test method includes:
[0095] S1A: Obtain a first gallium nitride preform.
[0096] Specifically, a first gallium nitride preform is obtained, which includes a cell region A, in which a plurality of cells are arranged, each cell includes a semiconductor stack 5 and a source 6 and a drain 7 spaced apart on one side of the semiconductor stack 5, wherein the source 6 includes a source metal layer 61, and the drain 7 includes a drain metal layer 71.
[0097] Specifically, the semiconductor stack 5 includes a substrate 51, a buffer layer 52 arranged on the substrate 51, a first semiconductor layer 53 arranged on the buffer layer 52, and a second semiconductor layer 54 arranged on the first semiconductor layer 53, which are stacked in sequence. The first semiconductor layer 53 and the second semiconductor layer 54 have a heterojunction structure, and the heterojunction between the first semiconductor layer 53 and the second semiconductor layer 54 can form a two-dimensional electron gas (2DEG) with high mobility, high density and high conductivity. When a voltage is applied to the drain 7 and the source 6, the two-dimensional electron gas can effectively conduct electrons, so that the first gallium nitride device 1 can have excellent performance.
[0098] In a specific embodiment, the material of the substrate 51 includes but is not limited to Si, SiC, etc. The material of the first semiconductor layer 53 includes GaN, and the material of the second semiconductor layer 54 includes AlGaN, and an AlGaN / GaN heterojunction structure is formed between the first semiconductor layer 53 and the second semiconductor layer 54 .
[0099] The source metal layer 61 is in ohmic contact with the semiconductor stack 5, and the drain metal layer 71 is in ohmic contact with the semiconductor stack 5. In some embodiments, the source metal layer 61 can be a single substance, alloy or compound including any one of Ti, Al, Ni, Au, and Ta, and the drain metal layer 71 can be a single substance, alloy or compound including any one of Ti, Al, Ni, Au, and Ta.
[0100] S2A: A field plate electrode 8 and a field plate pad 4 are fabricated on one side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 , and the field plate electrode 8 is connected to the field plate pad 4 .
[0101] Specifically, the field plate electrode 8 and the field plate pad 4 are manufactured on one side of the first gallium nitride preform where the source metal layer 61 and the drain metal layer 71 are provided, wherein the field plate electrode 8 and the field plate pad 4 are interconnected.
[0102] Specifically, in some embodiments, the step of manufacturing the field plate electrode 8 and the field plate pad 4 on the side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 in step S2, and connecting the field plate electrode 8 with the field plate pad 4, comprises:
[0103] A field plate metal layer M3 is fabricated on one side of the first gallium nitride preform where the source metal layer 61 and the drain metal layer 71 are disposed to form a field plate electrode 8 and a field plate pad 4 , which are connected to each other via a first wire L1 formed by the field plate metal layer M3 .
[0104] Specifically, a field plate metal layer M3 can be deposited on one side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 by evaporation or sputtering, and the field plate metal layer M3 is patterned, so that a field plate electrode 8 is formed between the source metal layer 61 and the drain metal layer 71 in the cell region A, the field plate electrode 8 is in direct contact with the second semiconductor layer 54 of the semiconductor stack 5, and a field plate pad 4 is formed outside the cell region A, and a first wire L1 connecting the field plate pad 4 and the field plate electrode 8 is formed, so that the field plate electrode 8 is connected to the field plate pad 4 through the first wire L1 formed by the field plate metal layer M3. The material of the field plate metal layer M3 can be a single substance, alloy or compound including any one of Ti, Al, Ni, Au and Ta.
[0105] In some embodiments, each cell of the first gallium nitride preform further includes a passivation layer 12. Before manufacturing the field plate electrode 8 and the field plate pad 4 in step S2A, the leakage current testing method further includes:
[0106] A first passivation layer 121 is formed on one side of the first gallium nitride preform where the source metal layer 61 and the drain metal layer 71 are provided. The first passivation layer 121 is located between the source metal layer 61 and the drain metal layer 71 .
[0107] Specifically, the first passivation layer 121 can be deposited by any one of atomic layer deposition (ALD), low pressure chemical vapor deposition (LPCVD), physical vapor deposition (PVD) and ion enhanced chemical vapor deposition (PECVD), so that the first passivation layer 121 is located between the source metal layer 61 and the drain metal layer 71 and is in contact with the surface of the second semiconductor layer 54 of the semiconductor stack 5, namely the AlGaN layer, and the first passivation layer 121 is spaced apart from the source metal layer 61.
[0108] In some embodiments, the field plate electrode 8 prepared by the field plate metal layer M3 includes a main body portion 81 and a lap portion 82 that are interconnected, the main body portion 81 is arranged on the surface of the semiconductor stack 5 close to the source metal layer 61 and the side of the main body portion 81 is arranged in contact with the side of the first passivation layer 121, and the lap portion 82 partially covers the surface of the first passivation layer 121 away from the semiconductor stack 5.
[0109] S3A: The source electrode 6 , the drain electrode 7 and the drain pad 2 are continuously manufactured on the side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 , and the drain electrode 7 is connected to the drain pad 2 .
[0110] Specifically, after the field plate electrode 8 and the field plate pad 4 are manufactured in step S2A, the source 6, the drain 7 and the drain pad 2 are manufactured on the side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71, and the drain 7 is connected to the drain pad 2.
[0111] Specifically, in some embodiments, the step of continuing to form the source electrode 6, the drain electrode 7 and the drain pad 2 on the side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 in step S3A, and connecting the drain electrode 7 with the drain pad 2, comprises:
[0112] A first metal layer M1 is formed on the surface of the first GaN preform provided with the field plate electrode 8 to form a source 6, a drain 7 and a drain pad 2. The drain 7 is connected to the drain pad 2 through a third wire L3 formed by the first metal layer M1.
[0113] Specifically, a first metal layer M1 can be deposited on the surface of the first gallium nitride preform provided with the field plate electrode 8 by using a process such as evaporation or sputtering, and the first metal layer M1 is patterned, so that the first metal layer M1 is formed on the source metal layer 61 and the drain metal layer 71 in the cell area A and outside the cell area A, the first metal layer M1 outside the cell area A forms a drain pad 2, the first metal layer M1 on the source metal layer 61 and the first metal layer M1 on the drain metal layer 71 are spaced apart from each other and disconnected, the first metal layer M1 outside the cell area A, i.e., the drain pad 2, is disconnected from the first metal layer M1 on the source metal layer 61, and a third wire L3 connecting the first metal layer M1 outside the cell area A, i.e., the drain pad 2, and the first metal layer M1 on the drain metal layer 71 is formed, and the third wire L3 is also formed by the first metal layer M1.
[0114] The source metal layer 61 is stacked with the first metal layer M1 formed on the source metal layer 61 and the two together form the source 6, that is, the source 6 includes the source metal layer 61 and the first metal layer M1 stacked; the drain metal layer 71 is stacked with the first metal layer M1 formed on the drain metal layer 71 and the two together form the drain 7, the drain 7 includes the drain metal layer 71 and the first metal layer M1 stacked, and the drain pad 2 includes the first metal layer M1. The material of the first metal layer M1 can be a single substance, alloy or compound including any one of Ti, Al, Ni, Au and Ta.
[0115] In other embodiments, the first metal layer M1 of the drain 7, the first metal layer M1 of the source 6, and the first metal layer M1 of the drain pad 2 may not be formed by the same metal layer, and the drain pad 2 and the drain 7 may not be connected by the third wire L3 formed by the first metal layer M1, and may be connected by other wires or methods, as long as the source 6 and the drain 7 are separated from each other and the drain 7 and the drain pad 2 can be electrically connected.
[0116] S4A: Apply voltage to the drain pad 2 and the field plate pad 4 to perform a leakage test.
[0117] Specifically, voltage is applied to the drain pad 2 and the field plate pad 4, and a test instrument, such as a B1500 tester, is used to perform a BV electrical curve on the first gallium nitride preform. Based on the test results or leakage data, such as the magnitude of the leakage current, the quality of the field plate electrode 8 and the leakage channel can be monitored, and the main leakage source of the first gallium nitride device 1 can be more accurately determined. The quality and defects of the first passivation layer 121 and the contact surface between the first passivation layer 121 and AlGaN are monitored to confirm the failure point. For example, when the BV electrical curve test is performed on the first gallium nitride preform using the B1500 tester, the voltage will be limited to 200V during the test, and the normal current during the test is at the nA level. If the leakage current is large, the current value will reach the mA level or even directly break down.
[0118] Through the above method, the electrical performance of the device structure, the reliability of the device, the dielectric defects and the defects between the dielectric contact surfaces can be accurately fed back. By utilizing the design of the field plate electrode 8, it is only necessary to connect the field plate pad 4 to the field plate electrode 8 and the drain pad 2 to the drain 7 after preparing the field plate electrode 8, the drain 7, the field plate pad 4 and the drain pad 2. By applying a voltage between the field plate electrode 8 and the drain 7, the defects of the first passivation layer 121 and the defects of the contact surface between the first passivation layer 121 and the AlGaN can be monitored in advance, the deficiencies of the process can be checked in advance, and the aged devices can be screened out in advance. This can effectively solve the problem that the performance of the device and the quality of the dielectric cannot be fed back in time in the manufacturing process of the gallium nitride device in the prior art, thereby reducing the cost.
[0119] See also Figure 4 The present application also provides another leakage test method, which can be used to detect the leakage of the first gallium nitride device 1 and prepare a Figure 1 The leakage test device 100 shown. Specifically, the leakage test method includes:
[0120] S1B: Obtain a first gallium nitride preform.
[0121] Specifically, it is the same as step S1A of the first embodiment of the leakage test method and can achieve the same or similar technical effects, so it is not repeated here.
[0122] S2B: A field plate electrode 8 and a field plate pad 4 are fabricated on one side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 , and the field plate electrode 8 is connected to the field plate pad 4 .
[0123] Specifically, it is the same as step S2A of the first embodiment of the leakage test method and can achieve the same or similar technical effects, so it will not be repeated.
[0124] S3B: After the field plate pad 4 is manufactured, before the drain electrode 7 and the drain pad 2 are connected to each other, an insulating dielectric layer 9 is manufactured on the surface of the field plate pad 4 .
[0125] Specifically, an insulating dielectric layer 9 is deposited on one side of the field plate pad 4 by any one of atomic layer deposition, low pressure chemical vapor deposition, physical vapor deposition and ion enhanced chemical vapor deposition, so that the insulating dielectric layer 9 covers the field plate pad 4, i.e., the surface of the field plate metal layer M3 outside the cell region A. By preparing the insulating dielectric layer 9 on the surface of the field plate pad 4, it is possible to avoid the problem of the source pad 3 contacting the field plate pad 4 and affecting the test effect when the source pad 3 is manufactured in the subsequent process.
[0126] S4B: Continue to manufacture the source 6 , the drain 7 and the drain pad 2 on one side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 , and the drain 7 is connected to the drain pad 2 .
[0127] Specifically, it is the same as step S3A of the first embodiment of the leakage test method and can achieve the same or similar technical effects, so it is not repeated here.
[0128] S5B: Apply voltage to the drain pad 2 and the field plate pad 4 to perform a leakage test.
[0129] Specifically, it is the same as step S4A of the first embodiment of the leakage test method and can achieve the same or similar technical effects, so it will not be repeated.
[0130] S6B: After the leakage test is performed, the source pad 3 is manufactured and the source 6 and the drain 7 are manufactured. The source 6 is connected to the source pad 3 .
[0131] Specifically, after the leakage test is performed, a source pad 3 is made outside the cell area A, and a source 6 and a drain 7 are continuously made inside the cell area A, so that the source 6 is connected to the source pad 3. The source pad 3 and the field plate pad 4 are arranged on the same side of the cell, and the projection of the source pad 3 on the plane where the field plate pad 4 is located at least partially overlaps with the field plate pad 4, and the insulating dielectric layer 9 is located between the field plate pad 4 and the source pad 3 to insulate the field plate pad 4 from the source pad 3. In some embodiments, the projection of the source pad 3 on the plane where the field plate pad 4 is located may completely overlap with the field plate pad 4, or may only partially overlap.
[0132] Specifically, in one embodiment, step S6B is a step of manufacturing the source pad 3 and continuing to manufacture the source 6 and the drain 7 after the leakage test, and the source 6 is connected to the source pad 3, including:
[0133] A second metal layer M2 is formed on the surface of the first gallium nitride preform provided with the first metal layer M1 to form a source 6, a drain 7 and a source pad 3. The source 6 and the source pad 3 are connected through a second wire L2 formed by the first metal layer M1.
[0134] Specifically, the second metal layer M2 may be deposited on the surface of the first gallium nitride preform provided with the first metal layer M1 by evaporation or sputtering, and the second metal layer M2 may be patterned, so that the second metal layer M2 is formed on the first metal layer M1 of the source 6 and the first metal layer M1 of the drain 7 in the cell region A and on the insulating dielectric layer 9 outside the cell region A, and a second wire L2 connecting the first metal layer M1 of the source 6 and the second metal layer M2 on the insulating dielectric layer 9 is formed. The second metal layer M2 on the first metal layer M1 of the source 6 in the cell region A is separated from the second metal layer M2 on the first metal layer M1 of the drain 7, the source metal layer 61 and the first metal layer M1 and the second metal layer M2 provided thereon jointly form the source 6, and the drain metal layer 71 and the first metal layer M1 and the second metal layer M2 provided thereon jointly form the drain 7. The second metal layer M2 on the insulating dielectric layer 9 forms a source pad 3 , and the source pad 3 is connected to the second metal layer M2 of the source 6 through a second wire L2 .
[0135] In some embodiments, the source pad 3 may also include a first metal layer M1. When the source 6, the drain 7 and the drain pad 2 are continuously manufactured on the side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 in step S4B, the first metal layer M1 may also be deposited on the surface of the insulating dielectric layer 9 outside the cell area A at the same time, so that the first metal layer M1 on the insulating dielectric layer 9 is disconnected from the first metal layer M1 of the source 6, the first metal layer M1 of the drain 7 and the first metal layer M1 of the drain pad 2, thereby avoiding Short circuit, the first metal layer M1 on the insulating dielectric layer 9 is used as a part of the source 6, and when the second metal layer M2 is manufactured on the surface of the first gallium nitride preform provided with the first metal layer M1 in step S6B, the second metal layer M2 is formed on the first metal layer M1 on the insulating dielectric layer 9 outside the cell area A, and the source pad 3 is formed by the stacked first metal layer M1 and the second metal layer M2 on the insulating dielectric layer 9, and the second metal layer M2 of the source pad 3 is connected to the second metal layer M2 of the source 6 through the second wire L2.
[0136] In some embodiments, the drain pad 2 may also include a field plate metal layer M3 and a second metal layer M2. When the field plate electrode 8 and the field plate pad 4 are fabricated on one side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 in step S2B, a field plate metal layer M3 disposed spaced apart from the field plate pad 4 may be fabricated outside the cell region A as a part of the drain pad 2. In step S4B, the first metal layer M1 of the drain pad 2 is prepared to cover the surface of the field plate metal layer M3 of the drain pad 2. The drain pad 2 The field plate metal layer M3 is separated from the field plate electrode 8 and the field plate pad. When the second metal layer M2 is produced on the surface of the first gallium nitride preform provided with the first metal layer M1 in step S6B, the second metal layer M2 can be simultaneously formed on the first metal layer M1 of the drain pad 2 outside the cell area A. The drain pad 2 is formed by the stacked field plate metal layer M3, the first metal layer M1 and the second metal layer M2. The first metal layer M1 of the drain pad 2 is connected to the first metal layer M1 of the drain 7 through the third wire L3.
[0137] In other embodiments, the source pad 3 may not include the first metal layer M1, and only include the second metal layer M2, and the drain pad 2 may not include the field plate metal layer M3 and / or the second metal layer M2. For example, the drain pad 2 may include the field plate metal layer M3 and the first metal layer M1, or the drain pad 2 may include the first metal layer M1 and the second metal layer M2, or the drain pad 2 may only include the first metal layer M1. It can be designed as needed, as long as the second metal layer M2 of the source pad 3 and the second metal layer M2 of the source 6 are interconnected to achieve electrical connection between the source pad 3 and the source 6, and the first metal layer M1 of the drain pad 2 and the first metal layer M1 of the drain 7 are interconnected to achieve electrical connection between the drain pad 2 and the drain 7.
[0138] In this embodiment, while the field plate electrode 8 and the field plate pad 4 are fabricated on the side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71 in step S2B, the gate 10 and the gate pad 11 may also be fabricated. Specifically, when the field plate metal layer M3 is fabricated on the side of the first gallium nitride preform provided with the source metal layer 61 and the drain metal layer 71, the field plate electrode 8 and the gate 10 which are spaced apart and disconnected from each other may be formed between the source metal layer 61 and the drain metal layer 71, and the gate pad 11 and the field plate pad 4 which are spaced apart from each other may be formed outside the cell region A, that is, the field plate electrode 8, the gate 10, the gate pad 11, and the field plate pad 4 all include the field plate metal layer M3, but the field plate metal layer M3 of the gate 10 and the gate pad 11 is connected, and the field plate metal layer M3 of the gate 10 and the gate pad 11 is disconnected from the field plate electrode 8 and the field plate metal layer M3 of the field plate pad 4.
[0139] In some embodiments, before preparing the gate 10 and the gate pad 11, a P-type nitride layer (not shown), such as a P-GaN layer, may be deposited on the surface of the semiconductor stack 5, and the P-type nitride may be etched by dry or wet etching to form a cap layer to determine the position of the gate 10 of the E-HEMT device to be prepared, and the active area of the E-HEMT device may be determined by an ion implantation process. After preparing the gate 10, the field plate metal layer M3 of the gate 10 covers the surface of the cap layer away from the semiconductor stack 5.
[0140] In this embodiment, before preparing the first metal layer M1 in step S5B, it is also necessary to deposit a second passivation layer 122, so that the second passivation layer 122 is located on the side of the gate 10 away from the semiconductor stack 5 and covers the gate 10, the field plate electrode 8, the first passivation layer 121 and the semiconductor stack 5, and the second passivation layer 122 is located between the source 6 and the drain 7. Before preparing the second metal layer M2 in step S6B, it is also necessary to deposit a third passivation layer 123, so that the third passivation layer 123 covers the side of the second passivation layer 122 away from the semiconductor stack 5 and is located between the source 6 and the drain 7. Specifically, the first passivation layer 121 or the second passivation layer 122 can be deposited by any one of atomic layer deposition, low pressure chemical vapor deposition, physical vapor deposition and ion enhanced chemical vapor deposition. The main constituent elements of the first passivation layer 121, and / or the second passivation layer 122, and / or the third passivation layer 123 include any one or more of Si, O, Al, and N.
[0141] In this embodiment, the BV electrical property curve of the first gallium nitride preform can be performed by the above method. According to the test results or leakage data, for example, the magnitude of the leakage current, the quality of the field plate electrode 8 and the leakage channel can be monitored, and the main leakage source of the first gallium nitride device 1 can be more accurately determined. The quality and defects of the first passivation layer 121 and the contact surface between the first passivation layer 121 and AlGaN can be monitored to confirm the failure point. At the same time, the following can be prepared: Figure 1 The leakage testing device 100 is shown.
[0142] See also Figure 5 , Figure 5 It is a structural schematic diagram of an embodiment of a semiconductor wafer provided in the present application.
[0143] See also Figure 5The present application also provides a semiconductor wafer 300, which includes multiple device areas 301 and multiple test areas 302. The device area 301 has a second gallium nitride device 200. The second gallium nitride device 200 has the same or similar structure as the first gallium nitride device 1 of the above embodiment, and will not be described in detail here. The test area 302 can be used for process and manufacturing process monitoring. The test area 302 is provided with at least one leakage test device 100. The leakage test device 100 can be used to test whether the second gallium nitride device 200 is leaking and determine the source of the leakage. The leakage test device 100 can be the leakage test device 100 in any of the above embodiments.
[0144] In addition to using the leakage test device 100 to test whether the first gallium nitride device 1 has leakage and the corresponding leakage situation, the semiconductor wafer 300 provided in the present application can also use the leakage test device 100 to characterize whether the second gallium nitride device 200 placed in the semiconductor wafer 300 has leakage and the corresponding leakage situation. In other words, if the first gallium nitride device 1 does not have leakage, it means that the second gallium nitride device 200 does not have leakage and can be used for sale; if the first gallium nitride device 1 has leakage, the leakage position / structure can be promptly identified, so as to achieve leakage improvement (process improvement, etc.) of the second gallium nitride device 200 placed in the semiconductor wafer 300 in the subsequent stage.
[0145] The above descriptions are merely embodiments of the present application and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A leakage test device, characterized in that: include: A first gallium nitride device includes a cell region, wherein a plurality of cells are arranged in the cell region, and each of the cells includes a semiconductor stack and a source electrode, a drain electrode, and a field plate electrode arranged at intervals on one side of the semiconductor stack; A drain pad is disposed outside the cell region and is electrically connected to the drain of each cell; A source pad, disposed outside the cell region and electrically connected to the source of each of the cells; A field plate pad is disposed outside the cell region and is electrically connected to the field plate electrode of each cell; The source pad and the field plate pad are arranged on the same side of the cell, and a projection of the source pad on the plane where the field plate pad is located at least partially overlaps with the field plate pad.
2. The leakage test device according to claim 1, characterized in that: Along the direction away from the cell, the source electrode includes a source metal layer, a first metal layer and a second metal layer which are stacked, and the drain electrode includes a drain metal layer, the first metal layer and the second metal layer which are stacked; the first metal layer and the second metal layer of the source electrode are disconnected from the first metal layer and the second metal layer of the drain electrode; The field plate electrode includes a field plate metal layer, the field plate pad includes the field plate metal layer, and the field plate metal layer of the field plate electrode is connected to the field plate metal layer of the field plate pad; The source pad includes the second metal layer, the second metal layer of the source is connected to the second metal layer of the source pad, and the second metal layer of the drain is disconnected from the second metal layer of the source pad; The drain pad includes the first metal layer. The first metal layer of the drain is connected to the first metal layer of the drain pad, and the first metal layer of the source is disconnected from the first metal layer of the drain pad.
3. The leakage test device according to claim 2, characterized in that: An insulating dielectric layer is disposed between the field plate pad and the source pad.
4. The leakage test device according to claim 3, characterized in that: The source pad further includes a first metal layer, and the drain pad further includes the second metal layer and the field plate metal layer.
5. The leakage test device according to any one of claims 2 to 4, characterized in that: The leakage test device also includes: A gate, the gate being disposed between the source and the field plate electrode, and the field plate electrode being disposed between the gate and the drain; A gate pad is disposed outside the cell region and is electrically connected to the gate of each of the cells; The gate and the gate pad both include the field plate metal layer, the gate and the field plate metal layer of the gate pad are connected, and the gate and the field plate metal layer of the gate pad are disconnected from the field plate electrode and the field plate metal layer of the field plate pad.
6. The leakage test device according to claim 5, characterized in that: The drain pad is connected to the drain electrodes in each cell in the cell region; The gate pad is connected to the gates in each cell in the cell region; The source pad is connected to the source electrodes in each cell in the cell area; The field plate pad is connected to each of the field plate electrodes in each cell.
7. The leakage test device according to claim 6, characterized in that: The field plate electrode is connected to the field plate pad through a first wire formed by the field plate metal layer; The source electrode is connected to the source electrode pad through a second wire formed by the second metal layer; The drain electrode is connected to the drain pad through a third wire formed by the first metal layer; Projections of the first conductive line and the second conductive line on the plane where the field plate pad is located are arranged at an interval.
8. The leakage test device according to claim 5, characterized in that: Each of the cells further comprises: A passivation layer is disposed on the semiconductor stack, and the passivation layer is used to insulate the source, the gate, the field plate electrode and the drain in the cell region.
9. The leakage test device according to claim 1, characterized in that: The semiconductor stack includes a substrate, a buffer layer disposed on the substrate, a first semiconductor layer disposed on the buffer layer, and a second semiconductor layer on the first semiconductor layer, wherein a heterojunction structure is formed between the first semiconductor layer and the second semiconductor layer.
10. A semiconductor wafer, characterized in that: include: A plurality of device regions, each of which has a second gallium nitride device; A plurality of test areas, each of which is provided with at least one leakage test device, wherein the leakage test device is the leakage test device according to any one of claims 1 to 9, and the leakage test device is used to test whether the second gallium nitride device has leakage and determine the source of the leakage.
11. A leakage test method, characterized in that: include: obtaining a first gallium nitride preform; The first gallium nitride preform comprises: a cell region, a plurality of cells are arranged in the cell region, each of the cells comprises a semiconductor stack and a source electrode and a drain electrode spaced apart and arranged on one side of the semiconductor stack; the source electrode comprises a source metal layer, and the drain electrode comprises a drain metal layer; A field plate electrode and a field plate pad are fabricated on one side of the first gallium nitride preform where the source metal layer and the drain metal layer are disposed, wherein the field plate electrode is connected to the field plate pad; The source electrode, the drain electrode and the drain pad are continuously manufactured on the side of the first gallium nitride preform provided with the source metal layer and the drain metal layer, and the drain electrode is connected to the drain pad; A voltage is applied to the drain pad and the field plate pad to perform a leakage test.
12. The leakage testing method according to claim 11, characterized in that: The leakage test method also includes: After the field plate pad is manufactured, before the drain electrode and the drain pad are connected to each other, an insulating dielectric layer is manufactured on the surface of the field plate pad.
13. The leakage testing method according to claim 12, characterized in that: The leakage test method also includes: After the leakage test is performed, a source pad is manufactured and the source and the drain are manufactured, and the source is connected to the source pad; The source pad and the field plate pad are arranged on the same side of the cell, and a projection of the source pad on the plane where the field plate pad is located at least partially overlaps with the field plate pad.
14. The leakage testing method according to claim 13, characterized in that: The step of manufacturing a field plate electrode and a field plate pad on a side of the first gallium nitride preform provided with the source metal layer and the drain metal layer, wherein the field plate electrode and the field plate pad are connected to each other comprises: A field plate metal layer is fabricated on one side of the first gallium nitride preform provided with the source metal layer and the drain metal layer to form the field plate electrode and the field plate pad, wherein the field plate electrode and the field plate pad are connected via a first wire formed by the field plate metal layer; The source electrode, the drain electrode and the drain pad are continuously manufactured on the side of the first gallium nitride preform provided with the source metal layer and the drain metal layer, and the step of connecting the drain electrode and the drain pad comprises: A first metal layer is formed on the surface of the first gallium nitride preform provided with the field plate electrode to form the source electrode, the drain electrode and the drain pad, wherein the drain electrode and the drain pad are connected via a third wire formed by the first metal layer; After the leakage test is performed, the source pad is manufactured and the source and the drain are manufactured, and the steps of connecting the source and the source pad include: A second metal layer is formed on the surface of the first gallium nitride preform provided with the first metal layer to form the source electrode, the drain electrode and the source electrode pad. The source electrode and the source electrode pad are connected through a second wire formed by the second metal layer.
Citation Information
Patent Citations
Structure and process method of IGBT device
CN113571497A
Leakage current measuring structure and measuring method
CN114743953A
Electric leakage testing device, electric leakage testing method and semiconductor wafer
CN117238890A
High-voltage GAN high electron mobility transistors
US20170301781A1
Iii-v semiconductor device
US20230117946A1