Gel-state electrolyte for lithium ion battery as well as preparation method and application of gel-state electrolyte

By using materials such as methyl methacrylate, acrylonitrile, and vinyltrimethoxysilane to prepare a gel electrolyte with a cross-linked network structure in lithium-ion batteries, combined with zinc oxide and N,N-dimethylformamide, It solves the problems of liquid electrolyte safety and mechanical strength, achieves high conductivity and strength while reducing preparation complexity.

CN118748271AActive Publication Date: 2024-10-08NOVEL COSMOS ADVANCED MATERIAL (ANHUI) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411079690.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-08
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The liquid electrolyte of existing lithium-ion batteries has problems such as low safety, easy leakage, and difficulty in inhibiting the growth of lithium dendrites. The room temperature conductivity and mechanical strength of the gel electrolyte are also difficult to meet the ideal effect at the same time.

Method used

Methyl methacrylate, acrylonitrile and vinyl trimethoxysilane are used as cross-linked polymer reaction monomers, and N, N-dimethylformamide is combined with N, N-dimethylformamide through the formation of a cross-linked network structure and grafting reaction with zinc oxide. As a plasticizer solution, a gel-state electrolyte with high room temperature conductivity and excellent mechanical strength was prepared.

Benefits of technology

The gel electrolyte achieves high room temperature conductivity (up to 10.3×10-3S/cm) and mechanical strength (tensile strength up to 2.3MPa), simplifies the preparation process, and reduces the risk of leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004983344780000071
    Figure BDA0004983344780000071
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a gel-state electrolyte for a lithium ion battery as well as a preparation method and application of the gel-state electrolyte. The invention provides a gel-state electrolyte for a lithium ion battery. The gel-state electrolyte comprises a polymer matrix with a cross-linked network structure, a plasticizer, a filler and a lithium salt, the matrix polymer is a cross-linked product of methyl methacrylate, acrylonitrile and vinyltrimethoxysilane, the plasticizer is a mixed solution of N, N-dimethylformamide and at least one of dimethyl carbonate, ethylene carbonate or methyl ethyl carbonate, and the filler is zinc oxide. The gel-state electrolyte can be obtained only through simple free radical polymerization, coating, soaking and other modes, the preparation method is simple and feasible, and large-scale production is easy to achieve. The room-temperature conductivity of the gel-state electrolyte can reach 10.3 * 10 <-3 > S / cm, the tensile strength can reach 2.3 MPa, the liquid absorption rate is greater than 310%, and the application prospect is huge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a gel electrolyte for lithium ion batteries and a preparation method and application thereof. Background Art

[0002] Among the electrolytes used in lithium-ion batteries, liquid electrolytes are widely used in various electronic products and electrical appliances as they have the advantages of high ionic conductivity, good electrode compatibility, wide temperature window, and no heavy metal pollution. However, liquid electrolytes have the problems of low safety, easy leakage of electrolytes, and difficulty in inhibiting the growth of lithium dendrites, which seriously affect the development and application of liquid electrolytes.

[0003] Gel polymer electrolyte, also known as gel electrolyte, is a semi-solid electrolyte mixed with liquid and solid. It is obtained by filling liquid electrolyte into the network structure of polymer molecules. The polymer molecules are cross-linked spatial network structures. The gaps in the network structure are filled with liquid plasticizers, and lithium salts are dissolved in the polymer and plasticizer. Compared with liquid electrolytes, gel electrolytes have the advantages of lower leakage risk, good elasticity and flexibility, and high safety.

[0004] However, the room temperature conductivity and mechanical strength of gel electrolytes still need to be further improved. At present, although there are methods to improve the ionic conductivity of electrolytes by adjusting the ratio of high molecular weight polymers to low molecular weight polymers, or to enhance the mechanical strength and electrochemical stability of electrolytes by adding nanofillers, these methods all have the contradiction that conductivity and mechanical strength cannot be satisfied at the same time, and ideal results cannot be achieved. Summary of the invention

[0005] In view of this, the present invention provides a gel electrolyte for lithium ion batteries and a preparation method and application thereof. The gel electrolyte has high room temperature conductivity, excellent mechanical strength and liquid absorption rate, and the preparation method is simple and feasible.

[0006] To solve the above technical problems, the first aspect of the present invention provides a gel electrolyte for lithium ion batteries, comprising: a polymer matrix with a cross-linked network structure, a plasticizer, a filler and a lithium salt; the matrix polymer is a cross-linked product of methyl methacrylate, acrylonitrile and vinyltrimethoxysilane, the plasticizer is a mixed solution of at least one of dimethyl carbonate, ethylene carbonate or ethyl methyl carbonate and N,N-dimethylformamide, and the filler is zinc oxide.

[0007] The present invention uses methyl methacrylate, acrylonitrile and vinyl trimethoxysilane as reaction monomers to prepare a cross-linked polymer, uses the silicon oxygen bond in vinyl trimethoxysilane as a cross-linking point, and cross-links the molecular chains of polymethyl methacrylate, polyacrylonitrile and their copolymers to form a network structure. In addition to being able to produce a strong interaction with the plasticizer, the carbon oxygen bond in polymethyl methacrylate can also play the role of a plasticizer, reducing the high crystallinity of the polymer brought by rigid acrylonitrile, thereby ensuring that the obtained gel electrolyte has a high room temperature conductivity; in addition to cross-linking polymethyl methacrylate and polyacrylonitrile or its copolymer to obtain a gel electrolyte with a network structure, the oxygen atoms in the silicon oxygen bond that are not involved in the cross-linking can also undergo a grafting reaction with the zinc atoms of the filler, thereby indirectly "connecting" the filler and the polymer in series, destroying the orderly arrangement of the polyacrylonitrile molecular chain, further reducing the polymer crystallinity, and improving the conductivity. In addition, the polymer matrix provided by the present invention has a cross-linked network structure, providing a more stable "framework" structure, and ensuring that the gel electrolyte has excellent mechanical strength.

[0008] In addition, the inventor accidentally discovered during the experiment that when a mixed solution of a certain amount of N,N-dimethylformamide and a traditional plasticizer is used as an electrolyte, the room temperature conductivity of the resulting gel electrolyte is significantly improved.

[0009] In combination with the first aspect, the mass ratio of methyl methacrylate to acrylonitrile is 1:5-10, and the mass ratio of methyl methacrylate to vinyltrimethoxysilane is 1:1-2. The mass ratio within this range can ensure that the gel electrolyte has good conductivity and mechanical properties.

[0010] Preferably, the mass ratio of the methyl methacrylate to acrylonitrile is 1:8, and the mass ratio of the vinyl trimethoxysilane to acrylonitrile is 1:14.

[0011] In combination with the first aspect, the mass ratio of the filler zinc oxide to vinyltrimethoxysilane is 1:3-5.

[0012] In combination with the first aspect, the lithium salt is selected from lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate or lithium trifluoromethylsulfonate. The above lithium salts have good solubility in plasticizers and are easier to "penetrate" into the pores between the molecular chains of the polymer matrix together with the plasticizer.

[0013] In combination with the first aspect, the mass proportion of N,N-dimethylformamide in the plasticizer is 15% to 30%. N,N-dimethylformamide in this ratio range can ensure that the obtained gel electrolyte has both high room temperature conductivity and good mechanical strength.

[0014] A second aspect of the present invention provides a method for preparing a gel electrolyte for a lithium ion battery, the steps comprising:

[0015] S1, adding an initiator to the mixed solution of methyl methacrylate, acrylonitrile and vinyltrimethoxysilane, stirring and dissolving, to obtain a first solution;

[0016] S2. Under inert conditions, the first solution is added dropwise to a 65-80° C. aqueous solution containing a dispersant, and the polymerization reaction is carried out while stirring. After the reaction is completed, the pH of the solution is adjusted to 8-9, and a filler zinc oxide is added. The mixture is stirred at the same temperature for 2-5 hours, and filtered to obtain an electrolyte precursor.

[0017] S3. Under inert conditions, the electrolyte precursor is dissolved in an organic solvent, and a flat film is applied. After the film is solidified, the film is immersed in a plasticizer containing a lithium salt for 15 to 30 minutes to obtain the gel electrolyte.

[0018] The present invention uses a simple free radical polymerization reaction to react methyl methacrylate, acrylonitrile and vinyl trimethoxysilane to generate a cross-linked polymer with a network structure, and then prepares a gel electrolyte by dissolving and casting. The steps are simple and easy to implement, and batch production is easy to achieve.

[0019] In combination with the second aspect, the concentration of the lithium salt in the plasticizer is 0.8 to 1 mol / L.

[0020] In combination with the second aspect, the mass proportion of the electrolyte precursor in the organic solvent is 10% to 30%.

[0021] Preferably, the initiator is dibenzoyl peroxide.

[0022] A third aspect of the present invention provides a lithium ion battery prepared using the above-mentioned gel electrolyte.

[0023] Beneficial effects of the present invention: The present invention provides a gel electrolyte with a cross-linked network structure. By ingeniously improving the electrolyte components and preparation methods, a high room temperature conductivity (up to 10.3×10 -3 S / cm), excellent mechanical strength (tensile strength can reach up to 2.3MPa), and gel electrolyte with liquid absorption rate greater than 310%. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] Polymethyl methacrylate is a chemically stable, colorless, transparent amorphous polymer with high liquid electrolyte absorption and excellent interfacial compatibility with lithium metal. However, its film-forming ability is poor, resulting in poor mechanical strength of the resulting film. Some studies have prepared polymer films by copolymerizing and cross-linking methyl methacrylate and acrylonitrile, and then obtaining a gel electrolyte by absorbing an electrolyte containing lithium salts, but the room temperature conductivity of the obtained gel electrolyte is still at a low level.

[0026] In this regard, the present invention provides a gel electrolyte. By improving the components and preparation method of the electrolyte, a gel electrolyte with significantly improved room temperature conductivity and still good mechanical strength is obtained, which has great practical application value.

[0027] The purity of each monomer used in the following examples is at least 99.98%.

[0028] Example 1

[0029] This embodiment provides a gel electrolyte for lithium ion batteries, which is prepared according to the following method:

[0030] S1. Accurately weigh 5.0 g of methyl methacrylate, 35.0 g of acrylonitrile and 7.5 g of vinyltrimethoxysilane, mix them evenly, then add 2.2 g of dibenzoyl peroxide, stir and dissolve, to obtain a first solution;

[0031] S2. Under the protection of inert gas, the first solution was slowly added dropwise to a 100 mL 75° C. aqueous solution containing 4.5 g of gelatin, and the polymerization reaction was carried out at a speed of 400 r / min for 6 h. After the reaction, the pH of the solution was adjusted to 8-9 with a sodium hydroxide solution, 2 g of zinc oxide was added, and the mixture was stirred at the same temperature for 3.5 h, filtered, and dried to obtain an electrolyte precursor having a cross-linked network structure;

[0032] S3. Under the protection of inert gas, 30g of electrolyte precursor was dissolved in 100g of N,N-dimethylformamide, and then applied to the surface of glass plate or polytetrafluoroethylene plate, and dried at 50℃ for 6h after film formation. Then the obtained film was immersed in 300g of plasticizer (including 25g of N,N-dimethylformamide and 225g of dimethyl carbonate) with a concentration of 0.9mol / L of lithium bis(trifluoromethylsulfonyl)imide for 20min, and taken out to obtain a gel electrolyte with a thickness of 32μm.

[0033] Example 2

[0034] This embodiment provides a gel electrolyte for lithium ion batteries, which is prepared according to the following method:

[0035] S1. Accurately weigh 5.0 g of methyl methacrylate, 25.0 g of acrylonitrile and 5.0 g of vinyltrimethoxysilane, mix them evenly, add 1.4 g of dibenzoyl peroxide, stir and dissolve, to obtain a first solution;

[0036] S2. Under the protection of inert gas, the first solution was slowly added dropwise to a 35 mL 65° C. aqueous solution containing 3.2 g of gelatin, and the polymerization reaction was carried out at a speed of 400 r / min for 7 hours. After the reaction, the pH of the solution was adjusted to 8-9 with a sodium hydroxide solution, 1.3 g of zinc oxide was added, and the mixture was stirred at the same temperature for 5 hours, filtered, and dried to obtain an electrolyte precursor having a cross-linked network structure;

[0037] S3. Under the protection of inert gas, 20g of electrolyte precursor was dissolved in 75g of N,N-dimethylformamide, and then applied to the surface of glass plate or polytetrafluoroethylene plate, and dried at 50℃ for 6h after film formation. Then the obtained film was immersed in 70g of plasticizer (including 8g of N,N-dimethylformamide and 62g of ethylene carbonate) with a concentration of 0.8mol / L of lithium difluorooxalate borate for 15min, and taken out to obtain a gel electrolyte with a thickness of 29μm.

[0038] Example 3

[0039] This embodiment provides a gel electrolyte for lithium ion batteries, which is prepared according to the following method:

[0040] S1. Accurately weigh 5.0 g of methyl methacrylate, 50.0 g of acrylonitrile and 10.0 g of vinyltrimethoxysilane, mix them evenly, add 3.4 g of dibenzoyl peroxide, stir and dissolve, to obtain a first solution;

[0041] S2. Under the protection of inert gas, the first solution was slowly added dropwise to a 160 mL 80° C. aqueous solution containing 5.9 g of gelatin, and the polymerization reaction was carried out at a speed of 400 r / min for 5 h. After the reaction, the pH of the solution was adjusted to 8-9 with a sodium hydroxide solution, 3 g of zinc oxide was added, and the mixture was stirred at the same temperature for 2 h, filtered, and dried to obtain an electrolyte precursor having a cross-linked network structure;

[0042] S3. Under the protection of inert gas, 45g of electrolyte precursor was dissolved in 300g of N,N-dimethylformamide, and then applied to the surface of glass plate or polytetrafluoroethylene plate, and dried at 50℃ for 6h after film formation. Then the obtained film was immersed in 205g of plasticizer (including 20g of N,N-dimethylformamide and 185g of ethyl methyl carbonate) with a concentration of 1mol / L of lithium bis(fluorosulfonyl)imide for 30min, and taken out to obtain a gel electrolyte with a thickness of 38μm.

[0043] Comparative Example 1

[0044] This comparative example provides a gel electrolyte for lithium ion batteries, the composition and preparation method of which are basically similar to those of Example 1, the only difference being that vinyltrimethoxysilane is replaced by an equimolar amount of polyethylene glycol dimethacrylate, and the rest of the preparation method is the same as that of Example 1. The thickness of the obtained gel electrolyte is 35 μm.

[0045] Comparative Example 2

[0046] This comparative example provides a gel electrolyte for lithium ion batteries, and its composition and preparation method are basically similar to those of Example 1, except that in step S2, after the polymerization reaction is completed, pH adjustment and zinc oxide addition are not performed, and filtering and drying steps are directly performed to obtain an electrolyte precursor in which the polymer chain is not grafted with zinc oxide. Steps S1 and S3 are the same as those of Example 1, and the thickness of the obtained gel electrolyte is 29 μm.

[0047] Comparative Example 3

[0048] This comparative example provides a gel electrolyte for lithium ion batteries, the composition and preparation method of which are basically similar to those of Example 1, the only difference being that the plasticizer used in step S3 does not contain N,N-dimethylformamide, and the remaining steps are the same as those of Example 1. The thickness of the obtained gel electrolyte is 33 μm.

[0049] Test Example 1

[0050] The tensile strength tests were performed on the gel electrolytes obtained in Examples 1 to 3 and Comparative Examples 1 to 3 (the length and width of the test samples were 20 mm and 12.5 mm, respectively, and the stretching rate was 12 mm / min), and the results are shown in Table 1. It can be seen that the tensile strengths of the gel electrolytes obtained in Examples 1 to 3 were all above 2.0 MPa; and from the results of Comparative Example 1, it can be seen that when the cross-linking agent used is a polymer with a certain length, the tensile strength of the gel electrolyte obtained is reduced.

[0051] Test Example 2

[0052] The gel electrolytes obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to AC impedance tests at room temperature to test their conductivity. The results are shown in Table 1.

[0053] Table 1

[0054]

[0055] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A gel electrolyte for lithium ion batteries, characterized in that: include: A polymer matrix with a cross-linked network structure, a plasticizer, a filler and a lithium salt; the matrix polymer is a cross-linked product of methyl methacrylate, acrylonitrile and vinyl trimethoxysilane, the plasticizer is a mixed solution of at least one of dimethyl carbonate, ethylene carbonate or ethyl methyl carbonate and N, N-dimethylformamide, and the filler is zinc oxide.

2. The gel electrolyte for lithium ion battery according to claim 1, characterized in that: The mass ratio of the methyl methacrylate to acrylonitrile is 1:5-10, and the mass ratio of the methyl methacrylate to vinyl trimethoxy silane is 1:1-2.

3. The gel electrolyte for lithium ion battery according to claim 1, characterized in that: The mass ratio of the filler zinc oxide to vinyltrimethoxysilane is 1:3-5.

4. The gel electrolyte for lithium ion battery according to claim 1, characterized in that: The lithium salt is selected from lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate or lithium trifluoromethylsulfonate.

5. The gel electrolyte for lithium ion battery according to claim 1, characterized in that: The mass proportion of the N,N-dimethylformamide in the plasticizer is 15% to 30%.

6. A method for preparing a gel electrolyte for a lithium ion battery, characterized in that the steps include: S1, adding an initiator to the mixed solution of methyl methacrylate, acrylonitrile and vinyltrimethoxysilane, stirring and dissolving, to obtain a first solution; S2. Under inert conditions, the first solution is added dropwise to a 65-80° C. aqueous solution containing a dispersant, and the polymerization reaction is carried out while stirring. After the reaction is completed, the pH of the solution is adjusted to 8-9, and a filler zinc oxide is added. The mixture is stirred at the same temperature for 2-5 hours, and filtered to obtain an electrolyte precursor having a cross-linked network structure. S3. Under inert conditions, the electrolyte precursor is dissolved in an organic solvent, and a flat film is applied. After the film is solidified, the film is immersed in a plasticizer containing a lithium salt for 15 to 30 minutes to obtain the gel electrolyte.

7. The method for preparing a gel electrolyte for a lithium ion battery according to claim 6, characterized in that: The concentration of the lithium salt in the plasticizer is 0.8-1 mol / L.

8. The method for preparing a gel electrolyte for a lithium ion battery according to claim 6, characterized in that: The mass proportion of the electrolyte precursor in the organic solvent is 10% to 30%.

9. A lithium ion battery, characterized in that: The gel electrolyte is prepared by using the gel electrolyte described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Auto-doped gel polymer electrolyte and preparation method thereof

    CN104485480A

  • Organic / inorganic crosslinked composite lithium-ion battery diaphragm and preparation method and application thereof

    CN109473609A

  • Low-temperature polymerized gel electrolyte and battery containing same

    CN116169353A

  • Branched polyhydroxyalkanoate polymer salt electrolytic compositions and method of preparation

    US5266422A

  • Composite diaphragm and preparation method therefor, and lithium-ion battery

    WO2015196854A1