Highly dispersed aluminum framework MFI zeolites and their use for selective aromatic methylation to para-xylene

By improving the acid site distribution of the MFI zeolite catalyst and incorporating boron, the problems of low p-xylene purity and methanol utilization in the toluene methylation process in the existing technology have been solved, and high-efficiency, low-cost xylene production has been achieved. Production.

CN118748988APending Publication Date: 2024-10-08UOP LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380023571.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-01
Filing Date
2023-03-01
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult to achieve high paraxylene purity and high methanol utilization in the toluene methylation process using existing technology, and the catalyst selective treatment is complex and unstable, resulting in high production costs.

Method used

Using an improved MFI zeolite catalyst, by changing the acid site distribution, adding a low number of proximal framework aluminum sites, and using specific organic structure directing agents such as ethylenediamine and 1,4 diazabicyclo under specific conditions [2.2.2] Octane, incorporated with boron, forms a catalyst with highly dispersed skeleton aluminum, optimizing the catalyst morphology and reaction conditions to improve paraxylene selectivity and methanol utilization.

Benefits of technology

It achieves high paraxylene purity and high methanol utilization, reduces the complexity and production cost of catalyst selectivity, improves the reproducibility and stability of the catalyst, and is suitable for efficient production of xylene under mild conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748988A_ABST
    Figure CN118748988A_ABST
Patent Text Reader

Abstract

A process for contacting a feed stream comprising an oxygenate feedstock and an aromatic feedstock comprising toluene with a catalyst and recovering a product comprising para-xylene. The catalyst comprises an improved MFI zeolite having a SiO2 / Al2O3 ratio of 50 to 600 in calcined and ion exchanged form and having a framework aluminum site distribution characterized by an initial xylene selectivity of greater than 70% in the TM diagnostic test.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority declaration

[0002] This application claims priority to U.S. Provisional Patent Application Serial No. 63 / 315,429 filed on March 1, 2022, the entire contents of which are incorporated herein by reference. Technical Field

[0003] This field is the production of para-xylene and includes a process comprising contacting toluene and an oxygenate over an MFI zeolite catalyst. Background Art

[0004] MFI zeolite is a versatile catalyst for carrying out a variety of catalytic processes for petrochemical production, such as the conversion of oxygenates to light olefins, to propylene in methanol) and to methanol to aromatics, or the co-production of light olefins and aromatics.

[0005] Typically, an aromatics complex is designed to co-produce xylenes and benzene, with xylenes being the main product. Among the xylene isomers, para-xylene accounts for the majority of the xylene product demand. The amount of xylene relative to benzene is predetermined by the ratio of methyl to phenyl of the reformate entering the aromatics complex, which is derived, for example, from a reforming process. The total ratio of methyl to phenyl in an aromatics complex is typically less than 2.0. A methyl to phenyl ratio of 2.0 is required to have 100% para-xylene production and net zero benzene production. One method of commercially maximizing para-xylene production is to use oxygenates such as methanol to methylate toluene and benzene to increase the ratio of methyl to phenyl to 2.0. The ratio of methyl to phenyl can be calculated by dividing the number of methyl groups by the number of aromatic centers of the entire product. For example, benzene has 0 methyl groups and 1 phenyl moiety, giving a methyl / phenyl ratio of 0. Toluene has 1 methyl group and 1 phenyl moiety, and the methyl / phenyl ratio is 1. Each of the three xylenes has 2 methyl groups and 1 phenyl group, with a methyl / phenyl ratio of 2. Methyl to phenyl ratios greater than 1, or greater than 1.5, or greater than 1.75 are desirable. Furthermore, in toluene methylation, it is highly desirable to perform the process to obtain high xylene yields at very high para-xylene to xylene ratios greater than, for example, 90%, to avoid the difficult and expensive para-xylene extraction process.

[0006] Typically, toluene methylation is operated to selectively produce paraxylene. Harsh process conditions are used, namely high temperatures, where methanol conversion to hydrocarbons (MTH) or methanol conversion to gasoline (MTG) becomes increasingly significant and methanol decomposes to CO xand H2 are measurable. Significant amounts of diluents such as H2O, H2 and therefore recycle streams are used, making it relatively difficult to prepare the catalyst reproducibly. MFI zeolite is the catalyst predominantly used in this process.

[0007] As used herein, zeolite can be referred to by an inappropriate name such as silicalite, an appropriate name such as ZSM-5, or by a structure type code such as MFI. These three-letter codes indicate atomic connections, thus indicating the aperture, shape and connection of various known zeolites. The list of these codes can be found in the zeolite framework type collection of illustrative plates maintained by the International Zeolite Association Structure Commission at http: / / www.iza-structure.org / databases / . At present, 255 kinds of structure types are known and are classified by IZA. One such structure type, MFI, is described as including 3-dimensional 10-ring channels with straight channels along crystal axis b and curved channels along axis a. Zeolites are distinguished from each other based on their composition, crystal structure and adsorption characteristics. A method commonly used to distinguish zeolites in the art is x-ray diffraction.

[0008] The toluene methylation process is mostly carried out by zeolite MFI. In order to achieve very high p-xylene purity in xylene, zeolite MFI is usually "selectivized" to obtain a shape selection effect that is conducive to the production of p-xylene molecules. The main means to achieve "selectivization" is to deposit SiO2 via a combination of silicon-containing compounds, alkaline earth metal oxides such as MgO, phosphates and the aforementioned substances, as shown in US6,504,072. After the chemical deposition step, steaming is regularly carried out to different degrees to further achieve the shape selection effect. The purpose of this type of "selectivization" treatment is to neutralize external acidity and constrain the zeolite pores to allow p-xylene to selectively diffuse out of microporous holes, while limiting the degree of both meta-xylene and o-xylene coming out of the micropores. Due to the morphological heterogeneity of the starting MFI material and the high reaction properties of the selectivization agent and the zeolite MFI surface, the selectivization process via conventional means is highly heterogeneous, and the result of the selectivization is affected by many material variables and process parameters.

[0009] The selectivation process can reduce the utilization of oxygenates. For example, as shown in US6,504,072, when the catalyst is modified to produce 86% to 92%, 97% and then 98% para-xylene purity using a catalyst composition of phosphorus, 225 Si / Al ratio ZSM-5 and a binder comprising silica alumina and clay, the methanol utilization can drop to below 60%, below 50% and even below 40%.

[0010] Silicon compounds have also been used to selectivate extrudates comprising ZSM-5 (Si / Al=13) and a SiO2 binder in US 2005 / 0143613, where the effects of the number of selectivation treatments, steaming, platinum incorporation, order of platinum incorporation, steam and ZSM-5 Si / Al ratio were studied. These variables had a significant effect on catalyst stability, p-xylene purity and methanol utilization only in the range of 40% to 50%. When using ZSM-5 with Si / Al=225 and steaming at 1060°C, a methanol utilization of 60% could be achieved at a p-xylene purity of 90%.

[0011] Another method for obtaining para-xylene selectivity is through the use of a specific morphology of zeolite MFI. It has been shown that crystals containing intergrown MFI (in which the sinusoidal channels expose more than 73% of the crystallite exterior) lead to enhanced para-xylene selectivity, Nature Communications, 2019, 10, 4348. Even under mild conditions that are favorable for the formation of para-xylene, i.e., atmospheric pressure, H2O and H2 co-feed and 470°C, using a feed with a molar ratio of toluene to methanol of 2.0 and a ZSM-5 with a Si / Al ratio of 150, only a moderate toluene conversion of 20% is achieved, with methanol utilization as low as 50%.

[0012] Mass transfer also needs to be considered. It has been shown that when a caustic modified zeolite ZSM-5 and subsequent MgO selectivity are used, toluene methylation and subsequent xylene isomerization are mass transfer controlled in the selective MFI (Ind. Eng. Chem. Res., 2017, 56, 9310-9321). Due to the kinetically controlled methanol conversion to hydrocarbons (MTH) side reaction, methanol utilization is still low. The disadvantage of improving mass transfer properties by generating mesopores is that a large number of surface functional groups, such as silanol groups, are attached, making surface passivation challenging.

[0013] Although high para-xylene purity is achieved via the foregoing process, the result is a trade-off of significantly low methanol utilization (40% to 60%). Methanol utilization is defined as (moles of xylenes formed - moles of benzene formed) / (moles of methanol converted). Methanol utilization reflects the amount of oxygenates that enter the xylenes, as opposed to non-aromatics including olefins and paraffins, as well as heavy aromatics. Due to the measurable cost of oxygenates, the technical economics of the aromatic methylation process will vary with the difference in oxygenate cost and the price of para-xylene versus benzene. Therefore, the feasibility and growth of aromatic methylation to para-xylene will at least overcome the oxygenate utilization problem.

[0014] Temperature also affects the xylene selectivity during toluene methylation. Lower reaction temperatures (below 300°C) favor the formation of o-xylene over p-xylene and m-xylene, due to the inherent product selectivity, reduced effects of secondary reactions (such as xylene isomerization, polymethylbenzene dealkylation, toluene disproportionation) and negligible xylene diffusion limitations typically observed on MFI zeolites. Low temperatures also favor methanol utilization due to a significant reduction in the rate of aromatic dealkylation.

[0015] It is therefore desirable to provide improved methods and apparatus for methylating aromatic compounds such as toluene and benzene in an aromatics complex. In addition, it is desirable to provide a cost-effective process for high selectivity to para-xylene over a catalyst comprising an improved MFI zeolite for toluene and / or benzene methylation, which process operates under mild conditions, promotes high feedstock utilization, and in which above equilibrium pX / X ratios can be achieved without dilution. Moreover, other desirable features and characteristics of the inventive subject matter will become apparent from the subsequent detailed description of the subject matter and the appended claims, taken in conjunction with this background of the subject matter. Summary of the invention

[0016] Here we disclose the catalyst comprising improved MFI zeolite for producing p-xylene with high conversion by contacting a feed stream comprising toluene with oxygenates, the improved MFI zeolite comprising a changed acid site distribution. Generally speaking, the improved MFI zeolite catalyst can be characterized as having a low number of proximal framework aluminum sites. The high dispersion of acid sites in MFI zeolite can also be associated with an increased fraction of acid sites located in the smaller channel pores relative to the larger channel intersection. The changed framework aluminum site distribution is further characterized by the performance of highly selective p-xylene formation in a TM diagnostic test under conditions where the molar ratio of oxygenates (dimethyl ether, DME) to toluene is 6 to 16 and the temperature is 130°C. Zeolite MFI is characterized by SiO2 / Al2O3 in the range of 50 to 600, and preferably, is characterized by boron being incorporated into the framework, Si / B in the range of 20 to 50. MFI zeolites for selective aromatic methylation for para-xylene production can be synthesized using a specific organic structure directing agent (OSDA) comprising ethylenediamine (EDA) and 1,4 diazabicyclo[2.2.2]octane (DABCO) with a SiO2 / Al2O3 ratio in the range of 40 to 1000 and preferably with boron incorporated into the synthesis gel.

[0017] The inherently more selective MFI zeolite will achieve higher para-xylene production throughput and lower production costs due to its significantly higher methanol utilization. In addition, when the inherent para-xylene selective MFI is combined with the favorable morphology for aromatic methylation, an economically favorable process can be obtained compared to the fluctuations in oxygenate feed costs and the difference in para-xylene and benzene prices. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a graph showing the xylene isomer selectivity of different MFI examples at 130°C, 4 kPa toluene and 66 kPa dimethyl ether. A indicates the material group of Comparative Example 2. B indicates the material group of Example 1. E is the equilibrium distribution of xylene isomers at 130°C.

[0019] Figure 2 is a graph showing the xylene isomer selectivity at different toluene conversions (0.1% to 1.0%) at 130°C during toluene methylation with dimethyl ether. The solid symbols are for Example 2.1, while the open symbols are for Example 1.1. p-Xylene (diamonds), m-Xylene (circles), o-Xylene (squares).

[0020] Figure 3 is a graph showing the xylene isomer selectivity at different toluene conversions (0.005% to 0.05%) at 130°C during toluene methylation with methanol. The solid symbols are for Example 2.1, while the open symbols are for Example 1.1. p-Xylene (diamonds), m-Xylene (circles), o-Xylene (squares).

[0021] definition

[0022] The term "communication" means that fluid flow is operatively allowed between the enumerated components, which can be characterized as "fluid communication".

[0023] The term "downstream communication" means that at least a portion of the fluid flowing to the body in the downstream communication can operatively flow from the object in fluid communication therewith.

[0024] As used herein, the terms "predominantly", "predominantly" or "mainly" mean greater than 50%, suitably greater than 75%, and preferably greater than 90%.

[0025] The term "Cx" is understood to refer to molecules having the number of carbon atoms represented by the subscript "x". Similarly, the term "Cx-" refers to molecules containing less than or equal to x, and preferably x and fewer carbon atoms. The term "Cx+" refers to molecules having greater than or equal to x, and preferably x and more carbon atoms.

[0026] As used herein, the term "xylenes" describes a class of dimethylbenzene molecules including one or more of 1,2-dimethylbenzene, 1,3-dimethylbenzene, and 1,4-dimethylbenzene. 1,2-dimethylbenzene is often referred to as ortho-xylene or oX. 1,3-dimethylbenzene is often referred to as meta-xylene or mX. 1,4-dimethylbenzene is often referred to as para-xylene or pX. DETAILED DESCRIPTION

[0027] The present disclosure provides a process for producing para-xylene, the process comprising contacting a feed stream with an improved zeolite MFI that is inherently more selective for para-xylene. By combining favorable morphology with favorable distribution of framework aluminum sites characterized by specific reactivity in TM diagnostic tests, selective aromatic methylation for para-xylene production can be achieved with high para-xylene purity and high oxygenate utilization in total xylene.

[0028] The purpose of selective aromatic methylation is to achieve high p-xylene purity and high oxygenate utilization. As described in the background art, the conventional means of achieving high p-xylene purity is via a selectivation process. The oxygenate used in the process for producing p-xylene may comprise methanol, dimethyl ether, dimethyl carbonate, or a mixture thereof.

[0029] The aforementioned trade-off of methanol utilization and paraxylene purity is inherent because the conversion of methanol to byproducts such as light olefins and paraffins is partially carried out through polymethylated intermediates in the MTH chemistry. Zeolite MFI prepared via conventional OSDA such as tetrapropylammonium (TPA) has been shown to produce more expanded ortho-xylene isomers and continuous methylated products such as trimethylbenzenes under prescribed diagnostic conditions of 130°C and a DME to toluene molar ratio of 16, as shown in the comparative examples described below. This reactivity pattern will direct the reaction along the path of light olefin and paraffin formation, thus reducing methanol utilization. This reactivity pattern also requires secondary isomerization reactions of ortho-xylene isomers to obtain the desired para-xylene.

[0030] The zeolite of MFI can be used for the preparation of the present invention.Dependent on the synthesis conditions, MFI zeolite can contain the acid site distribution that is positioned in the isolation configuration or near another acid site, wherein the near side acid site can be quantitatively measured by the cobalt titration technique.These acid sites can be located in a straight or sinusoidal channel (about 0.55nm gap size diameter) or in a larger intersection (about 0.65nm on gap size diameter).Gap size is defined as the average cross-sectional diameter of the channel or their intersection, as specified in the IZA database.For a given Si / Al ratio, the fraction of near side Al material can be controlled by changing the organic and inorganic structure directing agents used during the MFI zeolite synthesis.The acid site distribution in different pore positions in the zeolite or at different relative near sides has been confirmed as a parameter affecting various acid catalyzed reactions.

[0031] On the other hand, the MFI prepared according to the present disclosure shows that para-xylene can be produced, wherein small amounts of other xylenes and negligible amounts of continuous methylation products are observed. This reactivity pattern will translate into a low tendency for by-product formation and thus a higher methanol utilization.

[0032] This reactivity pattern under the TM diagnostic test reaction conditions further characterizes MFI samples with altered Al distribution, with highly dispersed framework aluminum, or lack of proximal framework aluminum. As shown in Table 1 below, the comparative examples synthesized by conventional OSDA (TPA) have a measurable fraction of framework aluminum in close proximity to each other. The proximity of framework aluminum is further characterized by measurements of the amount of cobalt ions exchanged onto the MFI zeolite during the "cobalt titration technique", as shown in Tables 1 and 2. The combined TM diagnostic test and cobalt titration technique may be the best available technique for characterizing the proximity of framework aluminum.

[0033] The MFI zeolites of the present disclosure have less than 18% proximal aluminum framework sites by cobalt titration technique, the values ​​of which are shown in Table 1 as 2×Co 2+ / Al. The values ​​in this test can range from 0 to 1, and therefore from 0% to 100%. They can have less than 15% or less than 10% proximal aluminum framework sites by the cobalt titration technique.

[0034] Methanol utilization for para-xylene production will be higher through the use of an inherently more selective MFI zeolite because it requires less catalyst selectivation to obtain a given level of para-xylene selectivity, and therefore less methanol utilization compromise. The properties that contribute to better para-xylene selectivity performance are uniform and make it more reproducible than conventional selectivation approaches. This material enables the toluene methylation process to operate at lower temperatures, with shorter contact times due to less selectivation required to achieve comparable higher para-xylene production capacity, and therefore higher methanol utilization.

[0035] The inherently more selective MFI zeolite for high paraxylene and lower light olefin and paraffin production will achieve higher paraxylene production throughput and lower production costs due to its significantly higher methanol utilization (or methanol consumption) for increasing the methyl to phenyl ratio out of the aromatics complex.

[0036] According to an exemplary embodiment, a process for producing paraxylene is provided, comprising reacting an oxygenate with an aromatic feedstock comprising toluene and / or benzene in the presence of a catalyst comprising a modified MFI zeolite in a methylation zone operated under alkylation conditions comprising a maximum temperature of 400°C to 675°C and a pressure of 10 kPa to 5000 kPa to provide a product stream comprising paraxylene.

[0037] According to another exemplary embodiment, a method for producing para-xylene is provided, comprising reacting a toluene stream and a methanol stream in the presence of a catalyst composition comprising an improved MFI zeolite in a toluene methylation zone operated under toluene methylation conditions comprising a maximum temperature of 400°C to 675°C and a pressure of 10 kPa to 5,000 kPa to produce a product stream comprising para-xylene.

[0038] According to another exemplary embodiment, a method for producing paraxylene is provided, comprising: subjecting a toluene stream and a methanol stream to a catalyst composition comprising an improved MFI zeolite at a maximum temperature of 400° C. to 675° C., a pressure of 10 kPa to 5,000 kPa, a temperature of 0.5 hr. -1 Up to 20 hours -1 The reaction is carried out in a toluene methylation zone operated under toluene methylation conditions at a weight hourly space velocity of 1000 Å and a molar ratio of toluene to methanol of 1:1 to 6:1 to produce a product stream comprising para-xylene.

[0039] The feed stream of the process of the present invention generally comprises the general formula C6H (6-n) R n wherein n is an integer from 0 to 5, and each R may be CH3, C2H5, C3H7, or C4H9 in any combination. The aromatic-rich feed stream for the process of the present disclosure may be derived from a variety of sources, including, but not limited to, conventional catalytic reforming, zeolite reforming to convert C6-C7 non-aromatics from light naphtha or aromatic extraction raffinates into benzene and toluene, steam pyrolysis of naphtha, distillates, or other hydrocarbons to produce light olefins and aromatic-rich byproducts (including gasoline-range materials, commonly referred to as "pyrolysis gasoline"), and catalytic or thermal cracking of distillates and heavy oils to produce gasoline-range products. The products from pyrolysis or other cracking operations are typically hydrotreated according to methods well known in the industry prior to loading into the complex in order to remove sulfur, olefins, and other compounds that would affect product quality and / or damage catalysts and downstream processes. Light cycle oil obtained from catalytic cracking may also be advantageously hydrotreated and / or hydrocracking according to known techniques to produce gasoline range products; hydrotreating is also preferably applied to catalytic reforming to produce an aromatics-rich feed stream. The feed stream may comprise primarily toluene.

[0040] In one aspect, the aromatic feedstock comprises toluene. In another aspect, the aromatic feedstock may comprise benzene. In one embodiment, the aromatic feedstock may comprise both benzene and toluene. The process conditions for forming paraxylene may include a maximum temperature of 400°C to 675°C, preferably 450°C to 650°C, and more preferably 500°C to 625°C. According to various embodiments, the maximum temperature may refer to the maximum temperature of the catalyst bed, and may be interchangeably referred to as the maximum bed temperature. In addition, the process conditions may include a pressure of 10 kPa to 5,000 kPa, preferably 100 kPa to 2000 kPa, and more preferably 300 kPa to 1000 kPa. The process conditions may also include a 0.1 hr -1 Up to 25 hours -1 , preferably 0.5hr -1 Up to 15 hours -1 and more preferably 2 hr -1 Up to 12 hours -1 The alkylation conditions may include a molar ratio of the aromatic feedstock to the oxygenate of from 0.5:1 to 10:1, preferably from 1:1 to 6:1, and more preferably from 1.5:1 to 4:1. In one embodiment, the conditions may include a maximum temperature of less than 650°C, a pressure of from 100 kPa to 1,000 kPa, and a molar ratio of toluene to methanol of from 1:2 to 6:1. The oxygenate may be selected from the group consisting of methanol, dimethyl ether, dimethyl carbonate, and mixtures thereof.

[0041] The diluent may also comprise a feed stream. The diluent may comprise H2, H2O, and combinations thereof. The molar ratio of diluent to the aromatic feedstock and the oxygenate feedstock may be in the range of 0.1 to 3.0, preferably 0.1 to 2.0, and most preferably 0.2 to 1.5. In one aspect, the molar ratio may be described as H2O / (toluene+methanol) and may be in the range of 0.1 to 3.0.

[0042] In the present disclosure, we tailor the morphology of zeolite MFI independently of the distribution of framework aluminum within the 12T-site of the MFI structure. The distribution of framework aluminum can be detected by using cobalt titration techniques and / or NH3 TPD. The improved MFI zeolite may contain heteroatoms Q selected from the group consisting of boron, gallium, indium and iron and mixtures thereof. As shown in Tables 1 and 2 below, the incorporation of heteroatoms such as boron in addition to framework aluminum can reduce the effective mass transfer path across crystallites. The heteroatom Q can be boron, and the ratio of Si / B can be in the range of 20 to 50. By incorporating boron and a specific OSDA comprising ethylenediamine (EDA) and 1,4 diazabicyclo [2.2.2] octane (DABCO) in the MFI synthesis with a SiO2 / Al2O3 ratio in the range of 40 to 1000, an improved methanol utilization rate can be achieved via highly dispersed framework aluminum for reduced MTH side reactions and via improved mass transfer properties for enhanced toluene methylation.

[0043] The improved MFI zeolite of the present disclosure may be formulated into a catalyst by combining with a binder.The improved MFI zeolite may comprise between 25% and 95% by weight of the catalyst.

[0044] Example

[0045] Example 1

[0046] Using the described procedure, zeolite MFI used in the subject disclosure for the selective methylation of aromatics such as toluene to p-xylene is synthesized via the use of a structure directing agent (SDA) comprising ethylenediamine (EDA) and / or 1,4 diazabicyclo[2.2.2]octane (DABCO). The MFI synthesis may contain heteroatoms, such as boron (named B-Al-MFI as opposed to Al-MFI), to reduce the zeolite size to obtain favorable mass transfer properties. Al-MFI and B-Al-MFI synthesized using EDA have Si / Al ratios ranging from 50 to 1000. The relationship between Si / Al and SiO2 / Al2O3 is 2 times. That is, a zeolite with Si / Al=50 has a SiO2 / Al2O3 of 100. They are characterized by a highly dispersed framework aluminum distribution measured by ion exchange of the zeolite with cobalt ions ("cobalt titration technique"), as shown in Tables 1 and 2. The experimental procedure of the cobalt titration technique is described in "Theoretical and Experimental Assessment of Aluminum Proximity in MFI Zeolite and its Alteration by Organic and Inorganic Structural Directing Agents" by CT Nimlos (Chem. Mater., 2020, 32(21), 9277-9298). The MFI zeolite of the present disclosure has less than 18% of proximal aluminum framework sites by the cobalt titration technique, the value of which is shown in Table 1 as 2×Co 2+ / Al. They may have less than 15% or less than 10% proximal aluminum framework sites by cobalt titration techniques.

[0047] Example 1.1

[0048] Zeolite MFI was synthesized using a combination of boron and aluminum as heteroatoms and a combination of EDA and TPA as SDA according to the procedures of the following documents: "Influence of tetrapropyl ammonium and Ethylenediamine Structural Directing Agents on Framework Aluminum distribution" by YG Hur (Industrial and Engineering Chemistry Research, 2019, 58 (27), 11849-11860) and "Increased Oligomer Selectivity in Olefin Oligomerization by Incorporation of Boron" by JT Miller (WO2019028035A2).

[0049] Example 1.2

[0050] Zeolite MFI was synthesized using aluminum as heteroatom and DABCO as SDA according to the procedure of the following document: CT Nimlos mentioned previously.

[0051] Example 1.3

[0052] Zeolite MFI was synthesized using aluminum as a heteroatom and EDA and TPA as SDA according to the procedure of the previously mentioned YG Hur and JT Miller and co-inventors "Improving oligomer selectivity in olefin oligomerization by incorporation of boron" (WO2019028035A2).

[0053] Example 1.4

[0054] Zeolite MFI was synthesized using aluminum as a heteroatom and EDA and TPA as SDA according to the procedure of the previously mentioned YG Hur and JT Miller and co-inventors "Improving oligomer selectivity in olefin oligomerization by incorporation of boron" (WO2019028035A2).

[0055] Example 1.5

[0056] Zeolite MFI was synthesized using a combination of boron and aluminum as heteroatoms and a combination of EDA and TPA as SDA according to the procedure of the previously mentioned YG Hur and JT Miller and co-inventors "Improving oligomer selectivity in olefin oligomerization by incorporating boron" (WO2019028035A2).

[0057] Comparative Example 2

[0058] For the purpose of comparison of different reactivity patterns of the zeolite MFI disclosed in the present subject matter, a series of MFIs with a high fraction number of proximal framework aluminum sites were synthesized using tetrapropylammonium (TPA) OSDA at similar Si / Al ratios in the comparative examples. Commercial MFI zeolite samples are also included here. The characteristics of the samples are summarized in Tables 1 and 2.

[0059] Example 2.1

[0060] Zeolite MFI was purchased from Zeolyst as CBV8014 with Si / Al=43.

[0061] Example 2.2

[0062] Zeolite MFI was synthesized using a combination of boron and aluminum as heteroatoms and TPA as SDA according to the procedures of the following documents: the previously mentioned YGHur and WO2019028035A2.

[0063] Example 2.3

[0064] Zeolite MFI was synthesized using aluminum as heteroatom and TPA as SDA according to the procedure of the following document: CT Nimlos mentioned previously.

[0065] Example 2.4

[0066] Zeolite MFI was synthesized using aluminum as heteroatom and TPA and Na as SDA according to the procedure of the following document: CT Nimlos mentioned previously.

[0067] Table 1

[0068]

[0069] Table 2

[0070] Example 2.1 2.2 2.3 2.4 Synthetic SDA Unknown substances <![CDATA[TPA + ]]> <![CDATA[TPA + ]]> <![CDATA[TPA + +That + ]]> skeleton Al-MFI B-Al-MFI Al-MFI Al-MFI Si / Al 43 59 50 55 <![CDATA[H + / Al]]> 0.85 0.84 1.01 0.97 Al / uc 2.18 1.57 1.89 1.73 <![CDATA[H + / u.c.]]> 1.85 1.31 1.91 1.68 Si / B No B 48 No B No B <![CDATA[2×Co 2+ / Al]]> 0.46 0.20 0.24 0.44 Average crystallite size (SEM) 0.3μm ~0.6μm 0.5μm 4μm

[0071] Example 2: Toluene methylation

[0072] The zeolites of the subject disclosure are further characterized by a catalytic diagnostic test performed at 130°C and a dimethyl ether (DME) to toluene molar ratio of 16, wherein the active sites are mostly covered by oxygenates. The test is a TM diagnostic test. The diagnostic test conditions limit toluene methylation to less than 5% conversion and are designed to probe and characterize the active sites for toluene methylation under a kinetically controlled reaction regime, and the results are summarized in Table 3 below.

[0073] Specifically, toluene methylation experiments were conducted in a tubular packed bed reactor (quartz, 7 mm ID) at 403 K. Fresh zeolite samples (0.010 g to 0.060 g; NH4 + -form) was pelleted, crushed and sieved to retain aggregates between 180 μm and 250 μm in diameter. The sieved sample was diluted with acid purified quartz sand (180 μm to 250 μm) to maintain a constant 1 g of solid material, which was supported between two quartz wool plugs. The bed temperature was measured using a K-type thermocouple in contact with the side of the quartz tube at the level of the bed and maintained at the desired temperature using a three-zone heating furnace (Applied Test Systems) and a Watlow controller (EZ-Zone). For higher conversion studies, a higher quality (1.8 g) MFI sample without silica diluent was evaluated at a molar ratio of DME to toluene of 6 and at a temperature of 130°C.

[0074] Before the catalytic run, a 5% O2 / He flow (UHP, Indiana Oxygen, 100 cm 3 / min) pre-treated catalyst (5K / min to 773K). After keeping for 4 hours, the catalyst was cooled (5K / min) to the reaction temperature and purged with He for at least 1 hour before introducing the reactants. With the help of a syringe pump (KD Scientific Legato 100), liquid toluene (Sigma Aldrich, HPLC grade,> 99.99%) was vaporized into a mixed stream of He (UHP, IndianaOxygen) and DME (Matheson, CP,> 99.5%) at a heated tee (473K). For toluene methylation with methanol, methanol and toluene were pre-mixed in a desired molar ratio and fed into the same tee. All heating lines upstream of the reactor were kept> 400K, while the heating lines from the reactor outlet to the GC were maintained> 440K to limit condensation. Methane (0cm 3 / min to 5cm 3 / min; 25% CH4 / Ar; Indiana Oxygen) was co-fed with the reactants and used as an internal standard. The total flow rate was maintained at 50 cm 3 / min to 100cm3 / min. Reactant and product concentrations were measured by online gas chromatography (Agilent 7890B) using a DB-Wax column (30m×320μm×0.5μm) and a flame ionization detector (25- to 30-minute sampling intervals). GC peak areas were quantified using a calibration curve developed by feeding known amounts of standards into the GC.

[0075] Before reaction, feed stream composition is stable, and is verified by bypass injection.Reaction is operated under 4kPa toluene and 66kPa DME (or 4kPa methanol) and fixed reaction conditions for 6 hours to 14 hours, and initial conversion remains lower than 0.4% simultaneously.Use quartz wool and SiO at 473K During the blank reactor test carried out, no product is observed.The xylene site time yield (STY) is calculated by the reactor outlet molar flow rate of the dimethylbenzene normalized by initial proton count (using NH3 TPD to obtain) when the reaction starts.NH3 TPD conditions and procedures are described in detail in the CTNimlos mentioned previously.Xylene selectivity is calculated by the single xylene STY normalized by total xylene STY.Toluene conversion is calculated based on product mole.Initial rate, xylene selectivity and conversion are reported with 0.2 hour to 0.5 hour running time. In one case, the external acidity of the MFI catalyst was poisoned using 2,6-di-tert-butylpyridine (DTBP) co-fed with toluene at a partial pressure of 0.006 kPa to 0.022 kPa.

[0076] Table 3

[0077]

[0078] The catalytic performance of the disclosed MFI zeolites in the TM diagnostic test is characterized by having an initial activity (defined as total xylenes STY) 1 / 5 to 1 / 10 times that of the comparative example MFI zeolites synthesized by conventional means and / or SDA (such as tetrapropylammonium). STY is expressed as moles of product / (moles H + )-seconds and was originally defined by Boudart, Chem. Rev., 1995, 95, 661-666. Under kinetically controlled reaction regimes, zeolite particle size controlled via boron incorporation in the synthesis plays no role in activity or preference requirements in forming specific xylene isomers.

[0079] The catalytic performance of the disclosed MFI zeolites in the TM diagnostic test is further characterized by having an initial para-xylene content of greater than 70% in total xylenes, which is twice that observed in MFI zeolites synthesized by conventional SDA. The catalytic performance of the disclosed MFI zeolites synthesized by EDA or DABCO SDA is further characterized by having a steady-state para-xylene to total xylene ratio of greater than 30% or greater than 35%. As shown in the accompanying invention summary, the comparative example MFI zeolites synthesized by conventional SDA exhibited para-xylene selectivities of 20% to 27% of total xylenes. For runs with STY less than 0.03, no (N / D) xylene selectivity values ​​were determined because insignificant amounts of xylene were generated to reliably determine a specific xylene fraction.

[0080] Low toluene methylation activity and high para-xylene selectivity are properties of active sites that are configured for more shape selective isomers (i.e., para-xylene in the toluene methylation reaction) and also for less continuous methylated products (i.e., polymethylated benzenes (PMB)). As previously noted, the properties of the active sites of the present disclosure in MFI zeolites characterized by having a low number of proximal framework aluminum sites are less inclined to promote the MTH reaction and are therefore inherently more selective for aromatic methylation to xylenes and, therefore, enhance methanol utilization.

[0081] At 130°C and higher toluene conversions up to 6%, the samples described in Example 2.1, o-xylene remained as the major product at 64% to 72% selectivity at all run times, while p-xylene (22% to 24%) and m-xylene (6% to 12%) remained as minor products at all run times. Xylenes accounted for >95% of the total aromatic products.

[0082] The samples described in Example 1.4 were evaluated in the presence and absence of a selective external acidic poison (DTBP) at 130° C. The initial xylene selectivity remained similar and dominated by para-xylene (69% to 71%), but the xylene selectivity at longer run times (9 hours) had a higher para-xylene selectivity (45%) compared to the para-xylene selectivity in the absence of co-fed DTBP (34%).

[0083] Table 4

[0084]

[0085] Embodiment 4 to Embodiment 6 .

[0086] To further minimize the fraction of proximal framework aluminum, EDA-MFI syntheses were performed with increasing SiO2 / Al2O3 ratios while incorporating boron into the synthesis to maintain particle size for favorable mass transfer properties, as described below in Examples 4 to 6 and in corresponding comparative examples prepared at comparable SiO2 / Al2O3 ratios. The properties of the resulting zeolite MFI are summarized in Table 3.

[0087] Example 4

[0088] An alumina-borosilicate solution was prepared by first mixing 11.19 g aluminum nitrate nonahydrate, 70.09 g boric acid, 53.77 g ethylenediamine, 30.33 g TPAOH (40% solution), and 791.45 g water while stirring vigorously. After thorough mixing, 443.18 g Ludox HS-40 (SiO2, mass-40%) was added. The reaction mixture was homogenized with a high-speed mechanical stirrer for 20 minutes and transferred to a 2-L Parr Hastelloy stirred autoclave. The mixture was crystallized at 175°C while stirring at 300 RPM for 88 hours. The solid product was recovered by filtration, washed with deionized water, and dried at 100°C. The product was identified as MFI by XRD. Chemical analysis gave the product composition Si / Al=111, Si / B=21.36. The sample was calcined at 580°C for 6 hours and the BET surface area was 287 m 2 / g, the micropore volume is 0.143cc / g, and the total pore volume is 0.164cc / g.

[0089] Comparative Example 4A

[0090] An alumina-borosilicate solution was prepared by first mixing 7.53 g aluminum nitrate nonahydrate, 47.18 g boric acid, 306.21 g TPAOH (40% solution), and 740.74 g water while stirring vigorously. After thorough mixing, 298.33 g Ludox HS-40 (SiO2, mass-40%) was added. The reaction mixture was homogenized with a high-speed mechanical stirrer for 20 minutes and transferred to a 2-L Parr Hastelloy stirred autoclave. The mixture was crystallized at 175°C while stirring at 300 RPM for 88 hours. The solid product was recovered by filtration, washed with deionized water, and dried at 100°C. The product was identified as MFI by XRD. Chemical analysis gave the product composition Si / Al=88, Si / B=35. The sample was calcined at 580°C for 6 hours, and the BET surface area was 344 m 2 / g, the micropore volume is 0.171cc / g, and the total pore volume is 0.190cc / g.

[0091] Comparative Example 4B

[0092] Tetrapropylammonium (TPA) was used as OSDA to synthesize zeolite silicalite with a target SiO2 / Al2O3 ratio of 95. The Si / Al ratio of the resulting zeolite after calcination to remove the organic template was 100 and the BET surface area was 358 m 2 / gm, the micropore volume is 0.184cc / g, and the total pore volume is 0.208cc / g.

[0093] Example 5

[0094] An alumina-borosilicate solution was prepared by first mixing 5.61 g aluminum nitrate nonahydrate, 70.31 g boric acid, 53.94 g ethylenediamine, 30.42 g TPAOH (40% solution), and 795.15 g water while stirring vigorously. After thorough mixing, 444.57 g Ludox HS-40 (SiO2, mass-40%) was added. The reaction mixture was homogenized with a high-speed mechanical stirrer for 20 minutes and transferred to a 2-L Parr Hastelloy stirred autoclave. The mixture was crystallized at 175°C while stirring at 300 RPM for 88 hours. The solid product was recovered by filtration, washed with deionized water, and dried at 100°C. The product was identified as MFI by XRD. Chemical analysis gave the product composition Si / Al=210.5, Si / B=19.27. The sample was calcined at 580°C for 6 hours and the BET surface area was 287 m 2 / g, the micropore volume is 0.145cc / g, and the total pore volume is 0.157cc / g.

[0095] Example 6

[0096] An alumina-borosilicate solution was prepared by first mixing 3.74 g aluminum nitrate nonahydrate, 70.39 g boric acid, 54.0 g ethylenediamine, 30.45 g TPAOH (40% solution) and 796.39 g water while stirring vigorously. After thorough mixing, 445.03 g Ludox HS-40 (SiO2, mass-40%). The reaction mixture was homogenized with a high-speed mechanical stirrer for 20 minutes and transferred to a 2-LParr Hastelloy stirred autoclave. The mixture was crystallized at 175°C while stirring at 300 RPM for 88 hours. The solid product was recovered by filtration, washed with deionized water, and dried at 100°C. The product was identified as MFI by XRD. Chemical analysis gave the product composition Si / Al=295.3, Si / B=18.85. The sample was calcined at 580°C for 6 hours and the BET surface area was 285 m 2 / g, the micropore volume is 0.144cc / g, and the total pore volume is 0.154cc / g.

[0097] Comparative Example 6A

[0098] An alumina-borosilicate solution was prepared by first mixing 3.02 g aluminum nitrate nonahydrate, 47.3 g boric acid, 306.99 g TPAOH (40% solution), and 743.6 g water while stirring vigorously. After thorough mixing, 299.09 g Ludox HS-40 (SiO2, mass-40%) was added. The reaction mixture was homogenized with a high-speed mechanical stirrer for 20 minutes and transferred to a 2-L Parr Hastelloy stirred autoclave. The mixture was crystallized at 175°C while stirring at 300 RPM for 88 hours. The solid product was recovered by filtration, washed with deionized water, and dried at 100°C. The product was identified as MFI by XRD. Chemical analysis gave the product composition Si / Al=240, Si / B=35. The sample was calcined at 580°C for 6 hours and the BET surface area was 342 m 2 / g, the micropore volume is 0.173cc / g, and the total pore volume is 0.184cc / g.

[0099] Comparative Example 6B

[0100] Tetrapropylammonium (TPA) was used as OSDA to synthesize zeolite silicalite with a target SiO2 / Al2O3 ratio of 500. The Si / Al ratio of the resulting zeolite after calcination to remove the organic template was 236 and the BET surface area was 353 m 2 / gm, the micropore volume is 0.170cc / g, and the total pore volume is 0.209cc / g.

[0101] Table 3

[0102] Example <![CDATA[SiO2 / Al2O3 target]]> <![CDATA[SiO2 / Al2O3]]> <![CDATA[Si / B2O3]]> BET SA uPV Total PV 4 221 221 42.3 287 0.143 0.164 4A 200 175 70 344 0.171 0.190 4B 190 199 Boron Free 358 0.184 0.208 5 400 421 38.55 287 0.145 0.157 6 591 590 37.7 285 0.144 0.154 6A 500 480 70 342 0.173 0.184 6B 500 472 Boron Free 353 0.170 0.209

[0103] Example 7 (Catalyst Preparation)

[0104] Representative and comparative examples of the aforementioned zeolite MFI can be formulated into extrudates or spray-dried particles containing 10% to 75% zeolite and 25% to 90% binder. The binders are silica, alumina and silica-alumina. Clay binders are incorporated into the formation at a content of 20% to 60% to densify and strengthen the spray-dried particles. Preferably, alkaline earth metal oxides and / or phosphates such as MgO are incorporated into the catalyst formulation to achieve para-xylene selectivity in the toluene methylation process. In addition, the catalyst is preferably steamed at a severity in the range of 500° C. to 1100° C. over a period of 30 minutes to 48 hours at a steam content greater than 80%.

[0105] Example 8 (Toluene Methylation Test)

[0106] The MFI zeolite disclosed in the subject matter can be deployed under the following process conditions: a toluene to methanol molar ratio in the range of 1.5 to 6.0, a temperature in the range of 400°C to 675°C, a WHSV in the range of 2 hr -1 Up to 20 hours -1 The catalyst may be present in a range of 100 psig to 1000 psig. Optionally, H2, H2O or H2 and H2O are co-fed with toluene and methanol to improve para-xylene selectivity and methanol utilization. Methanol utilization is expected to be greater than 50% or greater than 60% or greater than 70% or greater than 80%. The molar ratio of H2 / (toluene+methanol) and H2O / (toluene+methanol) may be in the range of 0.1 to 3.0, preferably 0.1 to 2.0 and most preferably 0.2 to 1.5. The catalyst may be deployed in a fixed bed process with occasional regeneration or in a fluidized bed or riser bed with frequent regeneration.

[0107] Specific implementation plan

[0108] While the following is described in conjunction with specific embodiments, it should be understood that this description is intended to illustrate and not to limit the scope of the foregoing description and the appended claims.

[0109] A first embodiment of the invention is a process for producing para-xylene comprising contacting a feed stream comprising an oxygenate feedstock and an aromatic feedstock comprising toluene with a catalyst, converting the feedstream to a product under reaction conditions, and recovering a product comprising para-xylene, wherein the catalyst comprises an improved MFI zeolite having a SiO2 / Al2O3 ratio of 50 to 600 in calcined and ion-exchanged form and having a low number of proximal framework aluminum sites characterized by an initial xylene selectivity of greater than 70% in a TM diagnostic test. An embodiment of the invention is one, any, or all of the preceding embodiments in this paragraph up to the first embodiment in this paragraph, wherein the product comprises one or more xylenes. An embodiment of the invention is one, any, or all of the preceding embodiments in this paragraph up to the first embodiment in this paragraph, wherein the SiO2 / Al2O3 ratio is 80 to 550. Embodiments of the invention are one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the low number of proximal framework aluminum sites is further characterized by a value of less than 18% by a cobalt titration technique. Embodiments of the invention are one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the improved MFI zeolite further comprises a heteroatom Q selected from the group consisting of boron, gallium, indium and iron and mixtures thereof. Embodiments of the invention are one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the molar ratio of Si / Q is between 2 and 100. Embodiments of the invention are one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the improved MFI zeolite comprises between 10% and 75% catalyst by weight. Embodiments of the invention are one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the catalyst further comprises greater than 0 wt% and less than 5 wt% phosphorus. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the catalyst also comprises greater than 0 wt % and less than 1 wt % calcium, magnesium or a mixture thereof. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the oxygen-containing compound is selected from methanol, dimethyl ether, dimethyl carbonate or a mixture thereof. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the reaction conditions include a maximum temperature of 400° C. to 675° C.An embodiment of the invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the reaction conditions include a pressure of 10 kPa to 5,000 kPa. An embodiment of the invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the reaction conditions include a molar ratio of aromatic feedstock to oxygenate of 0.5:1 to 10:1. An embodiment of the invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the reaction conditions include 0.1 hr. -1 Up to 20 hours -1 The weight hourly space velocity (WHSV) of the present invention is one, any one or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the feed stream comprises a diluent selected from the group consisting of H2, H2O, H2 and combinations thereof. The present invention is one, any one or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the molar ratio of the diluent to the aromatic feedstock and the oxygenate feedstock may be in the range of 0.1 to 3.0.

[0110] A second embodiment of the invention is a process for producing para-xylene comprising contacting a feed stream comprising an oxygenate feedstock and an aromatic feedstock comprising toluene with a catalyst, converting the feedstream to a product under reaction conditions, and recovering the product comprising para-xylene, wherein the catalyst comprises an improved MFI zeolite having a SiO2 / Al2O3 ratio of 100 to 500 in calcined and ion exchanged form, the improved MFI zeolite comprising heteroatoms Q selected from the group consisting of boron, gallium, indium and iron and mixtures thereof, wherein the molar ratio of Si / Q is between 2 and 100, and the improved MFI zeolite has a low number of proximal framework aluminum sites characterized by an initial xylene selectivity of greater than 70% in a TM diagnostic test. An embodiment of the invention is one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the reaction conditions comprise a molar ratio of aromatic feedstock to oxygenate of 0.5:1 to 10:1, 0.1 hr -1 Up to 20 hours -1 The weight hourly space velocity (WHSV) of 1,000 kPa and the pressure of 10 kPa to 5,000 kPa.

[0111] A third embodiment of the invention is a process for producing para-xylene comprising contacting a feed stream comprising methanol and toluene with a catalyst, converting the feed stream to a product under reaction conditions, and recovering the product comprising para-xylene, wherein between 10% and 75% by weight of the catalyst comprises an improved MFI zeolite having a SiO2 / Al2O3 ratio of 100 to 500 in calcined and ion exchanged form, the improved MFI zeolite comprising heteroatoms Q selected from the group consisting of boron, gallium, indium and iron and mixtures thereof, wherein the molar ratio of Si / Q is between 2 and 100, and the improved MFI zeolite has a low number of proximal framework aluminum sites characterized by an initial xylene selectivity of greater than 70% in a TM diagnostic test. An embodiment of the invention is one, any or all of the previous embodiments in this paragraph up to the third embodiment in this paragraph, wherein the reaction conditions comprise a molar ratio of aromatic feed to oxygenate of 0.5:1 to 10:1, 0.1 hr -1 Up to 20 hours -1 The invention is one, any or all of the previous embodiments in this paragraph up to the third embodiment in this paragraph, wherein the product has a methyl to phenyl ratio greater than 1.75 and less than 2.0. The invention is one, any or all of the previous embodiments in this paragraph up to the third embodiment in this paragraph, wherein the methanol utilization is greater than 60%.

[0112] Although there is no further detailed description, it is believed that those skilled in the art can utilize the present invention to the greatest extent by using the foregoing description and can easily determine the essential characteristics of the present invention without departing from the spirit and scope of the present invention to make various changes and modifications of the present invention and adapt it to various usages and conditions. Therefore, the aforementioned preferred specific embodiments should be understood as merely illustrative and not to limit the rest of the present disclosure in any way, and are intended to cover various modifications and equivalent arrangements included within the scope of the appended claims.

[0113] In the foregoing, all temperatures are set forth in degrees Celsius and all parts and percentages are by weight unless otherwise indicated.

Claims

1. A method for producing paraxylene, include: contacting a feed stream comprising an oxygenate feedstock and an aromatic feedstock comprising toluene with a catalyst, converting the feed stream to a product under reaction conditions, and recovering a product comprising para-xylene, wherein the catalyst comprises an improved MFI zeolite having a SiO2 / Al2O3 ratio of 50 to 600 in calcined and ion exchanged form and having a low number of proximal framework aluminum sites characterized by an initial xylene selectivity of greater than 70% in a TM diagnostic test 2. The process of claim 1, wherein the product comprises one or more xylenes.

3. The method according to claim 1, wherein the SiO2 / Al2O3 ratio is 80 to 550.

4. The method of claim 1 wherein the low number of framework aluminum sites is further characterized by a value of less than 18% by a cobalt titration technique.

5. The process according to claim 1, wherein the improved MFI zeolite further comprises a heteroatom Q selected from the group consisting of boron, gallium, indium and iron and mixtures thereof.

6. The process according to claim 5, wherein the molar ratio of Si / Q is between 20 and 100.

7. The process of claim 1 wherein said modified MFI zeolite comprises between 10 and 75% by weight of said catalyst.

8. The method of claim 1, wherein the catalyst further comprises greater than 0 wt% and less than 5 wt% phosphorus.

9. The method of claim 8, wherein the catalyst further comprises greater than 0 wt% and less than 1 wt% calcium, magnesium or a mixture thereof.

10. The method according to claim 1, wherein the oxygen-containing compound is selected from methanol, dimethyl ether, dimethyl carbonate or a mixture thereof.

11. The method of claim 1, wherein the reaction conditions include a maximum temperature of 400°C to 675°C 12. The method of claim 1, wherein the reaction conditions include a pressure of 10 kPa to 5,000 kPa.

13. The process of claim 1 wherein the reaction conditions include a molar ratio of aromatic feedstock to oxygenate of 0.5:1 to 10:

1.

14. The process of claim 1, wherein the reaction conditions comprise a weight hourly space velocity (WHSV) of 0.1 hr-1 to 20 hr-1.

15. The process of claim 1, wherein the feed stream comprises a diluent selected from the group consisting of H2, H2O, H2, and combinations thereof.

Citation Information

Patent Citations

  • Process for aromatic alkylation

    US20050143613A1

  • Selective para-xylene production by toluene methylation

    US6504072B1

  • Increased oligomer selectivity from olefin oligomerization by incorporation of boron