High-voltage cable fixing clamp

By using aluminum alloy components in high-voltage cable clamps and performing phosphoric acid anodizing and sealing treatments, the corrosion problem of the cable clamps in humid environments is solved, and the corrosion resistance and service life are improved.

CN118748377APending Publication Date: 2024-10-08HONGQI GRP ELECTRIC POWER FITTINGS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410777225.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

High-voltage cable fixed clamps are prone to corrosion due to accumulated water in underground cable tunnels in coastal areas, resulting in shortened service life. In addition, the creeping and thermal expansion and contraction effects of large currents on the fixed clamps increase the clamping force, making the clamping parts resistant to corrosion. Insufficient sex.

Method used

The fixed clip alloy component is made of aluminum alloy, with added Mg element to reduce electrochemical corrosion, low content of Fe to prevent the formation of bulk compound phases, and introduction of Sr, Zr, Cu, and Zn to adjust the metallographic distribution, combined with phosphoric acid anodizing treatment and sealing treatment to form a dense film layer to improve corrosion resistance.

Benefits of technology

Significantly improves the corrosion resistance and service life of high-voltage cable clamps in humid environments, ensuring improved clamping force and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748377A_ABST
    Figure CN118748377A_ABST
Patent Text Reader

Abstract

The invention discloses a high-voltage cable fixing clamp which comprises an alloy component, the alloy component comprises a base and a gland, the base and the gland comprise 7.2 wt%-7.5 wt% of Si, 0.40 wt%-0.45 wt% of Mg, 0.18 wt%-0.20 wt% of Ti, 0.03 wt%-0.05 wt% of Fe, 0.07 wt%-0.10 wt% of Cu, 0.07 wt%-0.15 wt% of Zr, 0.004 wt%-0.008 wt% of Sr, 0.006 wt%-0.008 wt% of Zn and the balance aluminum, and the alloy component has excellent corrosion resistance, so that the service life of the alloy component of the high-voltage cable fixing clamp in an underground humid environment and a soaking environment is long.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of high voltage power transmission, and in particular to a high voltage cable fixing clamp. Background Art

[0002] High-voltage cable clamps are devices for fixing high-voltage and high-current power cables. They are used to fix the correct position of underground power cables after laying and installation to prevent the movement of cables due to their own weight or other external forces.

[0003] With the increase of power supply in cities and the continuous improvement of various voltage levels, the larger the cross-section of cables, the larger the current flowing in the conductor, and the more obvious the impact of current on cable installation and fixation. When the load current of the cable changes, the temperature of the conductor inside the cable will change, causing the cable to expand or contract. The heat expansion of the cable will produce an outward expansion thrust on the clamping part of the high-voltage cable clamp, and the axial length change of the cable due to thermal expansion and contraction will produce axial pulling on the clamping part of the high-voltage cable clamp. In addition, cables with large currents are prone to creeping during daily use due to large currents, and huge short-circuit electric forces are generated when overloaded under electric short circuits. The force of such cables on the high-voltage cable clamp is increasingly greater on high-voltage cables with large currents. Therefore, high-strength aluminum alloys are often used to prepare the clamping parts of the cable clamp to ensure that the high-voltage cable clamp has sufficient grip to fix high-voltage cables with large currents.

[0004] During the application process, it was found that due to waterlogging, underground cable corridors in coastal areas are prone to waterlogging, and cable clamps are easily immersed in water. Under long-term work, harmful elements such as Fe in the alloy components of the cable clamps react with chlorine-containing impurities in the water, corroding the aluminum alloy and reducing the service life of the product. Summary of the invention

[0005] In order to extend the service life of a high-voltage cable fixing clamp in an underground cable corridor in a coastal area, a high-voltage cable fixing clamp is provided.

[0006] The above-mentioned first invention object of the present invention is achieved through the following technical solutions: A high-voltage cable fixing clamp comprises an alloy component, wherein the alloy component comprises a base and a gland made of an aluminum alloy, wherein the aluminum alloy comprises 7.2-7.5wt% Si, 0.40-0.45wt% Mg, 0.18-0.20wt% Ti, 0.03-0.05wt% Fe, 0.07-0.10wt% Cu, 0.07-0.15wt% Zr, 0.004-0.008wt% Sr, 0.006-0.008wt% Zn, and the remainder is aluminum.

[0007] By adopting the above technical solution, the content of Mg element in the alloy component is high, and electrochemical corrosion is not easy to occur in the corrosive medium; the electrode potential of Mg2Al3 is lower than that of the matrix Al. In the corrosive medium, the aluminum matrix is ​​formed as the cathode and Mg2Al3 is formed as the anode. When Mg2Al3 is corroded, a single aluminum solid solution is formed on the surface of the casting, thereby interrupting the corrosion; Furthermore, the content of Fe element is low, and no large Fe-containing compound phase will be formed. The alloy crystal phase is uniform and has strong corrosion resistance. In addition, alloy materials are different from other composite materials, in which the type and content of alloy elements will affect the metallographic distribution and alloy composition in the alloy. The present application further introduces Sr, Zr, Cu, and Zn on the basis of aluminum-magnesium alloy to adjust the alloy composition and metallographic phase; Therefore, the alloy component of the cable fixing clamp of the present application has excellent corrosion resistance.

[0008] Optionally, the alloy component has an anodized film on the outside, and the anodized film is obtained by surface anodizing treatment; the electrolyte used for the surface anodizing treatment is a phosphoric acid solution, and the phosphoric acid concentration is 6.4-8.3wt%.

[0009] By adopting the above technical solution, only phosphoric acid is used as the electrolyte for anodizing treatment. In the later stage of anodizing - when the thickness of the anodized film increases and holes are formed in the anodized film, H + The concentration should decrease due to loss and increased difficulty in migration; Aluminum ions and phosphates react at the bottom of the hole to form aluminum phosphate. In the absence of other organic cations, anions, and impurities, the aluminum phosphate will be formed in a dense deposition to fill the hole from the bottom to the outside, thereby reducing the depth of the anodic oxide film and increasing the thickness of the dense film layer. The filling process is carried out directly after the anodized film is formed. The deposited aluminum phosphate is more tightly bonded to the hole wall than the sealing agent, which significantly improves the corrosion resistance of the alloy component of the cable clamp, thereby extending the service life of the high-voltage cable clamp in underground humid environments and immersion environments.

[0010] Optionally, during the surface anodizing treatment, the DC voltage passed through the alloy component is 15 to 20 V, and the treatment time is 20 to 32 minutes.

[0011] By adopting the above technical solution, the anodized film is formed evenly with fewer leak holes. At the same time, the aluminum phosphate deposition in the holes of the anodized film is more densely bonded and has a greater deposition depth, and the alloy component of the cable clamp has better corrosion resistance.

[0012] Optionally, the alloy component is also immersed in a sealing treatment liquid for sealing treatment and forms an outer sealing film.

[0013] By adopting the above technical solution, the anodized film formed on the alloy component of the cable clamp after anodizing treatment uses phosphoric acid as an electrolyte to fill the holes, but the filling depth is difficult to achieve complete filling. Sealing the anodized film can further improve the corrosion resistance of the alloy component of the cable clamp.

[0014] Optionally, the sealing treatment solution includes an initial solution after pre-hydrolysis and alcoholysis, wherein the initial solution comprises methyltriethoxysilane and polyethylene glycol. The relative average molecular weight of the polyethylene glycol is 200, and the relative molecular weight distribution is 150 to 250; The methyltriethoxysilane accounts for 10-20 wt % in the initial solution, and the polyethylene glycol accounts for 13-24 wt % in the initial solution.

[0015] Optionally, the methyltriethoxysilane accounts for 20 wt % in the initial solution, and the polyethylene glycol accounts for 24 wt % in the initial solution.

[0016] By adopting the above technical scheme, silane and polyethylene glycol are used as the source of sealing components, and low relative molecular weight polyethylene glycol is used as a co-solvent for methyltriethoxysilane. At the same time, under the control of the relative molecular weight of polyethylene glycol in the present application, when methyltriethoxysilane is hydrolyzed, part of the polyethylene glycol also reacts with silane to cause its alcoholysis, and the polyethylene glycol is connected to the silane precondensate, which has better affinity for the anodized film, good sealing effect, better toughness and coverage of the resulting film layer, and improved corrosion resistance.

[0017] In addition, methyltriethoxysilane and polyethylene glycol as sources of sealing components are more environmentally friendly than chromate sealing agents.

[0018] Optionally, the sealing treatment liquid also includes ammonium acetate, and the ammonium acetate accounts for 2.4-3.1 wt %.

[0019] By adopting the above technical solution, the pH of the sealing treatment liquid will reduce the sealing density, and the addition of ammonium acetate can serve as a pH buffer to reduce the impact of residual phosphoric acid in the pores of the anodized film, thereby improving the sealing effect and enhancing the corrosion resistance of the alloy components of the cable clamp.

[0020] Optionally, the sealing treatment liquid also includes sodium sulfite, and the sodium sulfite accounts for 0.28-0.36wt%.

[0021] By adopting the above technical scheme, since the alloy component is composed of alloy, there are inevitably other metal ions remaining in the pores of the anodized film, among which iron ions have a great influence on the sealing of the pores. After immersion in the sealing treatment liquid, the acidity of the environment decreases, and the iron ions are easily converted into non-dense precipitates, thereby reducing the sealing density or hindering the sealing. Therefore, sodium sulfite is added to reduce the iron ions to ferrous ions, thereby avoiding their precipitation during the sealing process, thereby improving the sealing effect.

[0022] In summary, this application has at least the following beneficial effects: 1. Optimize the composition of the alloy components of the cable clamp. The alloy components are electrochemically corroded in a humid environment. They contain less Fe compound phase, and the alloy crystal phase is uniform and has strong corrosion resistance, so that the high-voltage cable clamp has a long service life in underground humid environments and immersion environments.

[0023] 2. Only phosphoric acid is used as the electrolyte for anodizing treatment to form an anodized film with a dense film layer thickness and small hole depth, which significantly improves the corrosion resistance of the alloy components of the cable clamp; 3. Methyltriethoxysilane, polyethylene glycol with a specific relative molecular weight, ammonium acetate, and sodium sulfite are compounded to form an initial solution, and then treated to obtain a sealing solution for sealing the alloy components of the cable clamp after anodization, forming a dense sealing layer on the surface of the anodized film, thereby improving the corrosion resistance of the alloy components of the cable clamp. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 It is a schematic diagram of the base and gland structure; Figure 2 Exploded view of the cable clamp.

[0025] Reference numerals: 1. Base; 11. Lower clamping block; 12. Fixed block; 2. Pressure cover; 21. Upper clamping block; 3. Notch; 4. Connector. DETAILED DESCRIPTION

[0026] The present application is further described in detail below in conjunction with the accompanying drawings.

[0027] raw material: Polyethylene glycol is polyethylene glycol with a relative average molecular weight lower than 1000. In the following examples, polyethylene glycol has two specifications: Polyethylene glycol, relative average molecular weight is 200, relative molecular weight distribution is 150-250; Polyethylene glycol, relative average molecular weight is 400, and relative molecular weight distribution is 350-450.

[0028] Other raw materials not otherwise specified are commercially available products.

[0029] Example 1 As attached Figure 1 As shown, a high-voltage cable fixing clamp comprises a base 1 and a gland 2.

[0030] The base 1 and the gland 2 are alloy components. The facing surfaces of the base 1 and the gland 2 are concave to form an arc-shaped notch 3, and the notch 3 is used to hold the cable tightly.

[0031] The base 1 has lower clamping blocks 11 extending from both sides of the notch 3, and the gland 2 has upper clamping blocks 21 extending from both sides of the notch 3. When the base 1 and the gland 2 hold the cable tightly, the upper clamping blocks 21 are aligned with the lower clamping blocks 11.

[0032] At the same time, a fixing block 12 is extended from the outer side of the base 1 facing away from the gland 2. The fixing block 12 has a hole or a groove, and the base 1 is fixed to a wall, a cable rack or other fixed body through other installation components, which is an open groove here.

[0033] The base 1 and the gland 2 are made of aluminum alloy, which are obtained by smelting and refining aluminum ingots and alloy ingots, pouring, and low-pressure casting. The alloy components in this embodiment are prepared from the same batch of aluminum alloys and tested for composition, specifically Si 7.2wt%, Mg 0.43wt%, Ti0.20wt%, Fe 0.04wt%, Cu 0.07wt%, Zr 0.1wt%, Sr 0.004wt%, Zn 0.007wt%, and the balance is aluminum.

[0034] As attached Figure 2 As shown, the high-voltage cable fixing clamp also includes a connecting member 3, which is used to connect the upper clamping block 21 and the lower clamping block 11. The connecting member 3 can be a clamp, a clip or a bolt assembly, and here it is a bolt assembly and the number is two.

[0035] The bolt assembly includes a bolt and a nut. The bolt passes through a set of upper clamping blocks 21 and lower clamping blocks 11 and is threadedly connected with the nut to clamp the base 1 and the gland 2 to clamp the cable.

[0036] The connecting member 3 can be an alloy component of the same type as the base 1 and the gland 2 and can be produced from the same batch of aluminum alloy according to application requirements.

[0037] The high-voltage cable fixing clamp of this embodiment has good corrosion resistance and long service life in underground humid environment and immersion environment.

[0038] Example 2 A high-voltage cable fixing clamp, which is different from Example 1 in that the alloy component of the high-voltage cable fixing clamp is prepared from the same batch of aluminum alloy and its composition is tested, and the specific composition is Si 7.5wt%, Mg 0.4wt%, Ti 0.18wt%, Fe 0.05wt%, Cu 0.10wt%, Zr 0.07wt%, Sr 0.004wt%, Zn 0.006wt%, and the balance is aluminum.

[0039] Example 3 A high-voltage cable fixing clamp, which is different from Example 1 in that the alloy component of the high-voltage cable fixing clamp is prepared from the same batch of aluminum alloy and its composition is tested, and the specific composition is Si 7.4wt%, Mg 0.45wt%, Ti 0.18wt%, Fe 0.03wt%, Cu 0.08wt%, Zr 0.15wt%, Sr 0.006wt%, Zn 0.008wt%, and the balance is aluminum.

[0040] Comparative Example 1 A high-voltage cable fixing clamp, the alloy component of which is made by melting and casting commercially available aluminum-magnesium alloy 5052.

[0041] The aluminum alloy materials of the alloy components of Examples 1 to 3 and Comparative Example 1 were tested for tensile strength and corrosion resistance.

[0042] The tensile strength is tested by tensile testing machine. The gripping force of the cable clamp on the cable is composed of the tensile resistance of the alloy components of the clamp and other parts. Therefore, the contribution of the alloy components to the gripping force of the cable clamp is determined by the shape and material properties of the alloy components. In this application, when comparing the contribution of the alloy components of the cable clamp to the gripping force of the cable clamp, in order to reduce the error of the shape in the display and detection of material properties, the tensile strength test is performed on strip specimens. The greater the tensile strength, the greater the contribution to the gripping force of the cable clamp.

[0043] The corrosion resistance test is carried out according to GB / T 10125 neutral salt spray environment test. The 100mm×100mm×10mm aluminum alloy plate cast from the same batch of aluminum alloy is used as the specimen, and the result is expressed in salt spray resistance time.

[0044] The test results are shown in Table 1 below.

[0045] Table 1. Test results of Examples 1 to 3 and Comparative Example 1 Tensile strength / MPa Neutral salt spray corrosion damage time / h Example 1 376 529 Example 2 354 508 Example 3 377 517 Comparative Example 1 276 212 From Table 1, it can be seen that the alloys used in the alloy components of Examples 1 to 3 have a high content of Mg element, and are not prone to electrochemical corrosion in corrosive media. The electrode potential of Mg2Al3 is lower than that of the matrix Al. In the corrosive medium, the aluminum matrix is ​​formed as the cathode and Mg2Al3 is formed as the anode. When Mg2Al3 is corroded, a single aluminum solid solution is formed on the surface of the casting to interrupt the corrosion. Furthermore, the content of Fe element is low, and no large Fe-containing compound phase is formed. The alloy crystal phase is uniform and has strong corrosion resistance. In addition, alloy materials are different from other composite materials, and the type and content of alloy elements will affect the metallographic distribution and alloy composition in the alloy. The present application further introduces Sr, Zr, Cu, and Zn on the basis of aluminum-magnesium alloy to adjust the alloy composition and metallographic phase, so that the alloy components have excellent corrosion resistance.

[0046] Therefore, the neutral salt spray corrosion damage time of Examples 1 to 3 is significantly better than that of the alloy component made of aluminum alloy 5052 in Comparative Example 1.

[0047] At the same time, the tensile strength of Examples 1 to 3 is significantly better than that of Comparative Example 1. Aluminum alloy 5052 is an outdoor building decoration alloy, and its selection targets in daily building materials are light weight and corrosion resistance. Examples 1 to 3 have better corrosion resistance than aluminum alloy 5052 and high strength performance that aluminum alloy 5052 does not have. Therefore, Examples 1 to 3 can be used for matching high-voltage cable fixing clamps and are corrosion-resistant and have a long service life.

[0048] Example 4 A high-voltage cable fixing clamp is different from the embodiment 1 in that the alloy component is also anodized to form an anodized film on the surface.

[0049] The steps of anodizing are as follows: The alloy component of Example 1 was washed with water to remove oil stains, and then ultrasonically cleaned at 42kHz for 30 minutes to obtain a pre-treated component. The pre-treated component was used as an anode and connected to direct current and immersed in an electrolyte for anodizing treatment. The electrolyte was a 7wt% phosphoric acid solution, the DC voltage was 15V, and the treatment time was 32 minutes. The residual liquid on the surface of the pre-treated part after anodizing treatment is removed and cleaned to obtain an alloy component of the cable fixing clamp after anodizing treatment.

[0050] Example 5 A high-voltage cable fixing clamp, which differs from Example 4 in that the concentration of the phosphoric acid solution is 4.1 wt %.

[0051] Example 6 A high-voltage cable fixing clamp, which differs from Example 4 in that the concentration of the phosphoric acid solution is 6.4 wt %.

[0052] Example 7 A high-voltage cable fixing clamp, which differs from Example 4 in that the concentration of the phosphoric acid solution is 8.3 wt %.

[0053] Example 8 A high-voltage cable fixing clamp, which differs from Example 4 in that the electrolyte is 7wt% sulfuric acid.

[0054] Example 9 A high-voltage cable fixing clamp is different from Example 4 in that the electrolyte is a mixed solution of tartaric acid and phosphoric acid, wherein the concentration of tartaric acid is 1.4wt% and the concentration of phosphoric acid is 7wt%.

[0055] Example 10 A high-voltage cable fixing clamp, which differs from Example 4 in that the DC voltage during anodizing treatment is 15V and the treatment time is 20 minutes.

[0056] Embodiment 11 A high-voltage cable fixing clamp, which differs from Example 4 in that the DC voltage during anodizing treatment is 15V and the treatment time is 25 minutes.

[0057] Example 12 A high-voltage cable fixing clamp, which differs from Example 4 in that the DC voltage during anodizing treatment is 20V and the treatment time is 20 minutes.

[0058] Embodiment 13 A high-voltage cable fixing clamp, which differs from Example 4 in that the DC voltage during anodizing treatment is 20V and the treatment time is 35 minutes.

[0059] Embodiment 14 A high-voltage cable fixing clamp is different from Example 4 in that the alloy component after anodizing is also subjected to a sealing treatment, the holes of the anodized film are repaired, and a sealing film is formed outside the anodized film.

[0060] The sealing process steps are as follows: The anodized alloy component obtained in Example 4 was immersed in the sealing treatment solution for 2 minutes; After immersion, the alloy components were taken out, dried under ventilation at room temperature, kept at 90°C for 1 hour, and then air-cooled to room temperature to obtain the alloy components after sealing treatment.

[0061] The steps for obtaining the sealing treatment liquid are as follows: Mixing methyltriethoxysilane, polyethylene glycol and water to obtain an initial solution, wherein methyltriethoxysilane accounts for 20wt% and polyethylene glycol accounts for 24wt%; The initial solution was stirred at 10 r / min for 2 h at 28° C., and then ammonium acetate and sodium sulfite were added to obtain a sealing treatment solution, in which ammonium acetate accounted for 3.1 wt % and sodium sulfite accounted for 0.36 wt %.

[0062] The relative average molecular weight of polyethylene glycol is 200, and the relative molecular weight distribution is 150-250.

[0063] Embodiment 15 A high-voltage cable fixing clamp, which differs from Example 14 in that the proportion of methyltriethoxysilane in the initial liquid is 10wt%, and the proportion of polyethylene glycol is 13wt%.

[0064] Example 16 A high-voltage cable fixing clamp, which differs from Example 14 in that the specification of polyethylene glycol is different, and the relative average molecular weight of the polyethylene glycol is 400 and the relative molecular weight distribution is 350-450.

[0065] Embodiment 17 A high-voltage cable fixing clamp, which differs from Example 14 in that the sealing treatment liquid comprises 2.4wt% of ammonium acetate and 0.28wt% of sodium sulfite.

[0066] Embodiment 18 A high-voltage cable fixing clamp, which differs from Example 14 in that the amount of ammonium acetate used in the sealing treatment liquid is 0.

[0067] Embodiment 19 A high-voltage cable fixing clamp, which differs from Example 14 in that the amount of sodium sulfite used in the sealing treatment liquid is 0.

[0068] The corrosion resistance test was carried out on Examples 4 to 19, and the results are recorded in Table 2.

[0069] Since the corrosion resistance of Examples 4 to 19 is improved after the formation of the anodized film, the corrosion resistance test was carried out according to the "GB / T42514-2023 Corrosion Assessment Chart Method for Aluminum and Aluminum Alloy Anodized Films and Organic Polymer Films", using neutral salt spray for 1240 hours, and the corrosion point detection was carried out, and the sample prepared with the aluminum alloy used in Example 1 was used as a blank control.

[0070] The results are expressed in terms of protection levels of 0 to 10 in the corrosion rating chart method for anodized films and organic polymer films of aluminum and aluminum alloys in GB / T 42514-2023. From "0" to "10", the number of corrosion spots decreases, indicating better corrosion resistance for the sample.

[0071] Table 2. Test results of Examples 4 to 19 and blank examples Corrosion grade-protection grade Corrosion grade-protection grade Example 4 7 Embodiment 13 6* Example 5 5 Embodiment 14 10 Example 6 7 Embodiment 15 9 Example 7 7 Example 16 8 Example 8 4 Embodiment 17 10 Example 9 5 Embodiment 18 9 Example 10 6 Embodiment 19 9 Embodiment 11 7 Blank example 0 Example 12 7 * Compared with Examples 4 to 12, the surface color of the sample of Example 13 (before testing) is significantly darker and the roughness can be clearly felt by hand.

[0072] Combined with Table 2, by comparing Examples 4 to 9 and the blank example, it can be seen that an anodic oxide film is formed on the surface of the alloy component of the high-voltage cable fixing clamp of the present application after anodizing treatment, and the corrosion resistance of the alloy component is significantly improved, so that the protection level of Examples 4 to 9 is significantly increased compared with the blank example.

[0073] Further comparing Examples 4 to 8, the protection levels of Examples 4, 6, and 7 are significantly greater than those of Examples 5, 8, and 9.

[0074] The reason why Examples 4, 6, and 7 are significantly greater than Examples 8 and 9 is that the electrolytes used for anodizing treatment in Examples 4, 6, and 7 are phosphoric acid solutions without other acids, while that in Example 8 is sulfuric acid, and that in Example 9 is a composite solution of phosphoric acid and tartaric acid.

[0075] In Examples 4, 6, and 7, only phosphoric acid was used as the electrolyte for anodization treatment. In the later stage of anodization, when the thickness of the anodized film increased and holes were formed in the anodized film, the H + The concentration should decrease due to loss and increased difficulty of migration; aluminum ions and phosphates react at the bottom of the pores to form aluminum phosphate. In the absence of other organic cations, anions, and impurities, the aluminum phosphate will be formed in a dense deposition to fill the pores from the bottom to the outside, thereby reducing the depth of the pores in the anodized film and increasing the thickness of the dense film layer. Moreover, the filling process is carried out directly after the anodized film is formed, and the deposited aluminum phosphate is more tightly bonded to the pore wall than when the pores are sealed with a sealing agent, thereby significantly improving the corrosion resistance of Examples 4, 6, and 7.

[0076] Examples 4, 6, and 7 are significantly larger than Example 5 because the anodized film is deposited from the bottom of the pores to fill the tightly bound and dense aluminum phosphate. + The concentration decreases, and sufficient concentration of phosphate is required in the solution environment, but the phosphate concentration in Example 5 is insufficient. Therefore, in order to achieve better corrosion resistance, the phosphoric acid concentration of 6.4-8.3wt% is preferably selected when the anodizing electrolyte is a phosphoric acid solution.

[0077] For anodizing treatment, the magnitude of voltage and treatment time affect the formation of anodized film. The greater the voltage, the faster the anodized film is formed; the longer the treatment time, the closer the anodized film is to the theoretical maximum thickness. On the other hand, the greater the voltage, the more likely the anodized film is to have local unevenness and poor density, and the longer the treatment time, the more obvious the situation. In combination with Examples 4, 9 to 13, it can be seen that the anodized film formed in Examples 4, 9 to 11 at a voltage of 15V is relatively dense and uniform, and the corrosion resistance is improved to a better situation after the treatment time is not less than 25min. In Examples 12 to 13, anodizing treatment was carried out at a voltage of 15V. The treatment time of Example 13 was too long, the surface unevenness and roughness increased, and the corrosion resistance decreased, which was caused by the excessive voltage and treatment time.

[0078] Therefore, in the present application, the anodizing treatment voltage of the alloy component is preferably 15 to 20 V, and the treatment time is preferably 20 to 32 minutes.

[0079] Combining Examples 14 to 19 with Example 4, the corrosion resistance of the alloy components of Examples 14 to 19 is improved after the sealing treatment, and the protection level of Examples 14 to 19 is greater than that of Example 4.

[0080] In Examples 14 to 15, the present application mixes polyethylene glycol, methyltriethoxysilane, and water with a relative molecular weight of 100 to 200 as the precursor material of the sealing treatment solution, the initial solution. When the specific relative molecular weight of polyethylene glycol is 100 to 200, the polyethylene glycol with a low relative molecular weight is used as a cosolvent for methyltriethoxysilane during the stirring process of the initial solution. At the same time, under the control of the relative molecular weight of polyethylene glycol in the present application, when methyltriethoxysilane is hydrolyzed, part of the polyethylene glycol also reacts with silane to make it alcoholyzed, and the polyethylene glycol is connected to the silane precondensate, which has better affinity for the anodized film, good sealing effect, and better toughness and coverage of the resulting film layer, and the corrosion resistance is improved. Therefore, the protection level of Examples 14 to 1 is greater than that of Example 16. In addition, methyltriethoxysilane and polyethylene glycol are more environmentally friendly as the source of sealing components than chromate sealing agents.

[0081] By comparing Example 14 with Examples 18 to 19, it can be seen that in Example 14, ammonium acetate and sodium sulfite are added after the initial liquid treatment to prepare a sealing treatment liquid. The protection level of Example 14 is greater than that of Examples 18 to 19. This is because the pH of the sealing treatment liquid will reduce the sealing density, and the addition of ammonium acetate can serve as a pH buffer to reduce the influence of residual phosphoric acid in the pores of the anodized film, thereby improving the sealing effect and enhancing the corrosion resistance of the alloy components of the cable clamp; the addition of sodium sulfite can reduce iron ions to ferrous ions, thereby avoiding the inevitable conversion of other residual metal ions in the pores of the anodized film into non-dense precipitates, thereby reducing the sealing density or hindering the sealing.

[0082] In combination with Example 17, the protection level of Example 17 is also greater than that of Examples 18 to 19, so the ammonium acetate content in the sealing treatment liquid is 2.4 to 3.1 wt%, and the sodium sulfite content is 0.28 to 0.36 wt%, to achieve the above effect.

[0083] This specific embodiment is only an explanation of the present invention, and it is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to this embodiment as needed, but as long as it is within the scope of protection required by the present invention, it will be protected by the patent law.

Claims

1. A high voltage cable fixing clamp, characterized in that: The invention comprises an alloy component, wherein the alloy component comprises a base (1) and a gland (2) made of an aluminum alloy, wherein the aluminum alloy comprises Si 7.2-7.5wt%, Mg 0.40-0.45wt%, Ti 0.18-0.20wt%, Fe 0.03-0.05wt%, Cu 0.07-0.10wt%, Zr 0.07-0.15wt%, Sr 0.004-0.008wt%, Zn 0.006-0.008wt%, and the balance is aluminum.

2. A high voltage cable fixing clamp according to claim 1, characterized in that: The alloy component has an anodic oxide film on the outside, and the anodic oxide film is obtained by surface anodic oxidation treatment; The electrolyte used for surface anodizing treatment is a phosphoric acid solution with a phosphoric acid concentration of 6.4~8.3wt%.

3. A high voltage cable fixing clamp according to claim 2, characterized in that: During the surface anodizing treatment, the DC voltage applied to the alloy component is 15-20V, and the treatment time is 20-32 minutes.

4. A high voltage cable fixing clamp according to claim 2, characterized in that: The alloy component is also immersed in a sealing treatment liquid for sealing treatment to form an outer sealing film.

5. A high voltage cable fixing clamp according to claim 4, characterized in that: The sealing treatment liquid includes an initial liquid after pre-hydrolysis and alcoholysis, and the initial liquid composition includes methyltriethoxysilane and polyethylene glycol. The relative average molecular weight of the polyethylene glycol is 200, and the relative molecular weight distribution is 150-250; The methyltriethoxysilane accounts for 10-20 wt % in the initial solution, and the polyethylene glycol accounts for 13-24 wt % in the initial solution.

6. A high voltage cable fixing clamp according to claim 5, characterized in that: The methyltriethoxysilane accounts for 20 wt % in the initial solution, and the polyethylene glycol accounts for 24 wt % in the initial solution.

7. A high voltage cable fixing clamp according to claim 5, characterized in that: The sealing treatment liquid also includes ammonium acetate, and the ammonium acetate accounts for 2.4-3.1wt%.

8. A high voltage cable fixing clamp according to claim 5, characterized in that: The sealing treatment liquid also includes sodium sulfite, and the sodium sulfite accounts for 0.28-0.36wt%.