Photosensitive resin composition set, optical waveguide and method for manufacturing same, optoelectric hybrid-mounted substrate, sheet set, resin composition for core, resin composition
By using a specific photosensitive resin composition kit, the refractive index difference of the optical waveguide is controlled, solving the problem of high transmission loss and realizing the manufacture of low-loss optical waveguides suitable for high-speed communication environments.
Patent Information
- Application Number
- CN202380018346.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-27
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-08
AI Technical Summary
Existing photosensitive resin compositions used in the manufacture of optical waveguides suffer from high transmission loss, making it difficult to meet the requirements of high-speed communication.
By employing a photosensitive resin composition kit containing phenolic resin, photoacid generator, and crosslinking agent, and controlling the refractive index difference between the core and coating resin compositions, an optical waveguide with an aperture number NA in the range of 0.05 to 0.4 is formed, thereby reducing transmission loss.
It effectively reduces the transmission loss of optical waveguides, improves communication efficiency, and is suitable for high-speed communication environments.
Smart Images

Figure BDA0004958279510000031 
Figure BDA0004958279510000081 
Figure BDA0004958279510000091
Abstract
Description
Technical Field
[0001] The present invention relates to a photosensitive resin composition kit, an optical waveguide and a method for producing the same, an optoelectronic hybrid substrate, a sheet kit, a core resin composition, a cladding resin composition, and a resin sheet. Background Art
[0002] Advances in technologies such as 5G communications, autonomous driving, IoT, artificial intelligence, and big data are driving the demand for ultra-high-speed and high-capacity communications. Semiconductor packaging, which underpins these technologies, has traditionally handled high-speed communications by circulating high-frequency currents. However, in recent years, the issues of noise generation, communication loss, and heat dissipation caused by high-speed communications have become increasingly apparent. To address these issues, efforts have been actively underway to integrate optical circuits into power wiring boards to achieve energy savings, low latency, and high-speed communications (Patent Documents 1 and 2).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2019-211540
[0006] Patent Document 2: Japanese Patent No. 5771978 Summary of the Invention
[0007] Problems to be solved by the invention
[0008] In particular, research into the introduction of silicon photonics technology is being actively pursued in data centers, where high-speed transmission is crucial. Silicon photonics technology is highly compatible with conventional LSI manufacturing processes. Therefore, by leveraging silicon photonics, leveraging technologies developed within electronic circuit integration, it is expected that nanometer-sized fine-line waveguides can be formed at low cost.
[0009] For example, silicon photonics technology promises to enable the use of fine-line waveguides to form optical integrated circuits on chips. When manufacturing an optoelectronic hybrid substrate incorporating such a chip, optical waveguides are required to be incorporated into the substrate to extract signal light from the fine-line waveguides within the chip and connect them to inter-chip wiring. To efficiently form fine optical waveguides, it is desirable to form the optical waveguides from cured photosensitive resin compositions. However, optical waveguides formed using conventional photosensitive resin compositions suffer from high transmission loss.
[0010] The present invention has been made in view of the aforementioned problems, and its object is to provide a photosensitive resin composition kit capable of producing an optical waveguide with low transmission loss; an optical waveguide capable of reducing transmission loss and a method for producing the same; an optoelectronic hybrid substrate including the optical waveguide; and a sheet kit, a core resin composition, a cladding resin composition, and a resin sheet capable of forming an optical waveguide with low transmission loss.
[0011] Means for solving problems
[0012] The present inventors conducted intensive research to address the aforementioned issues. As a result, they discovered that combining a core resin composition comprising (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent with a cladding resin composition comprising (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent can suppress light transmission loss when producing an optical waveguide having an aperture (NA) within a specific range, thereby completing the present invention.
[0013] That is, the present invention includes the following technical solutions.
[0014] [1] A photosensitive resin composition kit comprising a core resin composition and a coating resin composition,
[0015] The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent.
[0016] The coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent.
[0017] The number of openings NA represented by the following formula (1) is greater than 0.05 and less than 0.4.
[0018] [Mathematical formula 1]
[0019]
[0020] (In formula (1),
[0021] n core represents the refractive index of the cured product of the core resin composition,
[0022] n clad Refractive index of the cured product of the coating resin composition.
[0023] [2] The photosensitive resin composition kit according to [1], wherein the crosslinking agent (C) is an amino resin.
[0024] [3] The photosensitive resin composition kit according to [1] or [2], wherein the core resin composition contains (D) a polymer having a weight average molecular weight of 2500 or more.
[0025] [4] The photosensitive resin composition kit according to any one of [1] to [3], wherein the core resin composition contains (E) a compound represented by the following formula (E-1).
[0026] [Chemistry 1]
[0027]
[0028] (In formula (E-1), R e1 、R e2 and R e3 Each independently represents a hydrogen atom or a hydrocarbon group. e1 With R e2 Optional bond to form a ring.)
[0029] [5] The photosensitive resin composition kit according to any one of [1] to [4], which is a photosensitive resin composition kit for producing an optical waveguide.
[0030] [6] The photosensitive resin composition kit according to any one of [1] to [5], which is a photosensitive resin composition kit for producing an optical waveguide capable of transmitting light having a wavelength of 1300 nm to 1320 nm.
[0031] [7] The photosensitive resin composition kit according to any one of [1] to [6], which is a photosensitive resin composition kit for producing a single-mode optical waveguide.
[0032] [8] An optical waveguide comprising a core layer and a cladding layer,
[0033] The core layer comprises a cured product of a core resin composition, wherein the core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent.
[0034] The coating layer comprises a cured product of a coating resin composition, wherein the coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent.
[0035] The number of openings NA represented by the following formula (1) is greater than 0.05 and less than 0.4.
[0036] [Mathematical formula 2]
[0037]
[0038] (In formula (1),
[0039] n core represents the refractive index of the cured product of the core resin composition,
[0040] n clad Refractive index of the cured product of the coating resin composition.
[0041] [9] The optical waveguide according to [8], which is capable of transmitting light with a wavelength of 1300 nm to 1320 nm.
[0042]
[10] The optical waveguide according to [8] or [9], which is a single-mode optical waveguide.
[0043]
[11] An optoelectronic hybrid substrate comprising the optical waveguide according to any one of [8] to
[10] .
[0044]
[12] A method for manufacturing an optical waveguide, comprising:
[0045] forming a first composition layer comprising a coating resin composition;
[0046] a step of subjecting the first composition layer to an exposure treatment;
[0047] a step of curing the first composition layer;
[0048] forming a second composition layer comprising a core resin composition on the first composition layer;
[0049] a step of subjecting the second composition layer to an exposure treatment;
[0050] a step of developing the second composition layer;
[0051] a step of curing the second composition layer;
[0052] forming a third composition layer comprising a coating resin composition on the second composition layer;
[0053] a step of subjecting the third composition layer to an exposure treatment; and
[0054] a step of curing the third composition layer,
[0055] The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent.
[0056] The coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent.
[0057] The number of openings NA represented by the following formula (1) is greater than 0.05 and less than 0.4.
[0058] [Mathematical formula 3]
[0059]
[0060] (In formula (1),
[0061] n core represents the refractive index of the cured product of the core resin composition,
[0062] n clad Refractive index of the cured product of the coating resin composition.
[0063]
[13] A sheet set comprising a core resin sheet and a covering resin sheet,
[0064] The core resin sheet includes a core resin composition layer comprising a core resin composition containing (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent.
[0065] The coating resin sheet includes a coating resin composition layer comprising a coating resin composition containing (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent.
[0066] The number of openings NA represented by the following formula (1) is greater than 0.05 and less than 0.4.
[0067] [Formula 4]
[0068]
[0069] (In formula (1),
[0070] n core represents the refractive index of the cured product of the core resin composition,
[0071] n clad Refractive index of the cured product of the coating resin composition.
[0072]
[14] A core resin composition for forming a core layer in a cladding layer, wherein the cladding layer comprises a cured product of the cladding resin composition, wherein the cladding resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent,
[0073] The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent.
[0074] The number of openings NA represented by the following formula (1) is greater than 0.05 and less than 0.4.
[0075] [Formula 5]
[0076]
[0077] (In formula (1),
[0078] n core represents the refractive index of the cured product of the core resin composition,
[0079] n clad Refractive index of the cured product of the coating resin composition.
[0080]
[15] A resin sheet comprising a resin composition layer comprising the core resin composition according to
[14] .
[0081]
[16] A coating resin composition for forming a coating layer covering a core layer, wherein the core layer comprises a cured product of the core resin composition, wherein the core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent,
[0082] The coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent.
[0083] The number of openings NA represented by the following formula (1) is greater than 0.05 and less than 0.4.
[0084] [Formula 6]
[0085]
[0086] (In formula (1),
[0087] n core represents the refractive index of the cured product of the core resin composition,
[0088] n clad Refractive index of the cured product of the coating resin composition.
[0089]
[17] A resin sheet comprising a resin composition layer comprising the coating resin composition according to
[16] .
[0090] Effects of the Invention
[0091] According to the present invention, there are provided a photosensitive resin composition kit capable of producing an optical waveguide with low transmission loss; an optical waveguide capable of reducing transmission loss and a method for producing the same; an optoelectronic hybrid substrate including the optical waveguide; and a sheet kit, a core resin composition, a cladding resin composition, and a resin sheet capable of forming an optical waveguide with low transmission loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0092] Figure 1 This is a perspective view schematically showing an optical waveguide according to one embodiment of the present invention.
[0093] Figure 2 This is a schematic cross-sectional view for explaining step (I) of the method for manufacturing an optical waveguide according to one embodiment of the present invention.
[0094] Figure 3 This is a schematic cross-sectional view for explaining step (III) of the method for manufacturing an optical waveguide according to one embodiment of the present invention.
[0095] Figure 4 This is a schematic cross-sectional view for explaining step (IV) of the method for manufacturing an optical waveguide according to one embodiment of the present invention.
[0096] Figure 5 This is a schematic cross-sectional view for explaining step (V) of the method for manufacturing an optical waveguide according to one embodiment of the present invention.
[0097] Figure 6 This is a schematic cross-sectional view for explaining step (VI) of the method for manufacturing an optical waveguide according to one embodiment of the present invention.
[0098] Figure 7 This is a schematic cross-sectional view for explaining step (VII) of the method for manufacturing an optical waveguide according to one embodiment of the present invention.
[0099] Figure 8 This is a schematic cross-sectional view for explaining step (VIII) of the method for manufacturing an optical waveguide according to one embodiment of the present invention.
[0100] Figure 9 This is a schematic cross-sectional view for explaining step (X) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. DETAILED DESCRIPTION
[0101] The present invention will be described in detail below with reference to the embodiments and examples. However, the present invention is not limited to the embodiments and examples listed below, and can be implemented with any modifications within the scope of the claims and their equivalents.
[0102] In the following description, unless otherwise specified, the term "(meth)acrylic acid" includes acrylic acid, methacrylic acid, and a combination thereof, and the term "(meth)acrylate" includes acrylate, methacrylate, and a combination thereof.
[0103] [1. Overview of Photosensitive Resin Composition Kit]
[0104] A photosensitive resin composition kit according to one embodiment of the present invention includes a core resin composition and a cladding resin composition. The core resin composition and the cladding resin composition can be used to produce an optical waveguide having a core layer and a cladding layer, wherein the core layer comprises a cured product of the core resin composition and the cladding layer comprises a cured product of the cladding resin composition.
[0105] The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent. In addition, the coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent. Furthermore, according to the refractive index n of the cured product of the core resin composition, coreand the refractive index n of the cured product of the coating resin composition clad , the number of openings NA defined by the following formula (1) falls within a specific range.
[0106] [Formula 7]
[0107]
[0108] The photosensitive resin composition kit described in this embodiment enables the production of an optical waveguide with low transmission loss. Specifically, when the core layer is formed from a cured product of a core resin composition and the cladding layer is formed from a cured product of a cladding resin composition, an optical waveguide comprising a core layer and a cladding layer can be produced. An optical waveguide produced in this manner can suppress the transmission loss of light transmitted therethrough.
[0109] Since the core resin composition and the cladding resin composition are photosensitive resin compositions, fine optical waveguides can be efficiently produced by a method generally including exposure and development. In addition, the optical waveguides generally have excellent reflow resistance.
[0110] [2. Core resin composition]
[0111] The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent. The core resin composition may be a photosensitive resin composition, and thus a core layer having a desired pattern can be formed by a method comprising exposure and development. The "pattern" of the core layer, unless otherwise specified, refers to the shape of the core layer as viewed in the thickness direction.
[0112] Specifically, when exposed to light, the photoacid generator (B) typically generates an acid. This acid promotes the crosslinking reaction of the crosslinker (C). Consequently, the solubility of the core resin composition in the developer solution can be reduced in the light-exposed portion (hereinafter sometimes referred to as the "exposed portion"). Consequently, the core resin composition can form a latent image upon exposure.
[0113] In addition, the core resin composition can usually be removed using a developer. In particular, (A) phenolic resin is usually alkali-soluble, and therefore, the core resin composition can be well removed using an alkali developer. Thus, the core resin composition of the portion not irradiated by light (hereinafter sometimes referred to as the "non-exposed portion") can be removed using a developer to develop the latent image. "Alkali-soluble" means that the component having the alkali solubility can be dissolved in an alkaline aqueous solution (e.g., a 2.38% by mass tetramethylammonium hydroxide aqueous solution).
[0114] Therefore, a core layer with a fine pattern can be formed using a method comprising exposure and development using a core resin composition. This core layer can be combined with a cladding layer formed from a cured product of the cladding resin composition to produce an optical waveguide capable of transmitting light through the core layer. Furthermore, as described above, the optical waveguide comprising the core layer and cladding layer can suppress light transmission loss.
[0115] Furthermore, the core resin composition generally has excellent resolution. Furthermore, the cured product of the core resin composition generally has excellent mechanical strength such as elongation at break, and also has excellent heat resistance such as reflow resistance.
[0116] [2.1.(A) Phenolic resin]
[0117] The core resin composition includes a phenolic resin (A) as component (A). The phenolic resin (A) is soluble in a suitable developer, particularly an alkaline developer. Furthermore, the phenolic resin (A) is preferably capable of reacting with the crosslinking agent (C) to form a bond. This reaction can effectively reduce the solubility of the core composition in the developer by reacting with the crosslinking agent (C).
[0118] The (A) phenolic resin contains phenolic hydroxyl groups in its molecule. A phenolic hydroxyl group refers to a hydroxyl group bonded to an aromatic ring such as a benzene ring or a naphthalene ring. The number of phenolic hydroxyl groups possessed by the (A) phenolic resin may be one per molecule, or may be two or more. From the perspective of promoting the crosslinking reaction by the (C) crosslinking agent and increasing the degree of crosslinking to improve the mechanical strength of the cured product, the (A) phenolic resin preferably has two or more phenolic hydroxyl groups per molecule.
[0119] (A) phenolic resin can be used alone or in combination of two or more. Preferred examples of (A) phenolic resin include compounds having a structure represented by the following formula (A-1), compounds having a structure represented by the following formula (A-2), and compounds having a structure represented by the following formula (A-3). In the following description, the compound having a structure represented by the following formula (A-1), the compound having a structure represented by the following formula (A-2), and the compound having a structure represented by the following formula (A-3) are sometimes referred to as component (A-1), component (A-2), and component (A-3), respectively. When these components (A-1) to (A-3) are used, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition, and the mechanical strength and heat resistance of the cured product of the core resin composition can usually be made particularly good.
[0120] [Chemistry 2]
[0121]
[0122] (In formula (A-1), R1 Each independently represents a divalent hydrocarbon group optionally having a substituent, X 1 Each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n1 represents an integer of 0 to 4, and m1 represents an integer of 1 to 200. * represents a connecting bond.
[0123] In formula (A-2), R 2 represents a divalent group represented by the following formula (r-1), a divalent group represented by the following formula (r-2), a divalent group represented by the following formula (r-3), or a divalent group formed by a combination thereof, and X 2 and X 3 Each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. n2 and n3 each independently represent an integer of 0 to 4.
[0124] In formula (A-3), R 3 represents a divalent group represented by the following formula (r-1), a divalent group represented by the following formula (r-2), a divalent group represented by the following formula (r-3), or a divalent group formed by a combination thereof, and X 4 and X 5 Each independently represents an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a halogen atom, or a monovalent heterocyclic group optionally having a substituent. n4 and n5 each independently represent an integer of 0 to 3.
[0125] [Chemistry 3]
[0126]
[0127] (In formula (r-1), R 11 and R 12 Each independently represents a hydrogen atom, an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a monovalent heterocyclic group optionally having a substituent, an amino group, a carbonyl group, a carboxyl group, or a group consisting of a combination thereof, and R 11 and R 12 They are optionally bonded to each other to form a ring. * represents a connecting bond.
[0128] In formula (r-2), X 11 Each independently represents an alkyl group which may have a substituent. p1 represents an integer of 0 to 4. * represents a connecting bond.
[0129] In formula (r-3), X 12 and X 13 Each independently represents an alkyl group which may have a substituent. p2 and p3 each independently represent an integer of 0 to 4. * represents a connecting bond.
[0130] -Component (A-1): a compound having a structure represented by formula (A-1)-
[0131] The component (A-1) is a compound having a structure represented by the following formula (A-1). The component (A-1) may be used alone or in combination of two or more.
[0132] [Chemistry 4]
[0133]
[0134] (In formula (A-1), R 1 Each independently represents a divalent hydrocarbon group optionally having a substituent, X 1 Each independently represents an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a halogen atom, or a monovalent heterocyclic group optionally having a substituent. n1 represents an integer from 0 to 4, and m1 represents an integer from 1 to 200. * represents a connecting bond.
[0135] In formula (A-1), X 1 Each independently represents an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a halogen atom, or a monovalent heterocyclic group optionally having a substituent. 1 , preferably an alkyl group optionally having a substituent, an aryl group optionally having a substituent, or a halogen atom, more preferably an alkyl group optionally having a substituent and an aryl group optionally having a substituent, further preferably an alkyl group optionally having a substituent.
[0136] The alkyl group may be a linear, branched, or cyclic alkyl group. Furthermore, the cyclic alkyl group may be either monocyclic or polycyclic. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, isopropyl, sec-butyl, tert-butyl, 2-methylpropyl, and 3-heptyl. Among these, a methyl group is particularly preferred.
[0137] The aryl group is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and still more preferably an aryl group having 6 to 10 carbon atoms. Examples of the aryl group include a phenyl group and a naphthyl group.
[0138] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and a fluorine atom is preferred.
[0139] As a monovalent heterocyclic group, a monovalent heterocyclic group having 3 to 21 carbon atoms is preferred, a monovalent heterocyclic group having 3 to 15 carbon atoms is more preferred, and a monovalent heterocyclic group having 3 to 9 carbon atoms is further preferred. The monovalent heterocyclic group also includes a monovalent aromatic heterocyclic group (heteroaryl). Examples of the monovalent heterocyclic group include, for example, thienyl, pyrrolyl, furyl, furyl, pyridyl, pyridazinyl, pyrimidinyl, pyrazinyl, triazinyl, pyrrolidinyl, piperidinyl, quinolinyl, and isoquinolinyl. Among them, pyrrolidinyl is preferred. The monovalent heterocyclic group refers to a group obtained by removing one hydrogen atom from the heterocycle of a heterocyclic compound.
[0140] X 1 The alkyl group, aryl group, and monovalent heterocyclic group represented by may optionally have a substituent. Examples of the substituent include, for example, a halogen atom such as a fluorine atom, -OH, -O-C 1-6 alkyl group, -N(C 1-6 alkyl)2, C 1-6 alkyl group, C 6-10 aryl group, -NH2, -NH(C 1-6 alkyl), -CN, -C(O)O-C 1-6 alkyl group, -C(O)H, -NO2, etc.
[0141] In this specification, the expression "optionally having a substituent" means unsubstituted or having a substituent unless otherwise specified. The number of substituents may be 1 or 2 or more. In one example, the number of substituents can usually be 1 to 5 (preferably 1, 2, or 3). When there are multiple substituents, these substituents may be the same or different from each other. In addition, in this specification, the term "C p-q " (p and q are positive integers, and p < q.) represents that the number of carbon atoms of the organic group described immediately after this term is p to q. For example, the expression "C 1-6 alkyl group" represents an alkyl group having 1 to 6 carbon atoms.
[0142] In formula (A-1), R 1 each independently represents a divalent hydrocarbon group optionally having a substituent. Preferably, R 1 each independently represents a divalent group represented by formula (r-1).
[0143] [Chemical formula 5]
[0144]
[0145] (In formula (r-1), R 11 and R 12 each independently represents a hydrogen atom, an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a monovalent heterocyclic group optionally having a substituent, an amino group, a carbonyl group, a carboxyl group, or a group formed by a combination thereof, R11 and R 12 They are optionally bonded to each other to form a ring. * represents a connecting bond.)
[0146] In formula (r-1), R 11 and R 12 Each independently represents a hydrogen atom, an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a monovalent heterocyclic group optionally having a substituent, an amino group, a carbonyl group, a carboxyl group, or a group consisting of a combination thereof, and R 11 and R 12 They may be bonded to each other to form a ring. Among them, a hydrogen atom and an alkyl group are preferred.
[0147] R 11 and R 12 The alkyl group optionally having a substituent, the aryl group optionally having a substituent and the monovalent heterocyclic group optionally having a substituent may be combined with X in formula (A-1). 1 The alkyl group which may have a substituent, the aryl group which may have a substituent, and the monovalent heterocyclic group which may have a substituent are the same as those represented.
[0148] Examples of the group formed by the combination thereof include a group formed by a combination of an alkyl group and a carbonyl group, a group formed by a combination of an aryl group and a carbonyl group, a group formed by a combination of an alkyl group, an amino group and a carbonyl group, and a group formed by a combination of an aryl group, an amino group and a carbonyl group.
[0149] R 11 and R 12 They are optionally bonded to each other to form a ring. 11 and R 12 The optionally formed ring structure also includes spiro rings and fused rings. In this case, R 11 and R 12 Preferred are groups forming a cyclopentane ring, a cyclohexane ring, a 2,2-dimethyl-4-methylcyclohexane ring, a fluorene ring, a pyrrolidine ring, or a γ-lactam ring.
[0150] Specific examples of the divalent group represented by formula (r-1) include the following groups: In the formula, "*" represents a connecting bond.
[0151] [Chemistry 6]
[0152]
[0153] [Chemistry 7]
[0154]
[0155] In formula (A-1), R 1Each may independently be a divalent group represented by formula (r-4).
[0156] [Chemistry 8]
[0157]
[0158] (In formula (r-4), R 13 and R 14 Each independently represents an alkylene group, X 14 Each independently represents an alkyl group which may have a substituent, p4 represents an integer of 0 to 4, and m2 represents an integer of 1 to 3. * represents a connecting bond.
[0159] In formula (r-4), R 13 and R 14 Each independently represents an alkylene group. The number of carbon atoms in the alkylene group is usually 1 or more, preferably 18 or less, more preferably 12 or less, further preferably 6 or less, and particularly preferably 4 or less. Examples of the alkylene group include methylene, ethylene, propylene, and butylene.
[0160] In formula (r-4), X 14 Each independently represents an alkyl group which may have a substituent. 14 Can be combined with X in formula (A-1) 1 The alkyl groups optionally having substituents represented are the same.
[0161] In formula (r-4), p4 represents an integer of 0 to 4, preferably an integer of 0 to 3, more preferably 0 or 1, and particularly preferably 0.
[0162] In formula (r-4), m2 represents an integer of 1 to 3, preferably an integer of 1 to 2, and particularly preferably 2.
[0163] In formula (A-1), R 1 Each may independently be a divalent group represented by formula (r-5).
[0164] [Chemistry 9]
[0165]
[0166] (In formula (r-5), X 15 Each independently represents an alkyl group which may have a substituent, and p5 represents an integer from 0 to 12. * represents a connecting bond.
[0167] In formula (r-5), X 15 Each independently represents an alkyl group which may have a substituent. 15 Can be combined with X in formula (A-1) 1 The alkyl groups optionally having substituents represented are the same.
[0168] In formula (r-5), p5 represents an integer of 0 to 12, preferably an integer of 0 to 2, more preferably 0 or 1, and particularly preferably 0.
[0169] R 1 The OH group of the phenol portion in formula (A-1) is preferably bonded to any one of the ortho, meta, and para positions, more preferably to any one of the meta and para positions, and even more preferably to a mixture of the meta and para positions. 1 The structure and R bonded to the meta position relative to the OH group of the phenol portion in formula (A-1) 1 In the case of a structure in which R is bonded to the para position relative to the OH group of the phenol portion in formula (A-1), 1 The mass of the structure bonded to the meta position is set as m, and R 1 The mass of the structure bonded to the para position is defined as p. In this case, the mixing ratio (m:p) is preferably 1:0.1 to 1:10, more preferably 1:0.1 to 1:5, further preferably 1:0.1 to 1:2, and particularly preferably 1:0.5 to 1:1. 1 In the case of a divalent group represented by formula (r-1), the mixing ratio (m:p) is particularly preferably within the aforementioned range.
[0170] In formula (A-1), n1 represents an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably 0 or 1. 1 When it is a divalent group represented by formula (r-1), n1 is particularly preferably 1. 1 In the case of a divalent group represented by formula (r-4) or a divalent group represented by formula (r-5), n1 is particularly preferably 0.
[0171] In formula (A-1), m1 represents an integer of 1 to 200. Specifically, m1 is usually 1 or more, and may be 2 or more. Furthermore, m1 is usually 200 or less, preferably 150 or less, more preferably 100 or less, and particularly preferably 50 or less.
[0172] Specific examples of component (A-1) include the resins represented by the following formulas (A-1-1) to (A-1-3). It should be noted that in the specific example represented by formula (A-1-1), it is preferred that the methylene groups be mixed at a ratio of 60% to 40% of the OH groups in the phenol moiety, with the methylene groups being bonded to the meta position. In the following formulas (A-1-1) to (A-1-3), n6, n7, and n8 represent integers of 1 to 200.
[0173] [Chemistry 10]
[0174]
[0175] Component (A-1) can use commercially available products. Specific examples of commercially available component (A-1) include "TR4020G" (resin represented by formula (A-1-1)) manufactured by Asahi Organic Materials Co., Ltd.; AV-light series such as "TR4050G", "TR4080G", "TR5020G", "TR5050G", "TR6020G", "TR6050G", and "TR6080G" manufactured by Asahi Organic Materials Co., Ltd.; photoresist resin series manufactured by Sumitomo Becracy Co., Ltd.; Retopt series manufactured by Gunei Chemical Industry Co., Ltd.; "PR-30-40P", "PR-100" manufactured by DIC Corporation. L", "PR-100H", "PR-50", "PR-55", "PR-56-1", "PR-56-2", "WR-101", "WR-102", "WR-103", "WR-104" and other Fenolite series; "LF-100", "LF-110", "LF-120", "LF-200", "LF-400", "LF-500" manufactured by Lignite Co., Ltd.; base resin series for photoresists, MEH-7851 series manufactured by Meiwa Chemical Co., Ltd.; J-DPP series manufactured by JFE Chemical Co., Ltd., etc.
[0176] The amount of component (A-1) is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 50% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, relative to 100% by mass of the total amount of the phenolic resin (A). When the amount of component (A-1) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be particularly improved.
[0177] The amount of component (A-1) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and even more preferably 40% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, relative to 100% by mass of the non-volatile components of the core resin composition. When the amount of component (A-1) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be particularly improved.
[0178] -Component (A-2): a compound having a structure represented by formula (A-2)-
[0179] The component (A-2) is a compound having a structure represented by the following formula (A-2). The component (A-2) may be used alone or in combination of two or more.
[0180] [Chemistry 11]
[0181]
[0182] (In formula (A-2), R 2 represents a divalent group represented by the following formula (r-1), a divalent group represented by the following formula (r-2), a divalent group represented by the following formula (r-3), or a divalent group formed by a combination thereof, and X 2 and X 3 Each independently represents an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a halogen atom, or a monovalent heterocyclic group optionally having a substituent. n2 and n3 each independently represent an integer of 0 to 4.
[0183] [Chemistry 12]
[0184]
[0185] (In formula (r-1), R 11 and R 12 Each independently represents a hydrogen atom, an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a monovalent heterocyclic group optionally having a substituent, an amino group, a carbonyl group, a carboxyl group, or a group consisting of a combination thereof, and R 11 and R 12 They are optionally bonded to each other to form a ring. * represents a connecting bond.
[0186] In formula (r-2), X 11 Each independently represents an alkyl group which may have a substituent. p1 represents an integer of 0 to 4. * represents a connecting bond.
[0187] In formula (r-3), X 12 and X 13 Each independently represents an alkyl group which may have a substituent. p2 and p3 each independently represent an integer of 0 to 4. * represents a connecting bond.
[0188] In formula (A-2), R 2 It represents a divalent group represented by formula (r-1), a divalent group represented by formula (r-2), a divalent group represented by formula (r-3), or a divalent group formed by a combination thereof. The divalent group represented by formula (r-1) is as described above.
[0189] X in formulas (r-2) to (r-3) 11 、X 12 and X 13Each independently represents an alkyl group which may have a substituent. 11 ~X 13 Can be combined with X in formula (A-1) 1 The alkyl groups optionally having substituents represented are the same.
[0190] p1, p2, and p3 in formulae (r-2) to (r-3) each independently represent an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably 0 or 1.
[0191] Specific examples of the divalent group represented by formula (r-2) include the following groups: In the formula, "*" represents a connecting bond.
[0192] [Chemistry 13]
[0193]
[0194] Specific examples of the divalent group represented by formula (r-3) include the following groups: In the formula, "*" represents a connecting bond.
[0195] [Chemistry 14]
[0196]
[0197] Specific examples of the divalent group formed by the combination of the divalent group represented by formula (r-2) and the divalent group represented by formula (r-3), the divalent group formed by the combination of the divalent group represented by formula (r-1) and the divalent group represented by formula (r-2), and the divalent group formed by the combination of the divalent group represented by formula (r-1) and the divalent group represented by formula (r-3) include the following groups. In the formula, "*" represents a connecting bond.
[0198] [Chemistry 15]
[0199]
[0200] In formula (A-2), the OH group of the phenol portion is 2 It is preferably bonded to any of the ortho, meta, and para positions, more preferably bonded to any of the meta and para positions, and particularly preferably bonded to the para position.
[0201] In formula (A-2), X 2 and X 3 Each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. 2 and X 3 can be independently combined with X in formula (A-1) 1 same.
[0202] In formula (A-2), n2 and n3 each independently represent an integer of 0 to 4, and may be the same as n1 in formula (A-1).
[0203] Specific examples of the component (A-2) include the following groups.
[0204] [Chemistry 16]
[0205]
[0206] [Chemistry 17]
[0207]
[0208] [Chemistry 18]
[0209]
[0210] [Chemistry 19]
[0211]
[0212] [Chemistry 20]
[0213]
[0214] [Chemistry 21]
[0215]
[0216] [Chemistry 22]
[0217]
[0218] [Chemistry 23]
[0219]
[0220] [Chemistry 24]
[0221]
[0222] [Chemistry 25]
[0223]
[0224] (A-2) Component can use commercially available products. Specific examples of commercially available (A-2) components include:
[0225] "BisP-E" and "Bis-AF" manufactured by Asahi Organic Materials Co., Ltd.; "BisE" and "BisP-TMC" manufactured by Honshu Chemical Co., Ltd.; "BisA", "BisF", and "BisP-M" manufactured by Mitsui Chemicals, Inc.; "BisP-AP", "BisP-MIBK", "BisP-B", "Bis-Z", "BisP-CP", "o,o'-BPF", "BisP-IOTD", "BisP-IBTD", "BisP-DED", and "BisP-BA" manufactured by Honshu Chemical Co., Ltd. "Bis-C", "Bis26X-A", "BisOPP-A", "BisOTBP-A", "BisOCHP-A", "BisOFP-A", "BisOC-Z", "BisOC-FL", "BisOC-CP", "BisOCHP-Z", "Methylene Bis-P-CR", "TM-BPF", "BisOC-F", "Bis3M6B-IBTD", "BisOC-IST", "BisP-IST", "BisP-PRM", "BisP-LV", etc.
[0226] The amount of component (A-2) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, relative to 100% by mass of the total amount of the phenolic resin (A), and is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less. When the amount of component (A-2) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be particularly improved.
[0227] The amount of component (A-2) is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, relative to 100% by mass of the non-volatile components of the core resin composition, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less. When the amount of component (A-2) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be particularly improved.
[0228] When the mass of the (A-1) component relative to 100% by mass of the (A) phenolic resin is Wa1, and the mass of the (A-2) component relative to 100% by mass of the (A) phenolic resin is Wa2, the mass ratio Wa2 / Wa1 is preferably within a specific range. Specifically, the mass ratio Wa2 / Wa1 is preferably 0.01 or greater, more preferably 0.05 or greater, more preferably 0.1 or greater, and preferably 4 or less, more preferably 2 or less, and even more preferably 1 or less. When the mass ratio Wa2 / Wa1 is within the above range, the transmission loss of the optical waveguide can be effectively suppressed, and furthermore, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be made particularly good.
[0229] -Component (A-3): a compound having a structure represented by formula (A-3)-
[0230] The component (A-3) is a compound having a structure represented by the following formula (A-3). The component (A-3) may be used alone or in combination of two or more.
[0231] [Chemistry 26]
[0232]
[0233] (In formula (A-3), R 3 represents a divalent group represented by the aforementioned formula (r-1), a divalent group represented by the aforementioned formula (r-2), a divalent group represented by the aforementioned formula (r-3), or a divalent group formed by a combination thereof, and X 4 and X 5 Each independently represents an alkyl group optionally having a substituent, an aryl group optionally having a substituent, a halogen atom, or a monovalent heterocyclic group optionally having a substituent. n4 and n5 each independently represent an integer of 0 to 3.
[0234] In formula (A-3), R 3 represents a divalent group represented by formula (r-1), a divalent group represented by formula (r-2), a divalent group represented by formula (r-3), or a divalent group formed by a combination thereof. The divalent group represented by formula (r-1), the divalent group represented by formula (r-2), the divalent group represented by formula (r-3), and a divalent group formed by a combination thereof are as described above.
[0235] In formula (A-3), the OH group of the phenol portion is 3 It is preferably bonded to any of the ortho, meta, and para positions, more preferably bonded to any of the meta and para positions, and particularly preferably bonded to the para position.
[0236] In formula (A-3), X 4 and X5 Each independently represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a halogen atom, or a monovalent heterocyclic group which may have a substituent. 4 and X 5 can be independently combined with X in formula (A-1) 1 same.
[0237] In formula (A-3), n4 and n5 each independently represent an integer of 0 to 3. n4 and n5 each independently represent more preferably 0 or 1, and particularly preferably 0.
[0238] Specific examples of the component (A-3) include the following groups.
[0239] [Chemistry 27]
[0240]
[0241] (A-3) Component can use a commercial item. Specific examples of commercially available (A-3) component include "TBIS-RX" manufactured by Taoka Chemical Industry Co., Ltd. and the like.
[0242] The amount of component (A-3) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, relative to 100% by mass of the total amount of the phenolic resin (A), and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. When the amount of component (A-3) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be particularly improved.
[0243] The amount of component (A-3) is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, relative to 100% by mass of the non-volatile components of the core resin composition, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. When the amount of component (A-3) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be particularly improved.
[0244] -Component (A-4): Compounds other than components (A-1) to (A-3)
[0245] As the phenolic resin (A), compounds other than components (A-1) to (A-3) can be used. Examples of the phenolic resin (A) other than components (A-1) to (A-3) (hereinafter sometimes referred to as "component (A-4)") include "Marukalinka M" (polyparahydroxystyrene) manufactured by Maruzen Chemical Co., Ltd. and "SPDI" manufactured by JFE Chemical Co., Ltd.
[0246] The weight average molecular weight of the phenolic resin (A) is not particularly limited. Preferred ranges are: preferably 150 or greater, more preferably 160 or greater, and particularly preferably 170 or greater, and preferably less than 15,000, more preferably 14,000 or less, particularly preferably 13,000 or less, and may be less than 2,500. The weight average molecular weight can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).
[0247] The phenolic hydroxyl equivalent of the phenolic resin (A) is preferably 50 g / eq. or more, more preferably 100 g / eq. or more, and is preferably less than 3000 g / eq., more preferably 1000 g / eq. or less, further preferably 500 g / eq. or less, and particularly preferably 300 g / eq. or less. The phenolic hydroxyl equivalent of the phenolic resin (A) represents the mass of the phenolic resin (A) per 1 equivalent of phenolic hydroxyl groups.
[0248] Refractive index n of the cured product of the core resin composition core The refractive index n of the cured product of the core resin composition can be reduced by, for example, adjusting the composition of the (A) phenolic resin. core When a large amount of the phenolic resin (A) having a high refractive index is used, the refractive index n of the cured product of the core resin composition can be increased. core . The specific refractive index of (A) phenolic resin can be calculated using the Lorentz-Lorenz formula. Therefore, the type and amount of (A) phenolic resin can be selected based on the refractive index of (A) phenolic resin derived based on the Lorentz-Lorenz formula. Regarding the Lorentz-Lorenz formula, reference can be made to, for example, "Refractive Index Control of Optical Polymers: Theoretical Prediction and Molecular Design Methods" (Shinji Ando, "Optics", Vol. 44, No. 8, 2015, pp. 298-303), "Optical Properties and High Performance of Transparent Polymers" (Yoshihisa Tani, "Industrial Materials", March 2021, pp. 16-18). For example, depending on the phenolic resin containing fluorine atoms, there is a method that can reduce the refractive index n of the cured product. coreIn the following description, a phenolic resin containing fluorine atoms may be referred to as a "fluorine-based phenolic resin".
[0249] The (A) phenolic resin of the core resin composition preferably comprises one or more phenolic resins identical to the resin contained in the coating resin composition. That is, preferably one or more phenolic resins are contained in both the core resin composition and the coating resin composition. Like this, when the core resin composition and the coating resin composition comprise a common phenolic resin, the affinity of the core layer and the coating layer can be improved. Thus, the smoothness of the interface between the core layer and the coating layer can be improved, and therefore, the light attenuation caused by the scattering at the interface can be effectively suppressed, and therefore, the transmission loss can be effectively suppressed. In addition, the adhesion of the interface between the core layer and the coating layer can be improved, and therefore, the mechanical strength and heat resistance of the optical waveguide can be improved. And then, the thermal expansion coefficient of the core layer can usually be made close to the thermal expansion coefficient of the coating layer, and therefore, the deformation of the optical waveguide caused by thermal changes can be suppressed.
[0250] Sometimes the phenolic resin commonly contained in the core resin composition and the coating resin composition is referred to as "common phenolic resin". Relative to the overall 100% by mass of the (A) phenolic resin of the core resin composition, the range of the amount of the common phenolic resin contained in the (A) phenolic resin is preferably 40% by mass or more, more preferably 50% by mass or more, particularly preferably 60% by mass or more, usually 100% by mass or less, preferably 99% by mass or less, more preferably 97% by mass or less, particularly preferably 95% by mass or less. When the amount of the common phenolic resin is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the mechanical strength and heat resistance of the cured product of the core resin composition can usually be made particularly good.
[0251] The amount of the phenolic resin (A) is preferably 40% by mass or greater, more preferably 50% by mass or greater, and even more preferably 60% by mass or greater, relative to 100% by mass of the non-volatile components of the core resin composition, and is preferably 90% by mass or less, more preferably 80% by mass or less, and may be 70% by mass or less. When the amount of the phenolic resin (A) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition, as well as the mechanical strength and heat resistance of the cured product of the core resin composition, can generally be particularly improved.
[0252] [2.2.(B) Photoacid generator]
[0253] The core resin composition contains a (B) photoacid generator as component (B). The (B) photoacid generator generates an acid upon exposure to active light such as ultraviolet light, and the generated acid promotes the crosslinking reaction of the (C) crosslinker. Therefore, exposure to light effectively reduces the solubility of the core resin composition in a developer, enabling efficient formation of a negative pattern. The (B) photoacid generators may be used alone or in combination of two or more.
[0254] As the photoacid generator, a compound that generates an acid upon exposure to active light can be used. Examples of the photoacid generator include halogen-containing compounds, onium salt compounds, diazoketone compounds, sulfone compounds, sulfonic acid compounds, sulfonimide compounds, diazomethane compounds, and oxime ester compounds. Among them, oxime ester compounds are preferred.
[0255] Examples of halogen-containing compounds that can be suitably used as photoacid generators include hydrocarbon compounds containing alkyl halide and heterocyclic compounds containing alkyl halide. Specific examples of suitable halogen-containing compounds include 2-[2-(furan-2-yl)vinyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(5-methylfuran-2-yl)vinyl]-4,6-bis(trichloromethyl)-s-triazine, 2-(methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, and 2-[2-(4-methoxyphenyl)vinyl]-4,6-bis(trichloromethyl)-s-triazine. Halogen-containing compounds can be commercially available products. Examples of commercially available products include "TFE-triazine," "TME-triazine," "MP-triazine," "MOP-triazine," and "dimethoxytriazine" (a halogen-containing compound-based photoacid generator having a triazine skeleton) manufactured by Sanwa Chemical Co., Ltd.
[0256] Examples of onium salt compounds that can be suitably used as photoacid generators include iodonium salts, sulfonium salts, phosphonium salts, diazonium salts, and pyridinium salts. Specific examples of suitable onium salt compounds include tris(4-methylphenyl)sulfonium trifluoromethanesulfonate, tris(4-methylphenyl)sulfonium hexafluorophosphonate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium p-toluenesulfonate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluorophosphate, diphenyliodonium tetrafluoroborate, triphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium p-toluenesulfonate, triphenylsulfonium hexafluoroantimonate, 4-tert-butylphenyl-diphenylsulfonium trifluoromethanesulfonate, 4-tert-butylphenyl-diphenylsulfonium p-toluenesulfonate, and 4,7-di-n-butoxynaphthyltetrahydrothiophenium trifluoromethanesulfonate. As the onium salt compound, commercially available products can be used. Examples of commercially available products include "TS-01" and "TS-91" manufactured by Sanwa Chemical Co., Ltd.; "CPI-110A", "CPI-210S", "HS-1", "LW-S1", "IK-1", and "CPI-310B" manufactured by Sanapro; and "SI-110L", "SI-180L", and "SI-100L" manufactured by Sanshin Chemical Industry Co., Ltd.
[0257] Examples of diazoketone compounds that can be suitably used as photoacid generators include 1,3-diketo-2-diazonium compounds, diazobenzoquinone compounds, and diazonaphthoquinone compounds. Specific examples of suitable diazoketone compounds include phenolic 1,2-naphthoquinone didiazide-4-sulfonic acid ester compounds.
[0258] Examples of sulfone compounds that can be suitably used as photoacid generators include β-ketosulfone compounds, β-sulfonylsulfone compounds, and α-diazo compounds of these compounds. Specific examples of suitable sulfone compounds include 4-trisphenacylsulfone, tristolylphenacylsulfone, and bis(phenacylsulfonyl)methane.
[0259] Examples of sulfonic acid compounds that can be suitably used as photoacid generators include alkylsulfonates, halogenated alkylsulfonates, arylsulfonates, and iminosulfonates. Specific examples of suitable sulfonic acid compounds include benzoin tosylate, pyrogallol tris(trifluoromethanesulfonate), o-nitrobenzyl trifluoromethanesulfonate, and o-nitrobenzyl p-toluenesulfonate.
[0260] Specific examples of sulfonyl imide compounds that can be suitably used as photoacid generators include N-(trifluoromethylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(trifluoromethylsulfonyloxy)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, and N-(trifluoromethylsulfonyloxy)naphthyl imide.
[0261] Specific examples of diazomethane compounds that can be suitably used as the photoacid generator include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, etc. Commercially available diazomethane compounds can be used.
[0262] Specific examples of oxime ester compounds that can be suitably used as photoacid generators include 2-methyl-α-[2-[[(propylsulfonyl)oxy]imino]-3(2H)-thienylidene]-benzeneacetonitrile and 2-methyl-α-[2-[[[(4-methylphenyl)sulfonyl]oxy]imino]-3(2H)-thienylidene]-benzeneacetonitrile. Commercially available products include, for example, "PAG103," "PAG121," "PAG169," and "PAG203" manufactured by BASF.
[0263] From the viewpoint of improving the affinity between the core layer and the coating layer, the (B) photoacid generator of the core resin composition preferably contains one or more photoacid generators that are the same as the photoacid generator contained in the coating resin composition. That is, it is preferred that one or more photoacid generators are contained in both the core resin composition and the coating resin composition. Sometimes the photoacid generator commonly contained in both the core resin composition and the coating resin composition is referred to as a "common photoacid generator". The amount of the common photoacid generator contained in the (B) photoacid generator relative to the total 100% by mass of the core resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.
[0264] The amount of the photoacid generator (B) is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, relative to 100% by mass of the non-volatile component in the core resin composition as the photosensitive resin composition, and is preferably 3% by mass or less, more preferably 2% by mass or less, and particularly preferably 1.5% by mass or less.
[0265] [2.3.(C) Cross-linking agent]
[0266] The core resin composition includes a crosslinking agent (C) as component (C). The crosslinking agent (C) is capable of undergoing a crosslinking reaction. Through the crosslinking reaction of the crosslinking agent (C), the core resin composition can be insolubilized or cured in a developer to form a core layer. The crosslinking agent (C) does not include a substance that is a phenolic resin (A).
[0267] The crosslinking agent (C) is preferably an amino resin. When the amino resin is combined with the phenolic resin (A), a photosensitive resin composition having excellent photosensitivity can be obtained. Therefore, the photosensitivity of the core resin composition can be improved.
[0268] Furthermore, the crosslinking agent (C) is preferably one capable of undergoing a crosslinking reaction with the phenolic resin (A). Examples of crosslinking agents (C) capable of undergoing a crosslinking reaction with the phenolic resin (A) include compounds containing an alkoxymethyl group in the molecule. The alkoxymethyl group represents a group represented by the following formula (C-1). In formula (C-1), "*" represents a linking bond.
[0269] [Chemistry 28]
[0270] R 21 -O-CH2-* (C-1)
[0271] In formula (C-1), R 21 Represents an alkyl group optionally having a substituent. The alkyl group may be a linear, branched or cyclic alkyl group. In addition, the cyclic alkyl group may be either a monocyclic or polycyclic group. As the alkyl group, an alkyl group having 1 to 10 carbon atoms is preferred, an alkyl group having 1 to 6 carbon atoms is more preferred, and an alkyl group having 1 to 4 carbon atoms is further preferred. Examples of the alkyl group include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, isopropyl, sec-butyl, and tert-butyl. Among them, methyl and butyl are preferred, and methyl is more preferred. R 21 The represented alkyl group may have a substituent.
[0272] The alkoxymethyl group is preferably contained in an alkoxymethylamino group represented by the following formula (C-1'). Therefore, the crosslinking agent (C) preferably contains an alkoxymethylamino group represented by formula (C-1'), and more preferably contains two or more alkoxymethylamino groups represented by formula (C-1') in the molecule. In the formula, "*" represents a connecting bond.
[0273] [Chemistry 29]
[0274]
[0275] In formula (C-1'), R 22 and R in formula (C-1) 21 R represents a hydrogen atom or an alkoxymethyl group.
[0276] The crosslinking agent (C) is particularly preferably an amino resin containing two or more alkoxymethyl groups in the molecule. Examples of the amino resin containing two or more alkoxymethyl groups in the molecule include melamine resins and urea resins, with melamine resins being preferred.
[0277] As the melamine resin, for example, a melamine resin having a structure represented by the following formula (C-2) is preferable.
[0278] [Chemistry 30]
[0279]
[0280] In formula (C-2), X 21 、X 22 、X 23 and X 24 Each independently represents a hydrogen atom or an alkoxymethyl group. 50 represents a hydrogen atom, an amino group, an alkyl group optionally having a substituent, an aryl group optionally having a substituent, or an alkoxymethylamino group represented by formula (C-1'). 50 When X represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent, 21 、X 22 、X 23 and X 24 At least two of them are alkoxymethyl groups.
[0281] X 21 ~X 24 The alkoxymethyl group represented by R may be the same as the group represented by formula (C-1). 50 When X represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent, 21 ~X 24 At least two of them are alkoxymethyl. 50 When X represents a hydrogen atom, an amino group, an alkyl group which may have a substituent, or an aryl group which may have a substituent, 21 ~X 24 Two or more of them are alkoxymethyl groups. 21 ~X 24 At least three of them are alkoxymethyl, more preferably X 21 ~X 24 At least four of them are alkoxymethyl groups.
[0282] R 50 R represents a hydrogen atom, an amino group, an alkyl group which may have a substituent, an aryl group which may have a substituent, or an alkoxymethylamino group represented by formula (C-1'). 50 It is preferably an aryl group which may have a substituent or an alkoxymethylamino group represented by formula (C-1'), and more preferably an alkoxymethylamino group represented by formula (C-1'). 50 The alkyl group optionally having a substituent represented by 1 The alkyl group optionally having a substituent represented by 50 The aryl group optionally having a substituent represented by 1 The aryl groups optionally having substituents represented are the same.
[0283] The melamine resin having a structure represented by formula (C-2) is preferably a melamine resin having a structure represented by formula (C-2′).
[0284] [Chemistry 31]
[0285]
[0286] In formula (C-2'), X 25 、X 26 、X 27 、X 28 、X 29 and X 30 Each independently represents a hydrogen atom or an alkoxymethyl group. 25 、X 26 、X 27 、X 28 、X 29 and X 30 At least two of them are alkoxymethyl groups.
[0287] X 25 ~X 30 The alkoxymethyl group represented by X may be the same as the group represented by formula (C-1). 25 ~X 30 At least two of them are alkoxymethyl, preferably X 25 ~X 30 At least three of them are alkoxymethyl, more preferably X 25 ~X 30 At least four of them are alkoxymethyl groups, and more preferably X 25 ~X 30 All are alkoxymethyl groups.
[0288] Specific examples of the melamine resin include the following melamine resins.
[0289] [Chemistry 32]
[0290]
[0291] The melamine resin may be a commercially available product, such as "MW-390," "MW-100LM," and "MX-750LM" manufactured by Sanwa Chemical Co., Ltd., and the Cymel series manufactured by Ornex Japan Co., Ltd.
[0292] As the urea resin, for example, a urea resin having any one of the structures represented by the following formula (C-3) and the structure represented by the following formula (C-4) is preferred.
[0293] [Chemistry 33]
[0294]
[0295] In formula (C-3), X 31 、X 32 、X 33 and X 34 Each independently represents a hydrogen atom or an alkoxymethyl group. 31 、X 32 、X 33 and X 34 At least two of them are alkoxymethyl. 31 ~X 34 At least three of them are alkoxymethyl, more preferably X 31 ~X 34 At least four of them are alkoxymethyl groups.
[0296] In formula (C-4), X 35 and X 36 represents an alkoxymethyl group.
[0297] X 31 ~X 36 The alkoxymethyl group represented may be the same as the group represented by formula (C-1).
[0298] Commercially available urea resins may be used, and examples thereof include "MX-270," "MX-279," and "MX-280" manufactured by Sanwa Chemical Co., Ltd. and the Cymel series manufactured by Ornex Japan Co., Ltd.
[0299] (C) The cross-linking agent may be used alone or in combination of two or more.
[0300] The weight average molecular weight of the cross-linking agent (C) is not particularly limited. Preferred ranges are as follows: the weight average molecular weight of the cross-linking agent (C) is preferably 150 or greater, more preferably 160 or greater, and particularly preferably 170 or greater, and is preferably less than 15,000, more preferably 14,000 or less, and particularly preferably 13,000 or less, and may be less than 2,500.
[0301] The crosslinking agent (C) may contain a crosslinking group such as an alkoxymethyl group as a group capable of undergoing a crosslinking reaction. The crosslinking group equivalent weight of the crosslinking agent (C) is preferably 50 g / eq. or greater, more preferably 100 g / eq. or greater, and preferably less than 3000 g / eq., more preferably 1000 g / eq. or less, further preferably 500 g / eq. or less, and particularly preferably 300 g / eq. or less. The crosslinking group equivalent weight of the crosslinking agent (C) represents the mass of the crosslinking agent (C) per 1 equivalent of the crosslinking group.
[0302] From the viewpoint of improving the affinity of the core layer and the coating layer, the cross-linking agent (C) of the core resin composition preferably includes one or more cross-linking agents that are the same as the cross-linking agent included in the coating resin composition. That is, one or more cross-linking agents are preferably included in both the core resin composition and the coating resin composition. Sometimes the cross-linking agent commonly included in both the core resin composition and the coating resin composition is referred to as a "common cross-linking agent". Relative to the overall 100% by mass of the cross-linking agent (C) of the core resin composition, the amount of the common cross-linking agent included in the (C) cross-linking agent is preferably in the range of 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.
[0303] The amount of the crosslinking agent (C) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, relative to 100% by mass of the non-volatile components of the core resin composition, and is preferably 40% by mass or less, more preferably 35% by mass or less, and particularly preferably 30% by mass or less. When the amount of the crosslinking agent (C) is within the aforementioned range, the transmission loss of the optical waveguide can be effectively suppressed, and further, the resolution of the core resin composition and the mechanical strength and heat resistance of the cured product of the core resin composition can generally be particularly improved.
[0304] [2.4.(D) Polymer]
[0305] The core resin composition may be combined with the above-mentioned (A) to (C) components and may further include a (D) polymer as an optional component. The (D) polymer as the (D) component generally has a weight average molecular weight of 2,500 or more. Specifically, the weight average molecular weight of the (D) polymer is generally in the range of 2,500 or more, more preferably 5,000 or more, particularly preferably 10,000 or more, and preferably 100,000 or less, more preferably 80,000 or less, and further preferably 60,000 or less. When the core resin composition includes the (D) polymer, it is possible to improve the surface smoothness of the core layer or improve the interface smoothness between the core layer and the cladding layer, thereby effectively reducing the transmission loss of the optical waveguide. Furthermore, it is generally possible to easily form a coating film of the core resin composition or to improve the toughness of the core layer. In addition, according to the (D) polymer, it is generally possible to effectively improve the heat resistance and flexibility of the core layer or improve the transparency of the core layer, thereby effectively suppressing the transmission loss. However, the (D) polymer does not include substances belonging to the above-mentioned (A) to (C) components.
[0306] The polymer (D) may be a homopolymer or a copolymer. Examples of the polymer (D) include acrylic resins, phenoxy resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polyimide resins, polyamide-imide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyetheretherketone resins, and polyester resins. Among these, acrylic resins are preferred.
[0307] The acrylic resin may be a polymer comprising repeating units having a structure formed by polymerizing acrylic monomers such as acrylic acid, acrylic ester, methacrylic acid, and methacrylic ester, and may be produced, for example, by polymerizing acrylic monomers. The acrylic resin may be a homopolymer of an acrylic monomer, a copolymer of two or more acrylic monomers, or a copolymer of an acrylic monomer and any monomer other than an acrylic monomer. When an acrylic resin is used as the (D) polymer, it is possible to effectively improve the heat resistance and flexibility of the core layer, or to improve the transparency of the core layer and effectively suppress the transmission loss of the optical waveguide. Specific examples of acrylic resins include "Alphonse" (registered trademark) manufactured by Toagosei Co., Ltd.; "ART CURE" manufactured by Negami Industries; and "Actoflow" manufactured by Soken Chemical Co., Ltd.
[0308] Examples of phenoxy resins include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeletons, bisphenol F skeletons, bisphenol S skeletons, bisphenol acetophenone skeletons, novolac skeletons, biphenyl skeletons, fluorene skeletons, dicyclopentadiene skeletons, norbornene skeletons, naphthalene skeletons, anthracene skeletons, adamantane skeletons, terpene skeletons, and trimethylcyclohexane skeletons. The termini of the phenoxy resins may be any functional group such as a phenolic hydroxyl group or an epoxy group. Specific examples of phenoxy resins include "1256" and "4250" (both phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton), "YX7553", "YL6794", "YL7213", "YL7290" and "YL7482" manufactured by Mitsubishi Chemical Corporation; and "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Corporation.
[0309] Examples of the polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, with polyvinyl butyral resin being preferred. Specific examples of the polyvinyl acetal resin include Denka Buchlar 4000-2, Denka Buchlar 5000-A, Denka Buchlar 6000-C, and Denka Buchlar 6000-EP manufactured by Denka Corporation; and Eslake BH series, BX series, KS series, BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0310] Specific examples of polyimide resins include "RIKACOTE SN20" and "RIKACOTE PN20" manufactured by Shin Nippon Chemical Co., Ltd. Specific examples of polyimide resins include modified polyimides such as linear polyimides obtained by reacting difunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (described in JP-A-2006-37083), and polyimides containing a polysiloxane skeleton (described in JP-A-2002-12667 and JP-A-2000-319386).
[0311] Specific examples of polyamide-imide resins include "Biromax HR11NN" and "Biromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins include modified polyamide-imides such as "KS9100" and "KS9300," polyamide-imides containing a polysiloxane skeleton, manufactured by Hitachi Chemical Co., Ltd.
[0312] Specific examples of the polyethersulfone resin include "PES5003P" manufactured by Sumitomo Chemical Co., Ltd. and the like.
[0313] Specific examples of the polysulfone resin include polysulfones "P1700" and "P3500" manufactured by Solvay Band Polymers.
[0314] (D) The polymer may be used alone or in combination of two or more.
[0315] The (D) polymer preferably does not contain a functional group that can react with a phenolic hydroxyl group or a crosslinking group to form a bond. Even if the (D) polymer contains a functional group, it is preferred that the functional group is small. Therefore, the functional group equivalent of the (D) polymer is preferably large. The functional group equivalent of the (D) polymer represents the mass of the (D) polymer per 1 equivalent of the functional group. Specifically, the functional group equivalent of the (D) polymer is preferably 3000 g / eq. or more, more preferably 4000 g / eq. or more, and particularly preferably 5000 g / eq. or more. In addition, the range of the phenolic hydroxyl equivalent of the (D) polymer can be the same as the range of the functional group equivalent of the (D) polymer. The phenolic hydroxyl equivalent of the (D) polymer represents the mass of the (D) polymer per 1 equivalent of the phenolic hydroxyl group. Furthermore, the range of the crosslinking group equivalent of the (D) polymer can be the same as the range of the functional group equivalent of the (D) polymer. The crosslinking group equivalent of the (D) polymer represents the mass of the (D) polymer per 1 equivalent of the crosslinking group. Among them, the (D) polymer preferably has no functional group, and therefore preferably has no phenolic hydroxyl group, and further preferably has no crosslinking group.
[0316] From the viewpoint of improving the affinity of the core layer and the coating layer, the (D) polymer of the core resin composition preferably includes one or more polymers identical to the polymer included in the coating resin composition. That is, preferably one or more polymers are included in both the core resin composition and the coating resin composition. Sometimes the polymer commonly included in both the core resin composition and the coating resin composition is referred to as a "common polymer". Relative to the overall 100% by mass of the (D) polymer of the core resin composition, the amount of the common polymer included in the (D) polymer is preferably in the range of 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.
[0317] Regarding the range of the amount of the (D) polymer, it can be 0 mass% or greater than 0 mass% relative to 100 mass% of the non-volatile component of the core resin composition, and is preferably 1 mass% or greater, more preferably 2 mass% or greater, and particularly preferably 5 mass% or greater, and is preferably 30 mass% or less, more preferably 20 mass% or less, and particularly preferably 10 mass% or less.
[0318] [2.5.(E) Amine compounds]
[0319] The core resin composition may be combined with the above-mentioned (A) to (D) components and may further include (E) a compound represented by the following formula (E-1) as an optional component. Hereinafter, the compound represented by the (E) formula (E-1) as the (E) component may be referred to as the "(E) amine compound". The (E) amine compound functions as a quencher in the core resin composition and can suppress the diffusion rate of the acid generated by the (B) photoacid generator in the resin composition. Therefore, the resolution of the core resin composition can be improved by the (E) amine compound. However, the (E) amine compound does not include substances belonging to the above-mentioned (A) to (D) components.
[0320] [Chemistry 34]
[0321]
[0322] In formula (E-1), R e1 、R e2 and R e3 Each independently represents a hydrogen atom or a hydrocarbon group. As a hydrocarbon group, it may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. In addition, the aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group or an unsaturated aliphatic hydrocarbon group. In addition, the hydrocarbon group may contain a ring. Therefore, the aliphatic hydrocarbon group may be an alicyclic hydrocarbon group. The number of carbon atoms of the hydrocarbon group is usually 1 or more, preferably 2 or more, particularly preferably 5 or more, and preferably 20 or less, more preferably 18 or less, particularly preferably 12 or less. Examples of the hydrocarbon group include alkyl groups such as methyl, ethyl, hexyl, octyl, and decyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl and naphthyl; and groups obtained by combining them. In addition, R e1 With R e2 They are optionally bonded to form a ring.
[0323] Examples of the (E) amine compound include ammonia, aliphatic primary amine compounds, aliphatic secondary amine compounds, aliphatic tertiary amine compounds, and aromatic amine compounds.
[0324] Examples of the aliphatic primary amine compound include methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, sec-butylamine, tert-butylamine, pentylamine, tert-pentylamine, cyclopentylamine, hexylamine, cyclohexylamine, heptylamine, octylamine, nonylamine, decylamine, dodecylamine, and cetylamine.
[0325] Examples of the aliphatic secondary amine compound include dimethylamine, diethylamine, di-n-propylamine, diisopropylamine, di-n-butylamine, diisobutylamine, di-sec-butylamine, dipentylamine, dicyclopentylamine, dihexylamine, dicyclohexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, didodecylamine, dicetylamine, and pyrrolidine.
[0326] Examples of the aliphatic tertiary amine compound include trimethylamine, triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, triisobutylamine, tri-sec-butylamine, tripentylamine, tricyclopentylamine, trihexylamine, tricyclohexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, tridodecylamine, tricetylamine, dimethylethylamine, and methylethylpropylamine.
[0327] Examples of the aromatic amine compound include benzylamine, phenethylamine, benzyldimethylamine, diphenyl(p-tolyl)amine, methyldiphenylamine, triphenylamine, and naphthylamine; aniline; aniline derivatives such as N-methylaniline, N-ethylaniline, N-propylaniline, N,N-dimethylaniline, 2-methylaniline, 3-methylaniline, 4-methylaniline, ethylaniline, propylaniline, trimethylaniline, and N,N-dimethyltoluidine; pyrrole; pyrrole derivatives such as 2H-pyrrole, 1-methylpyrrole, 2,4-dimethylpyrrole, 2,5-dimethylpyrrole, and N-methylpyrrole; and the like.
[0328] From the viewpoint of improving the affinity of the core layer and the coating layer, the (E) amine compound of the core resin composition preferably includes one or more amine compounds that are the same as the amine compound included in the coating resin composition. That is, preferably one or more amine compounds are included in both the core resin composition and the coating resin composition. Sometimes the amine compound commonly included in the core resin composition and the coating resin composition is referred to as a "common amine compound". Relative to the overall 100% by mass of the (E) amine compound of the core resin composition, the range of the amount of the common amine compound included in the (E) amine compound is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.
[0329] Regarding the range of the amount of the (E) amine compound, relative to 100% by mass of the non-volatile component of the core resin composition, it can be 0% by mass or greater than 0% by mass, preferably 0.01% by mass or greater, more preferably 0.05% by mass or greater, particularly preferably 0.1% by mass or greater, and preferably 5% by mass or less, more preferably 2% by mass or less, particularly preferably 1% by mass or less.
[0330] [2.6.(F) Optional Additives]
[0331] The core resin composition may further contain (F) optional additives as optional components in combination with the above-mentioned components (A) to (E), within a range that does not significantly impair the effects of the present invention. The optional additives (F) do not include substances included in the above-mentioned components (A) to (E). The optional additives (F) may be used alone or in combination of two or more.
[0332] Examples of the optional additives (F) include ultraviolet absorbers, silane coupling agents, plasticizers, flame retardants, antistatic agents, antioxidants, antibacterial agents, defoaming agents, leveling agents, thickeners, adhesion-imparting agents, thixotropy-imparting agents, release agents, surface treatment agents, dispersants, surface modifiers, stabilizers, and the like.
[0333] (F) optional additives may include inorganic particles. For example, when nanoparticles of metal oxide are included, the refractive index of the cured product of the core resin composition can be increased. Wherein, from the viewpoint of effectively suppressing the transmission loss of the optical waveguide, the amount of inorganic particles included in the core resin composition is preferably small. Specifically, relative to 100% by mass of the non-volatile component of the core resin composition, the range of the amount of inorganic particles is preferably 10% by mass or less, more preferably 5% by mass or less, further preferably 1% by mass or less, and ideally 0% by mass. Thus, the core resin composition preferably does not contain inorganic particles.
[0334] [2.7.(G) Solvent]
[0335] The core resin composition may contain a (G) solvent as a volatile component in combination with the non-volatile components (A) to (F) above. The viscosity of the core resin composition can be adjusted by the (G) solvent as the (G) component. Examples of the (G) solvent include organic solvents.
[0336] Examples of the (G) solvent include ketone solvents such as ethyl methyl ketone and cyclohexanone; aromatic hydrocarbon solvents such as toluene, xylene, and tetramethylbenzene; glycol ether solvents such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ester solvents such as ethyl acetate, butyl acetate, butyl cellosolve acetate, carbitol acetate, and ethyl diglycol acetate; ether ester solvents such as propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate; aliphatic hydrocarbon solvents such as octane and decane; and petroleum solvents such as petroleum ether, naphtha, hydrogenated naphtha, and solvent naphtha. The (G) solvent may be used alone or in combination of two or more.
[0337] From the viewpoint of the coating properties of the core resin composition, the amount of the solvent is preferably appropriately adjusted.
[0338] [2.8. Method for producing core resin composition]
[0339] The core resin composition can be manufactured by mixing the various components that should be included in the core resin composition. Therefore, the core resin composition can be manufactured by mixing components (A) to (C) and components (D) to (G) as needed. During mixing, mixing can be performed using a mixing device such as a three-roll mill, a ball mill, a bead mill, or a sand mill, or stirring can be performed using a stirring device such as a super mixer or a planetary mixer. The order in which the components are mixed is not limited. In addition, cooling or heating can be performed during the mixing of the components.
[0340] [2.9. Characteristics of the core resin composition]
[0341] The core resin composition preferably has excellent resolution. For example, by the method described in [Evaluation of the resolution of the resin composition] of the embodiment described later, the core resin composition is used to form a line layer with L / S (line / space) of 10μm / 10μm, 5μm / 50μm and 3μm / 3μm. In this case, for any line layer, the aspect ratio of the line layer can be preferably greater than 0.6, more preferably greater than 1. Here, in L / S, L (line) represents the width of the line layer, and S (space) represents the space between the line layers. In addition, the aspect ratio of the line layer represents the ratio expressed by "layer thickness / line width" of the line layer. According to the core resin composition having such excellent resolution, a core layer with small width and space can be formed, and the miniaturization of the optical waveguide can be achieved.
[0342] The core resin composition can be cured by exposure and then heating as needed. Thus, a cured product can be obtained from the core resin composition. Generally, among the components contained in the core resin composition, volatile components such as (G) solvent can be volatilized by heat during drying or curing, but non-volatile components such as (A) to (F) components will not volatilize. Therefore, the cured product of the core resin composition can contain the non-volatile components of the core resin composition or their reaction products.
[0343] The core resin composition can provide a cured product having a refractive index suitable for forming an optical waveguide. core There is no limitation as long as the desired aperture NA can be obtained. For example, the refractive index n of the cured product of the core resin composition at a wavelength of 1310 nm is measured. core The refractive index of the core resin composition can be measured by the method described in [Measurement of the Refractive Index of a Cured Material of the Resin Composition] in the Examples described below.
[0344] The core resin composition can produce a cured product with excellent mechanical strength. For example, when the elongation at break of the cured product is measured by the method described in [Measurement of Elongation at Break of a Cured Product of a Resin Composition] in the Examples described below, the cured product preferably has an elongation at break of 1% or greater.
[0345] The core resin composition can provide a cured product with excellent heat resistance. For example, when a cured product obtained under the conditions described in the Examples below is heated under the conditions described in "(Appearance Observation after Reflow)", the generation of voids can be suppressed.
[0346] According to the cured product of the core resin composition, the surface of the cured product can be made highly smooth. Thus, according to the core resin composition, a core layer with a smooth surface can be formed, effectively suppressing transmission loss. For example, when the core layer is formed from the cured product of the core resin composition under the conditions described in the embodiments described later, the arithmetic mean roughness of the core layer can be reduced. Specifically, the arithmetic surface roughness of the core layer is preferably less than 200nm, more preferably less than 180nm, and particularly preferably less than 150nm. The lower limit is not particularly limited, for example, it can be more than 10nm. The surface roughness of the core layer can be measured by the method described in [Determination of surface roughness of core layer] in the embodiments described later.
[0347] The core resin composition can be used as a photosensitive resin composition for forming the core layer of an optical waveguide. For example, the core resin composition can be used to form an optical waveguide capable of transmitting light with a wavelength of 1300 nm to 1320 nm. In particular, the core resin composition is preferably used to form a single-mode optical waveguide, for example, a single-mode optical waveguide for light with a wavelength of 1310 nm.
[0348] From the viewpoint of forming an optical waveguide for light having a wavelength of 1300 nm to 1320 nm, the solution of the core resin composition preferably has a small absorbance at a wavelength of 1310 nm. Generally, when the absorbance of the solution of the resin composition is small, the absorbance of the cured product of the resin composition becomes smaller. Therefore, it is preferred that the absorbance of the solution of the resin composition at a wavelength of 1310 nm is small. For example, it is preferred that the absorbance of a 20% by mass solution of the core resin composition obtained under the conditions described in the embodiments described later is small. If specific examples are given, the absorbance of the solution of the core resin composition measured by the method described in the [Determination of the absorbance of the solution of the resin composition] of the embodiment is preferably 0.020 or less, more preferably 0.018 or less, and particularly preferably 0.015 or less when the optical path length is 1 cm.
[0349] [3. Coating resin composition]
[0350] The coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent. The coating resin composition may be a photosensitive resin composition, and therefore, a coating layer can be formed by a method comprising exposure. In addition, the coating resin composition can be formed into a coating layer having a desired pattern by a method comprising exposure and development, similarly to the core resin composition. The "pattern" of the coating layer, unless otherwise specified, represents the shape of the coating layer observed in the thickness direction.
[0351] The cladding layer can be combined with a core layer formed from a cured product of a core resin composition to produce an optical waveguide capable of transmitting light through the core layer. Furthermore, as described above, the optical waveguide comprising the core layer and the cladding layer can suppress light transmission loss.
[0352] Furthermore, the coating resin composition generally has excellent resolution. Furthermore, the cured product of the coating resin composition generally has excellent mechanical strength such as elongation at break, and also has excellent heat resistance such as reflow resistance.
[0353] [3.1.(a) Phenolic resin]
[0354] The coating resin composition includes (a) phenolic resin as (a) component. As the (a) phenolic resin of the coating resin composition, a resin in the same range as the (A) phenolic resin of the core resin composition can be used. In addition, the range of the amount of the (a) phenolic resin contained in the coating resin composition can be the same as the range of the amount of the (A) phenolic resin contained in the core resin composition. Thus, the range of the amount of the (a) phenolic resin relative to 100% by mass of the non-volatile component of the coating resin composition can be the same as the range of the amount of the (A) phenolic resin relative to 100% by mass of the non-volatile component of the core resin composition. In addition, the range of the amount of the (A-1) component, the (A-2) component and the (A-3) component relative to 100% by mass of the non-volatile component of the coating resin composition can be the same as the range of the amount of the (A-1) component, the (A-2) component and the (A-3) component relative to 100% by mass of the non-volatile component of the core resin composition. Furthermore, the amounts of components (A-1), (A-2), and (A-3) relative to 100% by mass of the total (a) phenolic resin can be in the same ranges as the amounts of components (A-1), (A-2), and (A-3) relative to 100% by mass of the total (A) phenolic resin. Furthermore, the mass ratio Wa2 / Wa1 of components (A-1) to (A-2) in the (a) phenolic resin can be in the same range as the mass ratio Wa2 / Wa1 of the (A) phenolic resin. Using the (a) phenolic resin allows the coating resin composition to achieve the same advantages as those achieved by using the (A) phenolic resin in the core resin composition.
[0355] The (a) phenolic resin contained in the coating resin composition and the (A) phenolic resin contained in the core resin composition may be the same as or different from each other.
[0356] The refractive index n of the cured product of the coating resin composition is similar to that of the cured product of the core resin composition. clad The specific type and amount of the phenolic resin (a) can be adjusted according to the composition of the phenolic resin (a). clad Therefore, from the viewpoint of obtaining an optical waveguide having a desired aperture NA by adjusting the composition of the (a) phenolic resin, it is preferred that at least a portion of the (a) phenolic resin of the cladding resin composition is different from the (A) phenolic resin of the core resin composition.
[0357] On the other hand, from the perspective of increasing the affinity between the core layer and the cladding layer and effectively improving the transmission loss, mechanical strength, and heat resistance of the optical waveguide, it is preferred that at least a portion of the phenolic resin (a) in the cladding resin composition is the same as the phenolic resin (A) in the core resin composition. In other words, one or more common phenolic resins are preferably contained in both the core resin composition and the cladding resin composition.
[0358] Therefore, the amount of the common phenolic resin contained in the (a) phenolic resin (i.e., the phenolic resin contained in both the core resin composition and the coating resin composition) relative to 100% by mass of the total amount of the (a) phenolic resin in the coating resin composition may be 100% by mass or less, and preferably within a specific range of less than 100% by mass. Specifically, the amount of the common phenolic resin contained in the (a) phenolic resin is preferably 40% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more, and is preferably 99.0% by mass or less, more preferably 98.5% by mass or less, and particularly preferably 98.0% by mass or less.
[0359] As a preferred combination of the (A) phenolic resin of the core resin composition and the (a) phenolic resin of the coating resin composition, for example, a combination of the (A) phenolic resin containing a phenolic resin having a structure having the effect of increasing the refractive index and the (a) phenolic resin not containing the aforementioned phenolic resin having a structure having the effect of increasing the refractive index can be listed. In addition, as another example, a combination of the (a) phenolic resin containing a phenolic resin having a structure having the effect of reducing the refractive index (such as a fluorine-based phenolic resin) and the (A) phenolic resin not containing the phenolic resin having a structure having the effect of reducing the refractive index can be listed. In any combination, the (A) phenolic resin and the (a) phenolic resin preferably include one or more common phenolic resins.
[0360] When the (a) phenolic resin of the coating resin composition contains a fluorinated phenolic resin, the amount of the fluorinated phenolic resin relative to 100% by mass of the total amount of the (a) phenolic resin is preferably in the range of 0.1% by mass or more, more preferably 0.2% by mass or more, particularly preferably 0.5% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, particularly preferably 20% by mass or less.
[0361] In addition, the mass range of fluorine atoms contained in the coating resin composition relative to 100 mass% of the non-volatile component of the coating resin composition is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, particularly preferably 0.03 mass% or more, and is preferably 10 mass% or less, more preferably 7 mass% or less, further preferably 5 mass% or less, and can be 1.0 mass% or less, 0.9 mass% or less, 0.8 mass% or less, etc.
[0362] [3.2.(b) Photoacid generator]
[0363] The coating resin composition contains a (b) photoacid generator as the (b) component. As the (b) photoacid generator of the coating resin composition, a substance in the same range as the (B) photoacid generator of the core resin composition can be used. In addition, the range of the amount of the (b) photoacid generator contained in the coating resin composition can be the same as the range of the amount of the (B) photoacid generator contained in the core resin composition. Therefore, the range of the amount of the (b) photoacid generator relative to 100% by mass of the non-volatile components of the coating resin composition can be the same as the range of the amount of the (B) photoacid generator relative to 100% by mass of the non-volatile components of the core resin composition. If the (b) photoacid generator is used, the coating resin composition can obtain the same advantages as the advantages of the core resin composition obtained by using the (B) photoacid generator.
[0364] The (b) photoacid generator contained in the coating resin composition may be the same as or different from the (B) photoacid generator contained in the core resin composition. From the perspective of improving the affinity between the core layer and the coating layer, the (b) photoacid generator in the coating resin composition preferably contains one or more common photoacid generators that are the same as the photoacid generator contained in the core resin composition. The amount of the common photoacid generator contained in the (b) photoacid generator relative to the total mass of 100% by mass of the (b) photoacid generator in the coating resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.
[0365] [3.3.(c) Cross-linking agent]
[0366] The coating resin composition contains a (c) cross-linking agent as the (c) component. As the (c) cross-linking agent of the coating resin composition, a cross-linking agent in the same range as the (C) cross-linking agent of the core resin composition can be used. In addition, the range of the amount of the (c) cross-linking agent contained in the coating resin composition can be the same as the range of the amount of the (C) cross-linking agent contained in the core resin composition. Therefore, the range of the amount of the (c) cross-linking agent relative to 100% by mass of the non-volatile components of the coating resin composition can be the same as the range of the amount of the (C) cross-linking agent relative to 100% by mass of the non-volatile components of the core resin composition. If the (c) cross-linking agent is used, the coating resin composition can obtain the same advantages as the advantages of the core resin composition obtained by using the (C) cross-linking agent.
[0367] The (c) cross-linking agent included in the coating resin composition may be the same as or different from the (c) cross-linking agent included in the core resin composition. From the viewpoint of improving the affinity of the core layer and the coating layer, the (c) cross-linking agent of the coating resin composition preferably includes one or more common cross-linking agents that are the same as the cross-linking agent included in the core resin composition. Relative to the overall 100% by mass of the (c) cross-linking agent of the coating resin composition, the amount of the common cross-linking agent included in the (c) cross-linking agent is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass.
[0368] [3.4.(d) Polymers]
[0369] The coating resin composition may be combined with the above-mentioned components (a) to (c) and may further include a (d) polymer as an optional component. As the (d) polymer as the (d) component of the coating resin composition, a polymer in the same range as the (D) polymer of the core resin composition may be used. In addition, the range of the amount of the (d) polymer contained in the coating resin composition may be the same as the range of the amount of the (D) polymer contained in the core resin composition. Therefore, the range of the amount of the (d) polymer relative to 100% by mass of the non-volatile component of the coating resin composition may be the same as the range of the amount of the (D) polymer relative to 100% by mass of the non-volatile component of the core resin composition. If the (d) polymer is used, the coating resin composition can obtain the same advantages as the advantages of the core resin composition obtained by using the (D) polymer.
[0370] (d) polymer included in the coating resin composition and (D) polymer included in the core resin composition may be the same or different. From the viewpoint of improving the affinity of the core layer and the coating layer, the (d) polymer of the coating resin composition preferably includes one or more common polymers identical to the polymer included in the core resin composition. Relative to the overall 100% by mass of the (d) polymer of the coating resin composition, the amount of the common polymer included in the (d) polymer is preferably more than 80% by mass, more preferably more than 90% by mass, particularly preferably 100% by mass.
[0371] [3.5.(e) Amine compounds]
[0372] In the coating resin composition, in combination with the above-mentioned (a) to (d) components, an (e) amine compound (i.e., a compound represented by formula (E-1)) may be further included as an optional component. For the (e) amine compound as the (e) component of the coating resin composition, substances in the same range as the (E) amine compound of the core resin composition can be used. In addition, the range of the amount of the (e) amine compound contained in the coating resin composition may be the same as the range of the amount of the (E) amine compound contained in the core resin composition. Therefore, the range of the amount of the (e) amine compound relative to 100% by mass of the non-volatile component of the coating resin composition may be the same as the range of the amount of the (E) amine compound relative to 100% by mass of the non-volatile component of the core resin composition. If the (e) amine compound is used, the coating resin composition can obtain the same advantages as the advantages of the core resin composition obtained by using the (E) amine compound.
[0373] The (e) amine compound included in the coating resin composition may be the same as or different from the (E) amine compound included in the core resin composition. From the viewpoint of improving the affinity of the core layer and the coating layer, the (e) amine compound of the coating resin composition preferably includes one or more common amine compounds identical to the amine compound included in the core resin composition. Relative to the overall 100% by mass of the (e) amine compound of the coating resin composition, the amount of the common amine compound included in the (e) amine compound is preferably 80% by mass or more, more preferably 90% by mass or more, particularly preferably 100% by mass.
[0374] [3.6.(f) Optional additives]
[0375] The coating resin composition may further include (f) an optional additive as an optional component in combination with the above-mentioned components (a) to (e). The optional additive (f) as the component (f) of the coating resin composition may be in the same range as the optional additive (F) of the core resin composition. Furthermore, the amount of the optional additive (f) contained in the coating resin composition may be in the same range as the amount of the optional additive (F) contained in the core resin composition.
[0376] [3.7.(g) Solvent]
[0377] The coating resin composition may contain a (g) solvent as a volatile component in combination with the non-volatile components such as the above-mentioned (a) to (f) components. As for the (g) solvent as the (g) component of the coating resin composition, the same range as the (G) solvent of the core resin composition can be used. In addition, the range of the amount of the (g) solvent contained in the coating resin composition may be the same as the range of the (G) solvent contained in the core resin composition. If the (g) solvent is used, the coating resin composition can obtain the same advantages as the advantages of the core resin composition obtained by using the (G) solvent.
[0378] [3.8. Method for producing coating resin composition]
[0379] The coating resin composition can be produced by mixing the components required for the coating resin composition. Thus, the coating resin composition can be produced by mixing components (a) to (c) and, if necessary, components (d) to (g). The mixing method can be the same as that used to produce the core resin composition.
[0380] [3.9. Characteristics of the coating resin composition]
[0381] The coating resin composition preferably has excellent resolution. For example, using the coating resin composition, wire layers with L / S (line / space) ratios of 10 μm / 10 μm, 5 μm / 50 μm, and 3 μm / 3 μm can be formed using the method described in [Evaluation of Resin Composition Resolution] in the Examples below. In this case, the aspect ratio of each wire layer can be preferably set to 0.6 or greater, and more preferably 1 or greater.
[0382] The coating resin composition can be cured by exposure and then heating as needed. Thus, a cured product can be obtained from the coating resin composition. Generally, among the components contained in the coating resin composition, volatile components such as (g) solvent can be volatilized by heat during drying or curing, but non-volatile components such as (a) to (f) components will not volatilize. Therefore, the cured product of the coating resin composition can contain the non-volatile components of the coating resin composition or their reaction products.
[0383] The coating resin composition can provide a cured product having a refractive index suitable for forming an optical waveguide. clad The range of the optical waveguide with the desired aperture NA is not limited. For example, the refractive index n of the cured product of the coating resin composition at a wavelength of 1310 nm is measured. clad The refractive index of the coating resin composition is preferably 1.4000 or more, more preferably 1.5000 or more, and particularly preferably 1.5900 or more, and is preferably 1.6500 or less, more preferably 1.61000 or less, and particularly preferably 1.6006 or less. The refractive index of the coating resin composition can be measured by the method described in [Measurement of the Refractive Index of the Cured Material of the Resin Composition] in the Examples described below.
[0384] The coating resin composition can produce a cured product having excellent mechanical strength. For example, when the elongation at break of the cured product is measured by the method described in [Measurement of Elongation at Break of a Cured Product of a Resin Composition] in the Examples described below, the cured product preferably has an elongation at break of 1% or greater.
[0385] The coating resin composition can provide a cured product having excellent heat resistance. For example, when a cured product obtained under the conditions described in the "(Appearance Observation after Reflow)" is heat-treated using the conditions described in the Examples below, the generation of voids can be suppressed. Furthermore, it is preferred that the cured product be able to suppress peeling from a substrate such as a silicon wafer.
[0386] The coating resin composition can be used as a photosensitive resin composition for forming a coating layer of an optical waveguide. For example, the coating resin composition can be used to form an optical waveguide capable of transmitting light having a wavelength of 1300 nm to 1320 nm. In particular, the coating resin composition is preferably used to form a single-mode optical waveguide, for example, a single-mode optical waveguide for light having a wavelength of 1310 nm.
[0387] [4. Relationship between the Cured Product of the Core Resin Composition and the Cured Product of the Covering Resin Composition]
[0388] The cured product of the core resin composition and the cured product of the covering resin composition have a refractive index n such that the aperture NA represented by the following formula (1) falls within a specific range.core and refractive index n clad .
[0389] [Formula 8]
[0390]
[0391] In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad Refractive index n represents the refractive index of the cured product of the coating resin composition. core and refractive index n clad The measurement wavelength is the wavelength of light transmitted by the optical waveguide, for example, 1310 nm. Specifically, the numerical aperture NA is usually greater than 0.05, preferably greater than 0.06, and particularly preferably greater than 0.065. Furthermore, it is usually less than 0.4, preferably 0.35 or less, more preferably 0.3 or less, and particularly preferably 0.2 or less.
[0392] The refractive index of the cured product of the photosensitive resin composition such as the core resin composition and the coating resin composition can be measured by the following method. The photosensitive resin composition is exposed to an optimum exposure dose of 3000 mJ and then heated at 90°C for 3 minutes. Furthermore, a 23°C and 2.38% by mass tetramethylammonium hydroxide aqueous solution is sprayed as a developer at a spray pressure of 0.1 MPa for 30 seconds to perform development. After this development, a 3 J / cm 2 The cured product was irradiated with ultraviolet light and then heated at 190°C for 90 minutes under a nitrogen atmosphere to obtain a cured product. The refractive index of the cured product was measured at room temperature and pressure (23°C, 1 atm). The specific measurement method can be the method described in [Measurement of the Refractive Index of the Cured Product of the Resin Composition] in the Examples.
[0393] When the aperture number NA falls within the above range, the optical waveguide including the core layer comprising the cured product of the core resin composition and the cladding layer comprising the cured product of the cladding resin composition can suppress the transmission loss of light. core and n clad The transmission loss of light at the measurement wavelength is preferably 2.0 dB / cm or less, more preferably 1.8 dB / cm or less, and particularly preferably 1.6 dB / cm or less. The lower limit of the transmission loss is ideally 0.0 dB / cm, and is usually 0.1 dB / cm or more.
[0394] The transmission loss of the optical waveguide can be measured by the method described in [Evaluation of Optical Waveguide] in the Examples described later.
[0395] Furthermore, the optical waveguide generally has excellent heat resistance and, therefore, can exhibit excellent reflow resistance. Specifically, when subjected to heat treatment using a reflow apparatus, the optical waveguide generally suppresses the formation of voids. Furthermore, when subjected to the heat treatment, the optical waveguide generally suppresses delamination from the substrate (e.g., a silicon wafer) on which the optical waveguide is mounted.
[0396] The heat treatment using a reflow apparatus can be performed by, for example, the method described in [Evaluation of Optical Waveguide] in the Examples described later.
[0397] The present inventors speculate that the principle that can achieve the above-mentioned effects is as follows. However, the technical scope of the present invention is not limited to the following principle.
[0398] Generally speaking, factors contributing to transmission loss in optical waveguides include attenuation caused by light absorption by materials contained in the core layer and attenuation caused by light reflection at the interface between the core layer and the cladding layer. In contrast, a cured product of a core resin composition containing components (A) to (C) can suppress light absorption.
[0399] In addition, when the numerical aperture NA is within the above-mentioned specific range, attenuation due to reflection at the interface between the core layer and the cladding layer can be suppressed.
[0400] For example, when forming an optical waveguide, heat is typically applied to the core resin composition and the cladding resin composition. This results in a thermal history being applied to the core and cladding layers, but this thermal history can become locally non-uniform in a portion of the optical waveguide. In this case, the difference in refractive index between the core and cladding layers in that portion can become too small, potentially leading to insufficient reflection at the interface in that portion. However, when the numerical aperture (NA) falls within the aforementioned specific range, even if a portion with a non-uniform thermal history occurs, the difference in refractive index between the core and cladding layers can be maintained at a consistently large value, thereby suppressing attenuation during reflection at the interface.
[0401] And then, when for example usually core layer and cladding are formed by the cured product of resin combination, the stress that a part or all of the refractive index of cured product may apply during because of processing and changes.Even if refractive index changes and produces the too little part of the difference of the refractive index of core layer and cladding, the reflection at the interface of this part may also be insufficient.But, when number of apertures NA is above the lower limit of aforementioned scope, even if stress is applied during processing, also can make the difference of the refractive index of core layer and cladding stably big.Thereby, attenuation when can suppress the reflection at interface.
[0402] In addition, when the above-mentioned number of openings NA is below the upper limit of the above-mentioned range, the cured product of the core resin composition and the cured product of the coating resin composition have a similar refractive index, and thus, can have a similar composition. Thus, even if there is a refractive index change due to the influence of the heat and moisture applied during manufacture and use, the same degree of this change can be produced in the core layer and the coating layer. Therefore, the change of the difference in the refractive index between the core layer and the coating layer can be suppressed, and the difference in the refractive index is stably large, and therefore, the attenuation during the reflection at the interface can be suppressed. In addition, when the cured product of the core resin composition and the cured product of the coating resin composition have a similar composition, the affinity of the core layer and the coating layer can be improved, and therefore, the smoothness of the interface can be highly improved. Thus, microscopically, the generation of the part where the angle of incidence of light incident on the interface becomes smaller can be suppressed, and therefore, the light in the core layer can be suppressed from leaking out to the coating layer, and the attenuation during the reflection at the interface can be suppressed.
[0403] Furthermore, commonly used focusing modules have a relatively small aperture. In contrast, when an optical waveguide having the aforementioned aperture NA transmits light to a focusing module with a smaller aperture, as described above, it is possible to suppress light leakage. This reduces connection loss on the optical waveguide's output side, thereby also suppressing transmission loss.
[0404] Therefore, transmission loss can be suppressed.
[0405] In addition, about the cured product of core resin composition and the cured product of coating resin composition, usually the material itself can have high heat resistance. And then, the cured product of core resin composition and the cured product of coating resin composition can have high affinity, therefore, can smoothly reach the close fitting of core layer and coating layer, thus, can suppress the residual of air at the interface between core layer and coating layer. And then, can improve the close fitting of core layer and coating layer, therefore, can suppress the peeling at the interface between core layer and coating layer. Therefore, can suppress the hole formation during heat treatment. And then, the cured product of core resin composition and the cured product of coating resin composition can have high mechanical strength, therefore, can suppress the generation of peeling (delamination) with resin destruction, thus, can suppress the peeling from base material. Therefore, usually can have high heat resistance.
[0406] Furthermore, when the cured product of the core resin composition and the cured product of the cladding resin composition have similar compositions, properties such as the coefficient of linear thermal expansion (CTE) and elasticity of the core and cladding layers can be similar. Consequently, in durability tests such as long-term heat resistance tests and damp heat tests, the core and cladding layers can exhibit similar refractive index fluctuation behaviors. This improves the heat resistance and damp heat resistance of the optical waveguide, and, in the aforementioned durability tests, can prevent the numerical aperture (NA) from unexpectedly deviating from the design range, thereby suppressing transmission loss.
[0407] From the viewpoint of improving the heat resistance and moisture-heat resistance of the optical waveguide, the difference ΔCTE between the linear thermal expansion coefficient of the cured product of the core resin composition and the linear thermal expansion coefficient of the cured product of the coating resin composition is preferably small. The specific range of the difference ΔCTE of the linear thermal expansion coefficient is preferably 20 ppm / °C or less, more preferably 18 ppm / °C or less, and particularly preferably 15 ppm / °C or less. The linear thermal expansion coefficient of the cured product of the core resin composition may be greater than that of the cured product of the coating resin composition, but the linear thermal expansion coefficient of the cured product of the coating resin composition is preferably greater than that of the cured product of the core resin composition. The linear thermal expansion coefficient of the cured product of the core resin composition and the linear thermal expansion coefficient of the cured product of the coating resin composition can be measured by the method described in [Measurement of the linear thermal expansion coefficient of the cured product of the resin composition] in the Examples.
[0408] The wavelength of light transmitted by an optical waveguide manufactured using the core resin composition and the cladding resin composition can be selected from a variety of wavelengths. For example, preferred wavelengths of light transmitted may range from 840 nm to 860 nm (e.g., 850 nm), 1300 nm to 1320 nm (e.g., 1310 nm), and 1540 nm to 1560 nm (e.g., 1550 nm). The core resin composition and the cladding resin composition are preferably used to manufacture an optical waveguide capable of transmitting light with a wavelength of 1300 nm to 1320 nm.
[0409] Optical waveguides include single-mode optical waveguides and multimode optical waveguides. The core resin composition and cladding resin composition can be used to manufacture either single-mode or multimode optical waveguides. The core resin composition and cladding resin composition are preferably used to manufacture single-mode optical waveguides. Therefore, for example, they are preferably used to manufacture single-mode optical waveguides for light within the aforementioned preferred wavelength range.
[0410] [5. Piece Kit]
[0411] Photosensitive resin compositions such as the above-mentioned core resin composition and the coating resin composition can be used as resin sheets. A resin sheet is a sheet having a resin composition layer containing a photosensitive resin composition. Thus, a resin sheet having a resin composition layer containing the core resin composition (hereinafter sometimes referred to as a "core resin sheet") can be obtained from the core resin composition. In addition, a resin sheet having a resin composition layer containing the coating resin composition can be obtained from the coating resin composition (hereinafter sometimes referred to as a "coating resin sheet."). Furthermore, a sheet set comprising these core resin sheets and coating resin sheets can be obtained in the form of a sheet set for manufacturing an optical waveguide. If these sheet sets, core resin sheets, and coating resin sheets are utilized, the same advantages as the above-mentioned photosensitive resin composition set, core resin composition, and coating resin composition can be obtained, and further, an optical waveguide can be manufactured by a lamination method, and therefore, the manufacture of the optical waveguide can be simply performed.
[0412] [5.1. Core resin sheet]
[0413] The resin composition layer of the core resin sheet typically comprises a core resin composition, and preferably comprises only the core resin composition. The thickness of the resin composition layer of the core resin sheet can be set according to the thickness of the core layer. Specifically, the thickness of the resin composition layer of the core resin sheet is preferably 0.5 μm or greater, more preferably 1 μm or greater, and even more preferably 3 μm or greater, and is preferably 100 μm or less, more preferably 50 μm or less, and particularly preferably 20 μm or less.
[0414] The core resin sheet may include a support. For example, the core resin sheet may include a support and a resin composition layer formed on the support. Examples of the support include polyethylene terephthalate films, polyethylene naphthalate films, polypropylene films, polyethylene films, polyvinyl alcohol films, triacetoacetate films, and the like, with polyethylene terephthalate films being particularly preferred. Commercially available supports include, for example, products such as "Alphan MA-410" and "E-200C" manufactured by Oji Paper Co., Ltd.; polypropylene films such as those manufactured by Shin-Etsu Paper Co., Ltd.; and polyethylene terephthalate films such as PS series products such as "PS-25" manufactured by Teijin Limited. In order to facilitate the peeling of the support after lamination, a peeling agent such as an alkyd release agent or a silicone coating agent may be applied to the surface of the support. The thickness of the support is preferably in the range of 5 μm to 100 μm, more preferably in the range of 10 μm to 50 μm.
[0415] The core resin sheet may include a protective film for protecting the resin composition layer. Typically, the protective film is provided on the side of the resin composition layer opposite to the support. As the protective film, for example, a film formed from the same material as the support can be used. The adhesion between the protective film and the resin composition layer is preferably less than the adhesion between the support and the resin composition layer. Typically, the core resin sheet is used after the protective film is removed.
[0416] The core resin sheet can be produced, for example, by coating a core resin composition on a support. To facilitate coating, a varnish-like core resin composition containing a solvent can be prepared and applied. When applying the core resin composition containing a solvent, drying can be performed after application, as needed.
[0417] The resin composition layer of the core resin sheet may contain a solvent, preferably in a small amount. In one example, the amount of solvent contained in the resin composition layer is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, relative to 100% by mass of the total amount of the resin composition layer.
[0418] [5.2. Coating resin sheet]
[0419] The resin composition layer of the covering resin sheet typically comprises the covering resin composition, and preferably comprises only the covering resin composition. The thickness of the resin composition layer of the covering resin sheet can be set according to the thickness of the covering layer. Specifically, the thickness of the resin composition layer of the covering resin sheet is preferably 5 μm or greater, more preferably 7 μm or greater, and even more preferably 10 μm or greater, and is preferably 40 μm or less, more preferably 30 μm or less, and particularly preferably 20 μm or less.
[0420] The coating resin sheet may be the same as the core resin sheet, except that it includes the aforementioned resin composition layer containing the coating resin composition instead of the resin composition layer containing the core resin composition. Therefore, the coating resin sheet may include a support. The support of the coating resin sheet may be the same as the support of the core resin sheet. Furthermore, the coating resin sheet may include a protective film. The protective film of the coating resin sheet may be the same as the protective film of the core resin sheet. Typically, the coating resin sheet can be used after the protective film is removed.
[0421] The cover resin sheet can be produced by the same method as that of the core resin sheet, except that the cover resin composition is used instead of the core resin composition.
[0422] The resin composition layer of the cover resin sheet may contain a solvent, preferably in a small amount. In one example, the range of the amount of solvent contained in the resin composition layer of the cover resin sheet may be the same as the range of the amount of solvent contained in the resin composition layer of the core resin sheet.
[0423] [6. Optical waveguide]
[0424] The core resin composition, core resin sheet, cladding resin composition, cladding resin sheet, photosensitive resin composition kit, and sheet kit can be used to produce an optical waveguide. Hereinafter, embodiments of the optical waveguide will be described using the accompanying drawings.
[0425] Figure 1 FIG is a perspective view schematically showing an optical waveguide 10 according to an embodiment of the present invention. Figure 1 As shown, the optical waveguide 10 includes a core layer 100 and a cladding layer 200. The core layer 100 comprises a cured product of a core resin composition, preferably only a cured product of the core resin composition. Furthermore, the cladding layer 200 comprises a cured product of a coating resin composition, preferably only a cured product of the coating resin composition.
[0426] The core layer 100 is disposed in the cladding layer 200. Thus, the core layer 100 is covered by the cladding layer 200. Typically, the entire circumference of the core layer 100 is covered by the cladding layer 200. The core layer 100 and the cladding layer 200 are in direct contact with each other without any other layer being sandwiched therebetween, and thus, an interface 100I can be formed between the core layer 100 and the cladding layer 200. Light (not shown) can typically be transmitted within the core layer 100 from one end (the incident side) 100A of the core layer 100 to the other end (the exit side) 100B while being repeatedly reflected by the aforementioned interface 100I.
[0427] The wavelength of light that can be transmitted through the optical waveguide 10 can be selected from a variety of wavelengths. For example, preferred wavelengths of light to be transmitted may range from 840 nm to 860 nm (e.g., 850 nm), 1300 nm to 1320 nm (e.g., 1310 nm), or 1540 nm to 1560 nm (e.g., 1550 nm). The wavelength of light transmitted through the optical transmission path 10 is preferably in the range of 1300 nm to 1320 nm.
[0428] The optical waveguide 10 can be a single-mode optical waveguide or a multi-mode optical waveguide, but is preferably a single-mode optical waveguide. The optical waveguide 10 is preferably a single-mode optical waveguide for light within the aforementioned preferred wavelength range. For example, the optical waveguide 10 is preferably a single-mode optical waveguide for light at 1310 nm.
[0429] The width L of the core layer 100 is preferably set appropriately within a range that allows light to be transmitted. Specifically, the line width L of the core layer 100 is preferably 0.5 μm or greater, more preferably 1 μm or greater, and particularly preferably 2 μm or greater, and is preferably 50 μm or less, more preferably 30 μm or less, and particularly preferably 20 μm or less. It can be 10 μm or less or 5 μm or less. The width L of the core layer 100 corresponds to the line width (line) of the core layer 100 when viewed in the thickness direction.
[0430] The spacing S of the core layers 100 is preferably set appropriately within a range that allows light to be transmitted. Specifically, the spacing S of the core layers 100 is preferably 50 μm or greater, more preferably 70 μm or greater, and particularly preferably 100 μm or greater, and is preferably 1000 μm or less, more preferably 500 μm or less, and particularly preferably 300 μm or less. The spacing S of the core layers 100 corresponds to the spacing (space) between the core layers as viewed in the thickness direction.
[0431] The thickness T of the core layer 100 is desirably set appropriately within a range that allows light to be transmitted. Specifically, the thickness T of the core layer 100 is preferably 0.5 μm or greater, more preferably 1 μm or greater, and particularly preferably 2 μm or greater, and is preferably 50 μm or less, more preferably 30 μm or less, and particularly preferably 20 μm or less, and may be 10 μm or less.
[0432] The thickness of the cladding layer 200 is generally greater than that of the core layer 100. The specific thickness of the cladding layer 200 is preferably 5 μm or more, more preferably 7 μm or more, particularly preferably 10 μm or more, and preferably 100 μm or less, more preferably 60 μm or less, further preferably 40 μm or less, further preferably 30 μm or less, and particularly preferably 20 μm or less.
[0433] The optical waveguide 10 may include any elements other than the core layer 100 and the cladding layer 200 as needed. For example, the optical waveguide 10 may include a substrate 300. In the optical waveguide 10 including the substrate 300, the cladding layer 200 is generally provided on the substrate 300, and the core layer 100 is provided within the cladding layer 200.
[0434] As the substrate 300, a hard substrate such as a glass substrate, a metal substrate, a ceramic substrate, a wafer, a circuit substrate, etc. can be used. As the wafer, for example, a semiconductor wafer such as a silicon wafer, a gallium arsenide (GaAs) wafer, an indium phosphide (InP) wafer, a gallium phosphide (GaP) wafer, a gallium nitride (GaN) wafer, a gallium telluride (GaTe) wafer, a zinc selenide (ZnSe) wafer, a silicon carbide (SiC) wafer, etc. can be used, or a simulation wafer can be used. As the simulation wafer, for example, a plate-like member having a molding resin and electronic components embedded in the molding resin can be used. As the circuit substrate, for example, a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, etc. can be listed. It should be noted that the circuit substrate here refers to a substrate having a patterned conductor layer (circuit) formed on one or both sides of the substrate as described above. Furthermore, a film formed of a plastic material such as polyethylene terephthalate, polyimide, or polyester can be used as the substrate 300 . Furthermore, a flexible circuit board can be used as the substrate 300 .
[0435] The optical waveguide 10 may optionally include a protective layer (not shown) for protecting the core layer 100 and the cladding layer 200. The protective layer may be provided, for example, to cover the surface of the cladding layer 200 opposite to the substrate 300.
[0436] As described above, the optical waveguide 10 can have low transmission loss. Furthermore, the optical waveguide 10 generally has excellent heat resistance, for example, excellent reflow resistance. Furthermore, the optical waveguide 10 can be formed using a core resin composition and a cladding resin composition having excellent resolution. This allows for fine wiring in the core layer and, as described above, allows for formation with a small line width L.
[0437] The optical waveguide 10 can be produced by using the core resin composition and the cladding resin composition in combination. For example, the optical waveguide 10 can be produced by a method including the following steps in sequence.
[0438] A step (I) of forming a first composition layer comprising a coating resin composition;
[0439] a step (II) of subjecting the first composition layer to an exposure treatment;
[0440] Step (III) of curing the first composition layer;
[0441] a step (IV) of forming a second composition layer comprising a core resin composition on the first composition layer;
[0442] a step (V) of subjecting the second composition layer to an exposure treatment;
[0443] a step (VI) of subjecting the second composition layer to a development treatment;
[0444] a step (VII) of curing the second composition layer;
[0445] a step (VIII) of forming a third composition layer comprising a coating resin composition on the second composition layer;
[0446] a step (IX) of subjecting the third composition layer to an exposure treatment; and
[0447] A step (X) of curing the third composition layer.
[0448] Figure 2 Schematic cross-sectional view for explaining step (I) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. Figure 2 As shown, the optical waveguide manufacturing method according to one embodiment of the present invention includes a step (I) of forming a first composition layer 210 containing a coating resin composition. In this embodiment, an example of forming the first composition layer 210 on a substrate 300 is described.
[0449] There is no particular limitation on the method for forming the first composition layer 210. For example, the first composition layer 210 can be formed by coating the coating resin composition on the substrate 300. To facilitate coating, a varnish-like coating resin composition containing a solvent can be prepared and coated.
[0450] Examples of coating methods include gravure coating, micro gravure coating, reverse coating, kiss reverse coating, die coating, slot die coating, lip coating, comma coating, blade coating, roll coating, knife coating, curtain coating, chamber gravure coating, slot orifice coating, spin coating, slit coating, spray coating, dip coating, hot melt coating, rod coating, applicator coating, air knife coating, curtain coating, offset printing, brush coating, and screen printing.
[0451] The coating resin composition can be applied once or several times. In addition, different coating methods can be combined. In order to avoid foreign matter from being mixed in, the coating is preferably implemented in an environment where foreign matter such as a clean room is less likely to be generated.
[0452] After the coating of the coating resin composition, the first composition layer 210 can be dried as needed. Drying can be carried out using a drying device such as a hot air furnace and a far infrared furnace. The drying conditions are preferably set appropriately according to the composition of the coating resin composition. If specific examples are given, the drying temperature is preferably 50°C or more, more preferably 70°C or more, particularly preferably 80°C or more, and preferably 150°C or less, more preferably 130°C or less, particularly preferably 120°C or less. In addition, the drying time is preferably 30 seconds or more, more preferably 60 seconds or more, particularly preferably 120 seconds or more, and preferably 60 minutes or less, more preferably 20 minutes or less, particularly preferably 5 minutes or less.
[0453] The first composition layer 210 can be formed using, for example, a coating resin sheet. Specifically, the first composition layer 210 can be formed on the substrate 300 by laminating the resin composition layer of the coating resin sheet onto the substrate 300. Lamination is typically performed by pressing the resin composition layer of the resin sheet onto the substrate 300 while heating it. Lamination is preferably performed under reduced pressure by a vacuum lamination method. Furthermore, prior to lamination, a preheating treatment may be performed to heat the resin sheet and the substrate, as needed.
[0454] The lamination conditions can be, for example, a lamination temperature of 70°C to 140°C and a lamination pressure of 1 kgf / cm 2 ~11kgf / cm 2 (9.8×10 4 N / m 2 ~107.9×10 4 N / m 2 ), the pressing time is 5 seconds to 300 seconds. In addition, lamination is preferably carried out under reduced pressure with the air pressure being 20 mmHg (26.7 hPa) or less. Lamination can be carried out in a batch manner or in a continuous manner using rollers.
[0455] The vacuum lamination method can be performed using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum applicator manufactured by Niccol Materials, a vacuum pressure laminator manufactured by Meiki Manufacturing Co., Ltd., a roll dry coater manufactured by Hitachi Industrie Co., Ltd., and a vacuum laminator manufactured by Hitachi Airline Co., Ltd.
[0456] When the first composition layer 210 is formed using a covering resin sheet having a support, the support is usually peeled off at an appropriate time before step (IV).
[0457] The first composition layer 210 formed on the substrate 300 in step (I) usually contains a coating resin composition, and preferably contains only a coating resin composition.
[0458] In the method for manufacturing an optical waveguide according to one embodiment of the present invention, after step (I), step (II) of subjecting the first composition layer 210 to an exposure treatment is included. In this exposure treatment, the first composition layer 210 is irradiated with light. When irradiated with light, the (b) photoacid generator generates acid in the first composition layer 210. As the light used in the exposure treatment, it is preferred to use appropriate active light that matches the composition of the coating resin composition. The wavelength of the active light is generally 190 nm to 1000 nm, preferably 240 nm to 550 nm, and light of other wavelengths can be used. Specific examples of active light sources include ultraviolet rays, visible rays, electron beams, X-rays, etc., and ultraviolet rays are particularly preferred.
[0459] The exposure dose of light is preferably set so that the first composition layer 210 in step (III) can be cured. In one example, the specific exposure dose is preferably in the range of 10 mJ / cm 2 More preferably, 50 mJ / cm 2 More than, particularly preferably 200mJ / cm 2 More than, and preferably 10,000 mJ / cm 2 Less than, more preferably 8,000 mJ / cm 2 Below, more preferably 4,000 mJ / cm 2 Below, particularly preferably 1,000 mJ / cm 2 the following.
[0460] When the first composition layer 210 is formed using a coating resin sheet having a support, in step (II), a support (not shown) may be present on the first composition layer 210. When a support is present on the first composition layer 210, exposure may be performed through the support or after peeling the support.
[0461] In the method for manufacturing an optical waveguide according to one embodiment of the present invention, after step (II), a step (III) of curing the first composition layer 210 is included. This step (III) generally includes heat-treating the first composition layer 210. According to the heat treatment, the cross-linking reaction of the cross-linking agent (c) is carried out using the acid generated in step (II) as a catalyst, so that the first composition layer 210 can be cured. The heat treatment conditions can be selected according to the type and amount of the resin component in the coating resin composition, and are preferably in the range of 150°C to 250°C and 20 minutes to 180 minutes, and more preferably in the range of 160°C to 230°C and 30 minutes to 120 minutes. The heat treatment is preferably performed in an inert atmosphere such as a nitrogen atmosphere.
[0462] Figure 31 is a schematic cross-sectional view for explaining step (III) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. By curing the first composition layer 210 in step (III), Figure 3 As shown, a cured first composition layer 220 is obtained on the substrate 300. The cured first composition layer 220 forms a portion of the covering layer 200, and is sometimes referred to as a "lower covering layer" 220 hereinafter.
[0463] Figure 4 : is a schematic cross-sectional view for explaining step (IV) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. In the method for manufacturing an optical waveguide according to one embodiment of the present invention, after step (III), as Figure 4 As shown, the process includes a step (IV) of forming a second composition layer 110 containing a core resin composition on the lower cladding layer 220 which is a cured first composition layer.
[0464] The method for forming the second composition layer 110 is not particularly limited. For example, the second composition layer 110 can be formed by applying the core resin composition to the lower coating layer 220. From the perspective of smooth coating, a varnish-like core resin composition containing a solvent can be prepared and the varnish-like core resin composition can be applied. The coating of the core resin composition can be carried out in the same manner as the coating resin composition. In addition, after the coating of the core resin composition, the second composition layer 110 can be dried as needed. The drying of the second composition layer 110 can be carried out using the same method and conditions as the drying of the first composition layer 210.
[0465] The second composition layer 110 can be formed using, for example, a core resin sheet. Specific examples are given, whereby the resin composition layer of the core resin sheet is laminated onto the lower cladding layer 220, thereby forming the second composition layer 110 on the lower cladding layer 220. The lamination of the core resin sheet can be performed in the same manner as the lamination of the cladding resin sheet. Furthermore, when the second composition layer 110 is formed using a core resin sheet having a support, the support is typically peeled off at an appropriate time prior to step (VI).
[0466] The second composition layer 110 formed on the lower cladding layer 220 in step (IV) usually contains a core resin composition, and preferably contains only a core resin composition.
[0467] Figure 5 : is a schematic cross-sectional view for explaining step (V) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. Figure 5As shown, after step (IV), step (V) of subjecting the second composition layer 110 to an exposure treatment is included.
[0468] In step (V), a latent image is formed on the second composition layer 110 through an exposure treatment. Specifically, during the exposure treatment, light P is selectively irradiated onto a specific portion of the second composition layer 110. Therefore, when the exposure treatment is performed, an exposed portion 111, which is irradiated with light, and a non-exposed portion 112, which is not irradiated with light, are formed in the second composition layer 110. Typically, the core resin composition functions as a negative-type photosensitive resin composition, so a latent image corresponding to the core layer is formed in the exposed portion 111.
[0469] From the viewpoint of selective exposure, the exposure treatment in step (V) is usually performed using a mask 400. Specifically, in this exposure treatment, light P is irradiated onto the second composition layer 110 via the mask 400 having a light-transmitting portion 410 and a light-shielding portion 420. The light P is incident on the exposure portion 111 through the light-transmitting portion 410, but cannot be incident on the non-exposure portion 112 by passing through the light-shielding portion 420. Therefore, the exposure portion 111 and the non-exposure portion 112 corresponding to the light-transmitting portion 410 and the light-shielding portion 420 can be provided on the second composition layer 110. The mask 400 can be as follows: Figure 5 As shown, the exposure method may be performed in close contact with the second composition layer 110 (contact exposure method), or exposure may be performed using parallel light without close contact (non-contact exposure method).
[0470] Generally speaking, the light-transmitting portion 410 of the mask 400 is formed to have a planar shape corresponding to the core layer of the optical waveguide. Consequently, the light-shielding portion 420 of the mask 400 is formed to have a planar shape corresponding to the portion of the optical waveguide without the core layer. Unless otherwise specified, the term "planar shape" refers to the shape as viewed from the thickness direction. Hereinafter, the light-transmitting portion 410 formed in a planar shape corresponding to the core layer may be referred to as a "mask pattern."
[0471] As the light P used in the exposure treatment of step (V), active light rays in the same range as those used in the exposure treatment of the first composition layer 210 in step (II) can be used. The exposure dose of light P is preferably set so that the desired core layer can be formed after curing in step (VII). In one example, the specific exposure dose in step (V) can be in the same range as that used for the first composition layer 210 in step (II).
[0472] When the second composition layer 110 is formed using a core resin sheet having a support, in step (V), a support (not shown) may be present on the second composition layer 110. When a support is present on the second composition layer 110, exposure may be performed through the support or after peeling the support.
[0473] The core resin composition functions as a negative-type photosensitive resin composition. Therefore, in the exposed portion 111, the photoacid generator (B) generates acid. This acid acts as a catalyst, causing the crosslinking reaction of the crosslinker (C) to proceed, resulting in reduced solubility in the developer. On the other hand, in the unexposed portion 112, the photoacid generator (B) does not generate acid, so the crosslinking reaction of the crosslinker (C) does not proceed or proceeds only to a limited extent, resulting in higher solubility in the developer. This difference in solubility between the exposed and unexposed portions 111, 112, is exploited to enable development in the subsequent step (VI).
[0474] In the optical waveguide manufacturing method according to one embodiment of the present invention, a step (XI) of heating the second composition layer 110 may be included after step (V) and before step (VI). The heating in step (XI) can promote the crosslinking reaction of the crosslinking agent (C). As a result, the solubility of the exposed portion 111 in the developer can be rapidly reduced. The heating in step (XI) can be performed using a hot plate or an oven. The heating temperature can be, for example, 40°C to 110°C. Furthermore, the heating time can be, for example, 30 seconds to 60 minutes.
[0475] Figure 6 This is a schematic cross-sectional view for explaining step (VI) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. The method for manufacturing an optical waveguide according to one embodiment of the present invention includes a step (VI) of performing a development treatment on the second composition layer 110 after step (V). The development treatment enables the latent image formed in step (V) to be developed. The core resin composition functions as a negative photosensitive resin composition, and therefore, as shown in FIG. Figure 6 As shown, the exposed portion 111 is not removed by the development process, while the non-exposed portion 112 (see FIG. Figure 5 ) is removed. The exposed portion 111 of the second composition layer 110 remaining after development may have a light-transmitting portion 410 (refer to FIG. 4 ) of the mask 400 used in step (V) Figure 5 ) has the same planar shape as the mask pattern.
[0476] The developing method is generally a wet developing method in which the second composition layer 110 is brought into contact with a developer. Examples of the developer include an alkaline aqueous solution, an aqueous developer, and an organic solvent.
[0477] As for the alkaline aqueous solution as a developer, for example, an aqueous solution of an alkali metal compound can be cited. As the alkali metal compound, for example, alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; alkali metal carbonates or bicarbonates such as sodium carbonate and sodium bicarbonate; alkali metal phosphates such as sodium phosphate and potassium phosphate; alkali metal pyrophosphates such as sodium pyrophosphate and potassium pyrophosphate, etc. can be cited. In addition, as the alkaline aqueous solution, for example, an aqueous solution of an organic base that does not contain metal ions such as tetraalkylammonium hydroxide can be cited. One alkaline aqueous solution can be used alone, or two or more can be used in combination. Among them, from the viewpoint of not containing metal ions, an aqueous solution of tetramethylammonium hydroxide (TMAH) is preferred. In one example, the pH range of the alkaline aqueous solution is preferably 8 or more, more preferably 9 or more, and preferably 14 or less, more preferably 12 or less, and particularly preferably 11 or less. In addition, the alkali concentration of the alkaline aqueous solution is preferably 0.1% by mass to 10% by mass.
[0478] Examples of organic solvents used in the developer include acetone, ethyl acetate, alkoxyethanols having an alkoxy group with 1 to 4 carbon atoms, ethanol, isopropyl alcohol, butanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether. One organic solvent may be used alone or in combination of two or more. The concentration of the organic solvent relative to the total amount of the developer is generally 2% by mass or more, preferably 50% by mass or more, more preferably 70% by mass or more, and particularly preferably 90% by mass or more. The developer may contain 100% by mass of the organic solvent. Examples of organic solvent-based developers used alone include 1,1,1-trichloroethane, N-methylpyrrolidone, N,N-dimethylformamide, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone.
[0479] The developer may contain additives such as a surfactant and a defoaming agent to enhance the developing effect as needed.
[0480] The development time is preferably 10 seconds to 5 minutes. The temperature of the developer during development is not particularly limited, but is preferably 20° C. or higher, preferably 50° C. or lower, and more preferably 40° C. or lower.
[0481] Examples of development methods include a puddle method, a spray method, an immersion method, a brush method, a scraping method, and an ultrasonic method. Among these, the spray method is preferred for improving resolution. The spray pressure when using the spray method is preferably 0.05 MPa to 0.3 MPa.
[0482] After development with a developer, the second composition layer 110 can be rinsed. Rinse is preferably performed using a solvent different from the developer. For example, the same solvent as that contained in the core resin composition or water can be used for rinsing. The rinsing time is preferably 5 seconds to 1 minute.
[0483] The optical waveguide manufacturing method according to one embodiment of the present invention includes, after step (VI), step (VII) of curing the second composition layer 110. This step (VII) typically includes heat-treating the second composition layer 110. The heat treatment allows the crosslinking agent (C) to undergo a crosslinking reaction, thereby curing the second composition layer 110. The heat treatment conditions can be selected based on the type and amount of the resin component in the core resin composition. For example, the heat treatment conditions in step (VII) can be the same as those used for the heat treatment of the first composition layer 210 in step (III).
[0484] Figure 7 : is a schematic cross-sectional view for explaining step (VII) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. By curing the second composition layer 110 in step (VII), Figure 7 As shown, the core layer 100 as the cured second composition layer is obtained on the lower cladding layer 220 .
[0485] Figure 8 Schematic cross-sectional view for explaining step (VIII) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. Figure 8 As shown, the optical waveguide manufacturing method according to one embodiment of the present invention includes, after step (VII), a step (VIII) of forming a third composition layer 230 comprising a cladding resin composition on the core layer 100. The third composition layer 230 is generally formed so as to cover the entire surface of the core layer 100 that is not in contact with the lower cladding layer 220. Therefore, the third composition layer 230 is formed so as to cover the core layer 100 and is also formed on the lower cladding layer 220.
[0486] The method for forming the third composition layer 230 is not particularly limited. For example, the third composition layer 230 can be formed by applying a coating resin composition on the core layer 100. When the coating resin composition is applied to the core layer 100, the coating resin composition can be applied to the lower coating layer 220 as needed. The coating resin composition used to form the third composition layer 230 can be applied in the same manner as the coating resin composition used to form the first composition layer 210. In addition, after applying the coating resin composition, the third composition layer 230 can be dried as needed. The third composition layer 230 can be dried using the same method and conditions as the drying of the first composition layer 210.
[0487] The third composition layer 230 can be formed using, for example, a coating resin sheet. Specifically, the third composition layer 230 can be formed on the core layer 100 by laminating a resin composition layer of the coating resin sheet onto the core layer 100. When the resin composition layer of the coating resin sheet is laminated onto the core layer 100, the resin composition layer of the coating resin sheet can be laminated onto the underlying coating layer 220 as needed. The lamination of the coating resin sheet used to form the third composition layer 230 can be performed in the same manner as the lamination of the coating resin sheet used to form the first composition layer 210. When the third composition layer 230 is formed using a coating resin sheet having a support, the support can be peeled off in any step.
[0488] The third composition layer 230 formed on the core layer 100 in step (VIII) usually contains a coating resin composition, and preferably contains only a coating resin composition.
[0489] The optical waveguide manufacturing method according to one embodiment of the present invention includes, after step (VIII), step (IX) of subjecting the third composition layer 230 to an exposure treatment. In this exposure treatment, the third composition layer 230 is irradiated with light. Upon irradiation with light, the (b) photoacid generator generates an acid in the third composition layer 230. The exposure treatment of the third composition layer 230 can be performed in the same manner as the exposure treatment of the first composition layer 210.
[0490] The optical waveguide manufacturing method according to one embodiment of the present invention includes, after step (IX), a step (X) of curing the third composition layer 230. This step (X) typically includes heat-treating the third composition layer 230. During the heat treatment, the cross-linking reaction of the cross-linking agent (c) proceeds using the acid generated in step (IX) as a catalyst, thereby curing the third composition layer 230. The heat treatment of the third composition layer 230 can be performed in the same manner as the heat treatment of the first composition layer 210.
[0491] Figure 9 1 is a schematic cross-sectional view for explaining step (X) of the method for manufacturing an optical waveguide according to one embodiment of the present invention. By curing the third composition layer 230 in step (X), Figure 9 As shown, a cured third composition layer 240 is formed on the core layer 100. This cured third composition layer 240 forms a portion of the cladding layer 200 and is hereinafter sometimes referred to as the "upper cladding layer" 240. Furthermore, the cladding layer 200 is formed by the upper cladding layer 240 and the lower cladding layer 220. Thus, the optical waveguide 10 can be obtained, which includes the cladding layer 200 including the lower cladding layer 220 and the upper cladding layer 240, and the core layer 100 disposed within the cladding layer 200.
[0492] The method for manufacturing the optical waveguide 10 may further include an optional step in combination with the above-mentioned steps.
[0493] The method for manufacturing the optical waveguide 10 may include, for example, a step of forming a protective layer (not shown). In addition, the method for manufacturing the optical waveguide 10 may include, for example, a step of dicing the manufactured optical waveguide 10 .
[0494] The above steps can be repeated in the method for manufacturing the optical waveguide 10. For example, steps (I) to (XI) can be repeated to manufacture an optical waveguide having a multilayer structure in which core layers and cladding layers are alternately provided on the substrate 300 in the thickness direction.
[0495] [7. Optoelectronic hybrid substrate]
[0496] The optoelectronic hybrid substrate described in one embodiment of the present invention includes the above-mentioned optical waveguide. Generally, the optoelectronic hybrid substrate includes an optical waveguide and a circuit substrate. The circuit substrate may include electronic components and wiring connected to the electronic components. As electronic components, there may be listed passive components such as capacitors, inductors, resistors, and active components such as semiconductor chips. In addition, the optical waveguide and the wiring of the circuit substrate may be connected by means of a photoelectric conversion element. The photoelectric conversion element may be a combination of a light-emitting element (such as a surface-emitting light-emitting diode) that can convert electricity into light and a light-receiving element (such as a photodiode) that can convert light into electricity. Furthermore, the optoelectronic hybrid substrate may include optical elements such as mirrors in order to adjust the optical path.
[0497] A preferred example of an optoelectronic hybrid substrate includes a chip with an optical integrated circuit formed on a silicon wafer. This chip is expected to be rapidly commercialized using silicon photonics technology, and for example, it is expected to be incorporated into a semiconductor package. An optoelectronic hybrid substrate incorporating this chip comprises, for example, a circuit substrate, a chip mounted on the circuit substrate, and an optical waveguide. The optical waveguide can be used to connect wiring on the circuit substrate to the chip or to connect multiple chips.
[0498] Chips manufactured using silicon photonics technology typically use light with wavelengths of 1310 nm and 1550 nm, with 1310 nm being the most common wavelength (Sho Yoshida, Daisuke Suganuma, and Takaaki Ishiba, "Fabrication and Loss Reduction of Single-Mode Polymer Waveguides Using the Mosquito Method," 28th Spring Conference of the Society of Electronic Device Engineers, 2014). Therefore, optical waveguides are preferably capable of transmitting light at wavelengths of 1310 nm and 1550 nm, or wavelengths close thereto; for example, light with wavelengths of 1300 nm to 1320 nm is preferred. The optical waveguides described in the above embodiments are capable of transmitting light at these wavelengths.
[0499] Generally speaking, between single-mode and multi-mode, single-mode can achieve faster transmission. Therefore, from the perspective of high-speed transmission, as an optical waveguide used in optoelectronic hybrid circuits, a single-mode optical waveguide is preferred. In a single-mode optical waveguide, the width of the core layer is preferably small. For example, it is preferred to form a core layer with a width of less than 10 μm or less than 5 μm. In addition, when the optical waveguide is applied to a semiconductor package, an optical waveguide with a small core layer is also preferred from the perspective of increasing the design freedom of the package. According to the optical waveguide described in the above embodiment, the width of the core layer can be reduced as described above.
[0500] In addition, a single-mode optical waveguide is generally desired to have a small numerical aperture NA. The optical waveguide described in the above embodiment can have a small numerical aperture NA, and therefore can also be applied to a single mode from the viewpoint of the numerical aperture NA.
[0501] On the other hand, when connecting multiple optoelectronic hybrid substrates, these substrates are sometimes connected via optical fibers. For example, multiple optoelectronic hybrid substrates may be placed on a frame and connected to each other via optical fibers. The mainstream optical fibers used to connect these substrates are multimode. Therefore, to ensure connection with these optical fibers, multimode optical waveguides can be used as optical waveguides in the optoelectronic hybrid substrates.
[0502] From the perspective of improving versatility, it is expected that the optical waveguide can be applied in both single mode and multimode. Furthermore, it is expected to reduce the minimum width of the core layer of these optical waveguides and increase the line width freedom of the core layer. According to the optical waveguide described in the above embodiment, by using a core resin composition and a coating resin composition as a photosensitive resin composition with excellent resolution, it is possible to achieve a high fine wiring forming capability, and therefore, the minimum width of the core layer can be reduced. In addition, according to the optical waveguide described in the above embodiment, any optical waveguide in single mode and multimode can also be obtained. Therefore, the optical waveguide described in the above embodiment can be applied to a wide range. Moreover, since it can be applied to a wide range and the transmission loss of light can be suppressed, the optical waveguide described in the above embodiment is suitable for application to optoelectronic hybrid substrates.
[0503] When connecting optical waveguides, it is preferable that the modes of these connected waveguides be identical, and their aperture numbers NA be similar. For example, when transmitting light from a first optical waveguide having an aperture number NA1 to a second optical waveguide having an aperture number NA2, it is desirable that NA1 ≥ NA2 to suppress light leakage at the connection. Therefore, when connecting multiple optical waveguides provided on a single optoelectronic hybrid substrate, it is desirable that the aperture numbers NA of these waveguides be appropriately set as described above.
[0504] Furthermore, when connecting an optical waveguide to an optical fiber, it is desirable that the optical waveguide have an aperture number (NA) within an appropriate range consistent with the aperture number of the optical fiber. For example, single-mode optical fibers with a large aperture number, such as those with an aperture number of 0.35, are already in practical use. Therefore, to ensure connection with a single-mode optical fiber, it is desirable that the single-mode optical waveguide have an aperture number (NA) that is approximately equal to or less than the aperture number of the aforementioned optical fiber. The optical waveguide described in the above embodiment can suppress transmission loss with an aperture number (NA) of 0.35 or less, and is therefore preferably suitable for use as an optical waveguide connected to a single-mode optical fiber.
[0505] Example
[0506] The present invention will be described in detail below with reference to the following examples, but the present invention is not limited to these examples. It should be noted that, in the following descriptions, "parts" and "%" indicating quantities, unless otherwise specified, mean "parts by mass" and "mass %," respectively. Furthermore, the operations described below were performed at room temperature and pressure (23° C., 1 atm) in the atmosphere unless otherwise specified.
[0507] (Synthesis example 1)
[0508] In a flask, 100 g of 4-hydroxyphenyl methacrylate (manufactured by Seiko Chemical Co., Ltd.), 300 g of N,N-dimethylacetamide, and 4.0 g of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed to obtain a reaction solution. The reaction solution was heated to 80° C. under a nitrogen atmosphere and a polymerization reaction was performed for 8 hours. Thereafter, 200 g of methanol was added to the reaction solution and added dropwise to a large amount of stirred ion-exchanged water. The precipitated polymer was filtered and dried to obtain a polymer. When the weight average molecular weight of the polymer was measured by GPC, it was 20,000 in terms of polystyrene.
[0509] [Production Examples 1 to 13]
[0510] The materials in the amounts shown in Tables 1 and 2 were blended and mixed using a high-speed rotary stirrer to obtain a resin varnish as a resin composition. In Tables 1 and 2, the numerical values of each component are expressed in parts by mass. In addition, the abbreviations in Tables 1 and 2 have the following meanings.
[0511] <(A) Phenolic Resin>
[0512] "TR4020G": manufactured by Asahi Organic Materials Co., Ltd., weight-average molecular weight: 13,000.
[0513] "BisP-E": 1,1-bis(4-hydroxyphenyl)propane, manufactured by Asahi Organic Materials Co., Ltd.
[0514] "Bis-AF": 2,2-bis(4-hydroxyphenyl)hexafluoropropane manufactured by Asahi Organic Materials Co., Ltd.
[0515] Marukalinka M: Polyparahydroxystyrene manufactured by Maruzen Petrochemical Co., Ltd.
[0516] “Synthesis Example 1”: the polymer synthesized in Synthesis Example 1.
[0517] "J-DPP-85": manufactured by JFE Chemical Co., Ltd., dicyclopentadiene skeleton-type phenol.
[0518] “SPDI”: manufactured by JFE Chemical Co., Ltd., spirobiindanphenol.
[0519] "TBIS-RX": manufactured by Taoka Chemical Industry Co., Ltd., spiro[fluorene-9,9'-xanthene]-3',6'-diol.
[0520] <(B) Photoacid Generator>
[0521] "PAG-103": a compound manufactured by BASF Corporation and having the following structural formula.
[0522] [Chemistry 35]
[0523]
[0524] <(C) Cross-linking Agent>
[0525] "MW-390", manufactured by Sanwa Chemical Co., Ltd., hexamethoxymethyl melamine.
[0526] <(D) Polymer>
[0527] CB-3098: Produced by Soken Chemical Co., Ltd. This acrylic resin does not contain phenolic hydroxyl groups or methoxymethyl groups. Its weight-average molecular weight is 3,000.
[0528] <(E) Amine Compound>
[0529] "Trioctylamine": manufactured by TCI, tri-n-octylamine.
[0530] <(F) Optional Components>
[0531] “ZCR-1797H”: Acid-modified epoxy acrylate having a biphenyl skeleton, manufactured by Nippon Kayaku Co., Ltd. (70% concentration solution).
[0532] “FA-324A”: Ethylene oxide-modified bisphenol A diacrylate, manufactured by Showa Denko K.K.
[0533] "NC-3000H": Biphenyl skeleton epoxy resin, manufactured by Nippon Kayaku Co., Ltd.
[0534] "Omnirad 819": phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, manufactured by IGM.
[0535] <(G) Solvent>
[0536] "MEK": Methyl ethyl ketone, manufactured by Junsei Chemical Co., Ltd.
[0537] “Cyclohexanone”: dipentaerythritol hexaacrylate, manufactured by Nippon Kayaku Co., Ltd.
[0538] "PGMEAc": propylene glycol monomethyl ether acetate, manufactured by Kanto Chemical Co., Ltd.
[0539] [Manufacturing of resin sheet]
[0540] Using the resin varnish produced in the above-mentioned Production Example, a plurality of resin sheets including resin composition layers having different thicknesses were produced by the following method.
[0541] As a support, a polyethylene terephthalate film ("Lumirror T6AM" manufactured by Toray Industries, Ltd., with a thickness of 38 μm and a softening point of 130°C) was prepared. A resin varnish was uniformly applied to the support using a die coater so that the thickness of the resin composition layer after drying would be 5 μm, 6.5 μm, 8 μm, 10 μm, 15 μm, or 20 μm. The film was then dried at 80°C to 110°C (maximum temperature 110°C) for 7 minutes to form a resin composition layer. Subsequently, a cover film (biaxially oriented polypropylene film, "MA-411" manufactured by Oji Eptex) was placed on the surface of the resin composition layer and laminated at 80°C to produce a three-layer resin sheet consisting of support / resin composition layer / cover film.
[0542] [Measurement of Refractive Index of Cured Material of Resin Composition]
[0543] The refractive index of the cured product of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was measured using a resin sheet by the following method.
[0544] The cover film was peeled off from the resin sheet having a resin composition layer with a thickness of 6.5 μm. Thereafter, the resin sheet was laminated on a silicon wafer at 80°C, and the support was peeled off to form a resin composition layer with a thickness of 6.5 μm on the silicon wafer. Thereafter, the resin composition layer was exposed using a projection exposure device ("UFX-2240" manufactured by Ushio Electric Co., Ltd.) at an optimum exposure amount of 3000 mJ. After exposure, heating was performed at 90°C for 3 minutes, and then a 23°C and 2.38% by mass tetramethylammonium hydroxide aqueous solution as a developer was sprayed on the resin composition layer at a spray pressure of 0.1 MPa for 30 seconds to perform spray development. After spray development, the resin composition layer was subjected to a 3J / cm 2 The sample was irradiated with ultraviolet light and then heated at 190°C for 90 minutes under a nitrogen atmosphere to obtain a sample formed of a cured product of the resin composition. The refractive index n (1310 nm) of the obtained sample was measured at room temperature and atmospheric pressure using a 1310 nm laser using a 2010M prism coupler (manufactured by Metrikon Corporation).
[0545] [Evaluation of Resolvability of Resin Composition]
[0546] The resolution of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was evaluated by the following method using a resin sheet.
[0547] For the copper layer of the glass epoxy substrate (copper clad laminate) having a copper layer with a thickness of 18 μm, a surface treatment agent (CZ8100, manufactured by MEC) containing an organic acid is used to perform a roughening treatment to prepare a substrate. The covering film is peeled off from the resin sheet prepared in Manufacturing Example 1, and laminated to the previous substrate at 100°C, and the support is peeled off to form a resin composition layer. Thereafter, a projection exposure device ("UFX-2240" manufactured by Ushio Electric Co., Ltd.) is used to expose the entire surface of the resin composition layer with an optimal exposure amount of 3000mJ. After exposure, the resin composition layer is heated at 90°C for 3 minutes, and then a 23°C and 2.38% by mass tetramethylammonium hydroxide aqueous solution as a developer is sprayed at a spray pressure of 0.1MPa for 30 seconds to perform spray development. After development, the resin composition layer is subjected to 3J / cm 2 The copper-clad laminate was irradiated with ultraviolet rays and then subjected to a heat treatment at 190° C. for 90 minutes in a nitrogen atmosphere, thereby forming a lower cladding layer on the copper-clad laminate.
[0548] The cover film was peeled off from the resin sheet with a resin composition layer having a thickness of 10 μm manufactured in each of the above manufacturing examples. A resin sheet was arranged on the lower coating layer in such a manner that the resin composition layer of the resin sheet was in contact with the lower coating layer, and a vacuum laminator ("VP160" manufactured by Nikka Materialus Co., Ltd.) was used for lamination to form a resin composition layer on the lower coating layer. The lamination conditions were set as follows: a vacuum time of 30 seconds, a pressing temperature of 100°C, a pressing pressure of 0.7 MPa, and a pressing time of 30 seconds. Thus, a laminate having a copper-clad laminate, a lower coating layer, and a resin sheet was obtained in sequence. Thereafter, the support was peeled off to expose the resin composition layer.
[0549] The resin composition layer was exposed using a projection exposure device ("UFX-2240" manufactured by Ushio Electric Co., Ltd.) at an optimal exposure dose of 200 mJ to 2000 mJ. The exposure was performed using a quartz glass mask having a first mask pattern with straight lines drawn at an L / S (line / space) of 10 μm / 10 μm, a second mask pattern with straight lines drawn at an L / S (line / space) of 5 μm / 50 μm, and a third mask pattern with straight lines drawn at an L / S (line / space) of 3 μm / 3 μm. After exposure, heating was performed at 90°C for 3 minutes, and then a 2.38% by mass tetramethylammonium hydroxide aqueous solution as a developer was sprayed at a spray pressure of 0.1 MPa for 30 seconds on the resin composition layer for spray development. After spray development, the resin composition layer was subjected to a 3 J / cm 2The wafer was irradiated with ultraviolet light and then heat treated at 190° C. for 90 minutes in a nitrogen atmosphere to obtain a sample having a silicon wafer, a lower cladding layer, and a line layer (a layer formed of a cured product of the resin composition) in this order.
[0550] The obtained sample was observed using a scanning electron microscope (SEM) (magnification of 2000 times) to measure the minimum fine line formation width (the width of the line layer with the smallest width among the formed line layers). The aspect ratio was calculated by dividing the thickness of the line layer by the minimum fine line formation width. If the aspect ratio of all line layers with a line width of less than 10 μm is greater than 1, the resolution is evaluated as "excellent", if the aspect ratio of all line layers with a line width of less than 10 μm is greater than 0.6 and less than 1, the resolution is evaluated as "qualified", and if the aspect ratio of at least one of the line layers with a line width of less than 10 μm is less than 0.6, the resolution is evaluated as "poor". Here, the line width refers to the width of the line layer.
[0551] [Measurement of Elongation at Break of Cured Product of Resin Composition]
[0552] The cover film was peeled off from the resin film with a resin composition layer having a thickness of 15 μm manufactured in the above-mentioned manufacturing example. Thereafter, the resin composition layer was subjected to 1000 mJ of ultraviolet irradiation and heated at 190 ° C and 90 minutes under a nitrogen atmosphere to thermally cure the resin composition layer. Thereafter, the support was peeled off to obtain a sample film formed by a cured product of the resin composition. According to Japanese Industrial Standards (JIS K7127), a TENSILON universal testing machine ("RTC-1250A" manufactured by ORIENTEC) was used to perform a tensile test on the obtained sample film to determine the elongation at break. The greater the elongation at break, the higher the strength of the sample film, and thus, the more excellent the mechanical strength of the cured product.
[0553] "Excellent": Elongation at break is 1% or more.
[0554] “Poor”: Elongation at breaking point is less than 1%.
[0555] [Measurement of absorbance of resin composition solution]
[0556] A solution of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was prepared, and the absorbance of the solution was measured by the following method.
[0557] Specifically, a mixed solvent of MEK and cyclopentanone (MEK:pentanone = 1:1) was mixed with the resin varnish prepared in the manufacturing example to prepare a solution having a resin composition concentration of 20% by mass. This solution was placed in a 1 cm quartz cuvette, and the absorbance (Abs) at a wavelength of 1310 nm was measured using a UV-visible-near-infrared spectrophotometer (V-770, manufactured by Bunko Co., Ltd., Japan).
[0558] [Measurement of Linear Thermal Expansion Coefficient of Cured Product of Resin Composition]
[0559] The linear thermal expansion coefficient of the cured product of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was measured using a resin sheet by the following method.
[0560] That is, the cover film is peeled off from the resin film with a resin composition layer having a thickness of 15 μm manufactured in the manufacturing example. Thereafter, the resin composition layer is irradiated with 1000 mJ of ultraviolet light and heated at 190 ° C and 90 minutes under a nitrogen atmosphere to thermally cure the resin composition layer. Thereafter, the support is peeled off to obtain a cured product for evaluation. The cured product for evaluation is cut to obtain a test piece with a width of 5 mm and a length of 15 mm. A thermomechanical analysis device (Rigaku Corporation, Thermo Plus, TMA8310) is used to perform a thermomechanical analysis of the test piece using a tensile load method. In the aforementioned thermomechanical analysis, after the test piece is mounted on the aforementioned device, it is continuously measured twice under the measurement conditions of a load of 1 g and a heating rate of 5 ° C / min. The linear thermal expansion coefficient of the cured product is determined by calculating the average linear thermal expansion coefficient (ppm) from 25 ° C to 150 ° C in the second measurement.
[0561] [Measurement of Surface Roughness of Cured Product of Resin Composition]
[0562] The surface roughness of the cured product of the resin composition contained in the resin varnish produced in the above-mentioned Production Example was measured using a resin sheet by the following method.
[0563] That is, the cover film is peeled off from the resin film with a resin composition layer having a thickness of 15 μm manufactured in the manufacturing example. Thereafter, a resin sheet is arranged on a 4-inch silicon wafer in such a way that the resin composition layer is in contact with the silicon wafer, and laminated using a vacuum laminator ("VP160" manufactured by Nikka Materialus Co., Ltd.). The lamination conditions are as follows: vacuuming time is 30 seconds, pressing temperature is 100 ° C, pressing pressure is 0.7 MPa, and pressing time is 30 seconds. Thereafter, the support is peeled off, and exposure is implemented with 3000 mJ of ultraviolet rays using a projection exposure device ("UFX-2240" manufactured by Ushio Electric Co., Ltd.). After exposure, after heating at 90 ° C and 3 minutes, a 23 ° C and 2.38 mass % tetramethylammonium hydroxide aqueous solution as a developer is sprayed at a spray pressure of 0.1 MPa for 30 seconds for the resin composition layer, and spray development is performed. After spray development, the film was placed in a clean oven and heated from room temperature to 190°C. After reaching 190°C, it was heated for 90 minutes under a nitrogen atmosphere to cure the resin composition layer. The surface condition of the cured product was evaluated using a non-contact interference microscope (manufactured by WYKO Bruker AXS), and the arithmetic mean roughness Ra was measured as the surface roughness of the cured product.
[0564] [Composition and physical properties of resin composition]
[0565] The compositions and physical properties of the resin compositions produced in the above-mentioned production examples are shown in the following Tables 1 and 2. In the following Tables 1 and 2, the amounts of the reagents are expressed in parts by mass. In the following Tables 1 and 2, the abbreviations have the following meanings.
[0566] F content: the amount of fluorine atoms (mass %) relative to 100% by mass of the nonvolatile components of the resin composition.
[0567] n(1310 nm): The refractive index of the cured product of the resin composition at a wavelength of 1310 nm was measured.
[0568] Abs: The absorbance of the resin composition solution at a wavelength of 1310 nm was measured.
[0569] CTE: Coefficient of linear thermal expansion of a cured product of a resin composition.
[0570] [Table 1]
[0571] [Table 1. Composition and physical properties of the resin compositions of Production Examples 1 to 7]
[0572] Manufacturing Example 1 2 3 4 5 6 7 (A)TR4020G 10 10 9.9 9.3 9 8 2 (A)BisP-E 2 2 2 2 2 2 2 (A)Bis-AF 0.1 0.3 1 2 8 (A)Malkank-M (A) Synthesis Example 1 1 1 1 1 1 1 (A)J-DPP-85 (A)SPDI (A)TBIS-RX (B)PAG-103 0.2 0.2 0.2 0.2 0.2 0.2 0.2 (C)MW-390 4 4 4 4 4 4 4 (D)CB-3098 1 1 1 1 1 1 1 (E) Trioctylamine 0.04 0.04 0.04 0.04 0.04 0.04 0.04 (F)ZCR-1797H (F)FA-324A (F)NC-3000H (F)Omnirad819 (G)MEK 7 7 7 7 7 (G) Cyclohexanone 5 5 5 5 5 5 5 (G)PGMEAc 1 8 1 8 1 1 1 Total solid content 18.24 18.24 18.24 17.84 18.24 17.24 18.24 Varnish total 31.24 31.24 31.24 30.84 31.24 30.24 31.24 F content 0.000 0.000 0.186 0.571 1.860 3.936 14.881 n(1310nm) 1.6010 1.6010 1.6005 1.5995 1.5960 1.5910 1.5600 Abs@1310nm 0.0100 0.0120 0.0080 0.0080 0.0140 0.0070 0.0100 Discrimination excellent excellent excellent excellent excellent excellent qualified CTE (ppm / ℃) 60 60 60.3 61.2 62.2 63.4 70.3 Elongation at breaking point excellent excellent excellent excellent excellent excellent excellent Surface roughness (nm) 50 50 50 50 50 50 50
[0573] [Table 2]
[0574] [Table 2. Composition and physical properties of the resin compositions of Production Examples 8 to 13]
[0575] Manufacturing Example 8 9 10 11 12 13 (A)TR4020G 7 10 (A)BisP-E 2 2 (A)Bis-AF (A)Malkank-M 12 12 12 (A) Synthesis Example 1 1 1 (A)J-DPP-85 3 (A)SPDI 3 3 (A)TBIS-RX 3 (B)PAG-103 0.2 0.2 0.2 0.2 0.2 (C)MW-390 4 8 4 5 6 (D)CB-3098 1 1 1 (E) Trioctylamine 0.04 0.04 (F)ZCR-1797H 30 (F)FA-324A <![CDATA
[15] ]> (F)NC-3000H 5 (F)omnirad819 1 (G)MEK 7 7 (G) Cyclohexanone 5 5 (G)PGMEAc 1 1 1 1 1 10 Total solid content 18.24 22.24 20.20 20.20 21.20 42.00 Varnish total 31.24 35.24 21.20 21.20 22.20 61.00 F content 0.000 0.000 0.000 0.000 0.000 0.000 n(1310nm) 1.6118 1.5700 1.5780 1.5620 1.5580 1.5800 Abs@1310nm 0.0100 0.0100 0.0044 0.0044 0.0044 0.0 170 Discrimination excellent inferior excellent excellent excellent inferior CTE (ppm / ℃) 65.2 65.4 70.3 67.8 72.1 85.4 Elongation at breaking point excellent inferior excellent excellent excellent excellent Surface roughness (nm) 50 50 50 50 50 50
[0576] [Example 1]
[0577] (1-1. Formation of Lower Cladding Layer)
[0578] The cover film was peeled off from the resin sheet having a resin composition layer having a thickness of 10 μm manufactured in Manufacturing Example 5. A resin sheet was arranged on a 4-inch silicon wafer in such a manner that the resin composition layer was in contact with the silicon wafer, and laminated using a vacuum laminator ("VP160" manufactured by Nitsuko-Materials Co., Ltd.). The lamination conditions were as follows: vacuuming time of 30 seconds, pressing temperature of 100° C., pressing pressure of 0.7 MPa, and pressing time of 30 seconds. Thereafter, the support was peeled off to obtain an intermediate laminate I having a silicon wafer and a resin composition layer.
[0579] The resin composition layer of intermediate laminate I was exposed to 3000 mJ of ultraviolet light using a projection exposure apparatus (UFX-2240, manufactured by Ushizai Electric Co., Ltd.). After exposure, intermediate laminate I was placed in a clean oven and heated from room temperature to 190°C. After reaching 190°C, it was heated for 90 minutes under a nitrogen atmosphere to cure the resin composition layer. The curing of the resin composition layer formed a lower cladding layer, resulting in intermediate laminate II comprising a silicon wafer and a lower cladding layer.
[0580] (1-2. Formation of Core Layer)
[0581] The cover film was peeled off from the resin sheet having a 5 μm thick resin composition layer produced in Production Example 1. A resin sheet was placed on the surface of the lower cladding layer of the intermediate laminate II so that the resin composition layer was in contact with the lower cladding layer, and laminated using a vacuum laminator ("VP160" manufactured by Niccol Materials). The lamination conditions were as follows: vacuuming time of 30 seconds, pressing temperature of 100°C, pressing pressure of 0.7 MPa, and pressing time of 30 seconds. Thereafter, the support was peeled off to obtain an intermediate laminate III having a silicon wafer, a lower cladding layer (base cladding layer), and a resin composition layer in that order.
[0582] The resin composition layer of the intermediate laminate III was exposed to ultraviolet light using a projection exposure apparatus (UFX-2240, manufactured by Ushio Electric Co., Ltd.) at an optimal exposure dose of 200 to 2000 mJ. Exposure was performed using a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at a line / space ratio of 5 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at a line / space ratio of 5 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at a line / space ratio of 5 μm / 100 μm. The line / space ratio of the quartz glass mask corresponds to the width of the core layer, and the space corresponds to the spacing between the core layers. After exposure, the resin composition layer was heated at 90°C for 3 minutes. A 2.38% by mass tetramethylammonium hydroxide aqueous solution at 23°C was then sprayed onto the resin composition layer at a spray pressure of 0.1 MPa for 30 seconds for spray development. After spray development, the intermediate laminate III was placed in a clean oven and heated from room temperature to 190°C. Once at 190°C, the resin composition layer was heated for 90 minutes under a nitrogen atmosphere to cure. Curing of the resin composition layer formed a core layer, resulting in an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0583] (1-3. Formation of Upper Cladding Layer)
[0584] The cover film was peeled off from the resin sheet having a 20 μm thick resin composition layer produced in Production Example 5. The resin sheet was placed on the core layer of intermediate laminate IV so that the resin composition layer was in contact with the core layer, and laminated using a vacuum laminator ("VP160" manufactured by Niccol Materials). Lamination conditions were as follows: vacuum time of 30 seconds, pressing temperature of 100°C, pressing pressure of 0.7 MPa, and pressing time of 30 seconds. The support was then peeled off, yielding intermediate laminate V comprising, in this order, a silicon wafer, a lower cladding layer, a core layer, and a resin composition layer.
[0585] The resin composition layer of the intermediate laminate V was exposed to 3000 mJ of ultraviolet light using a projection exposure apparatus (UFX-2240, manufactured by Ushio Electric Co., Ltd.). After exposure, the intermediate laminate V was placed in a clean oven and heated from room temperature to 190°C. After reaching 190°C, it was heated for 90 minutes under a nitrogen atmosphere to cure the resin composition layer. The curing of the resin composition layer formed an upper cladding layer, resulting in a sample laminate comprising a silicon wafer, a lower cladding layer, a core layer, and an upper cladding layer in this order.
[0586] In this sample stack, the combination of the lower and upper cladding layers constitutes the cladding layer. Thus, an optical waveguide comprising the cladding layer and the core layer located within it can be obtained. Furthermore, in this sample stack, the core layer has linear patterns with lengths of 1 cm, 2 cm, and 3 cm, corresponding to the mask pattern of the quartz glass mask. The width (line width) and spacing (spaces) of the core layer contained in these patterns match the width (line width) and spacing (spaces) of the mask pattern.
[0587] [Example 2]
[0588] (2-1. Formation of Lower Cladding Layer)
[0589] An intermediate laminate II including a silicon wafer and a lower cladding layer was manufactured by the same method as step (1-1) of Example 1 except that the resin sheet having a 10 μm thick resin composition layer manufactured in Manufacturing Example 3 was used as the resin sheet for forming the lower cladding layer.
[0590] (2-2. Formation of Core Layer)
[0591] As a resin sheet for forming the core layer, the resin sheet having a resin composition layer with a thickness of 5 μm manufactured in Manufacturing Example 8 is used. In addition, a core layer is formed on the lower cladding layer of the intermediate stack II obtained in the aforementioned step (2-1) by the same method as the step (1-2) of Example 1, thereby obtaining an intermediate stack IV having a silicon wafer, a lower cladding layer and a core layer in sequence.
[0592] (2-3. Formation of Upper Cladding Layer)
[0593] As a resin sheet for forming the upper cladding layer, the resin sheet having a resin composition layer with a thickness of 20 μm manufactured in Manufacturing Example 3 was used. In addition, an upper cladding layer was formed on the core layer of the aforementioned intermediate stack IV obtained in the aforementioned step (2-2) by the same method as the step (1-3) of Example 1, thereby manufacturing a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0594] [Example 3]
[0595] (3-1. Formation of Lower Cladding Layer)
[0596] By the same method as step (1-1) of Example 1, an intermediate laminate II including a silicon wafer and a lower cladding layer was produced.
[0597] (3-2. Formation of Core Layer)
[0598] The resin varnish produced in Production Example 2 was applied to the surface of the lower cladding layer of the intermediate laminate II obtained in step (3-1) using a spin coater ("MS-B100" manufactured by Mikasa Corporation). The varnish was then dried by heating at 110°C for 3 minutes on a hot plate to form a 3 μm thick resin composition layer. This yielded an intermediate laminate III comprising a silicon wafer, a lower cladding layer (base cladding layer), and a resin composition layer in this order.
[0599] The resin composition layer of the intermediate laminate III was exposed using a projection exposure apparatus (UFX-2240, manufactured by Ushio Electric Co., Ltd.) at an optimal exposure dose of 200 to 2000 mJ. Exposure was performed using a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at a line / space ratio of 3 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at a line / space ratio of 3 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at a line / space ratio of 3 μm / 100 μm. After exposure, the resin composition layer was heated at 90°C for 3 minutes. A 2.38% by mass aqueous solution of tetramethylammonium hydroxide at 23°C was then sprayed onto the resin composition layer at a spray pressure of 0.1 MPa for 30 seconds to perform spray development. After spray development, the intermediate laminate III was placed in a clean oven and heated from room temperature to 190°C. After reaching 190°C, it was heated for 90 minutes under a nitrogen atmosphere to cure the resin composition layer. Curing of the resin composition layer formed a core layer, resulting in an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0600] (3-3. Formation of Upper Cladding Layer)
[0601] By the same method as step (1-3) of Example 1, an upper cladding layer is formed on the core layer of the intermediate stack IV obtained in the aforementioned step (3-2), thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0602] [Example 4]
[0603] (4-1. Formation of Lower Cladding Layer)
[0604] An intermediate laminate II including a silicon wafer and a lower cladding layer was manufactured by the same method as step (1-1) of Example 1 except that the resin sheet having a 10 μm thick resin composition layer manufactured in Manufacturing Example 6 was used as the resin sheet for forming the lower cladding layer.
[0605] (4-2. Formation of Core Layer)
[0606] By the same method as step (3-2) of Example 3, a core layer was formed on the lower cladding layer of the intermediate laminate II obtained in the above step (4-1) to obtain an intermediate laminate IV having a silicon wafer, a lower cladding layer and a core layer in this order.
[0607] (4-3. Formation of Upper Cladding Layer)
[0608] As a resin sheet for forming the upper cladding layer, the resin sheet having a resin composition layer with a thickness of 20 μm manufactured in Manufacturing Example 6 was used. In addition, an upper cladding layer was formed on the core layer of the intermediate stack IV obtained in the aforementioned step (4-2) by the same method as in step (1-3) of Example 1, thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0609] [Example 5]
[0610] (5-1. Formation of Lower Cladding Layer)
[0611] An intermediate laminate II including a silicon wafer and a lower cladding layer was produced by the same method as in step (1-1) of Example 1 except that the resin varnish produced in Production Example 4 was used to form the resin composition layer by the following method.
[0612] The resin composition layer was formed using the resin varnish produced in Production Example 4 by the following method. Specifically, the resin varnish produced in Production Example 4 was applied onto a 4-inch silicon wafer using a spin coater ("MS-B100" manufactured by Mikasa Corporation), and then dried by heating at 110°C for 3 minutes on a hot plate to form a resin composition layer having a thickness of 10 μm.
[0613] (5-2. Formation of Core Layer)
[0614] The resin sheet for forming the core layer was the resin sheet having an 8 μm thick resin composition layer produced in Production Example 1. The quartz glass mask was replaced with a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at an L / S (line / space) ratio of 8 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at an L / S (line / space) ratio of 8 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at an L / S (line / space) ratio of 8 μm / 100 μm. With the exception of the above, a core layer was formed on the surface of the lower cladding layer of the intermediate laminate II obtained in the aforementioned step (5-1) by the same method as in step (1-2) of Example 1, yielding an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0615] (5-3. Formation of Upper Cladding Layer)
[0616] Using the resin varnish produced in Manufacturing Example 4, a resin composition layer was formed by the following method. In addition, an upper cladding layer was formed on the core layer of the intermediate stack IV obtained in the aforementioned step (5-2) by the same method as step (1-3) of Example 1, thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0617] The resin composition layer was formed using the resin varnish produced in Production Example 4 by the following method. Specifically, the resin varnish produced in Production Example 4 was applied to the surface of the core layer of the intermediate laminate IV using a spin coater ("MS-B100" manufactured by Mikasa Corporation), and then dried by heating at 110°C for 3 minutes on a hot plate to form a resin composition layer having a thickness of 20 μm.
[0618] [Example 6]
[0619] (6-1. Formation of Lower Cladding Layer)
[0620] By the same method as step (1-1) of Example 1, an intermediate laminate II including a silicon wafer and a lower cladding layer was produced.
[0621] (6-2. Formation of Core Layer)
[0622] The coating thickness of the resin varnish was changed to 5 μm, and the thickness of the core layer was changed to 5 μm. Furthermore, the quartz glass mask was replaced with a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at an L / S (line / space) ratio of 8 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at an L / S (line / space) ratio of 8 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at an L / S (line / space) ratio of 8 μm / 100 μm. Except for the above, a core layer was formed on the surface of the lower cladding layer of the intermediate laminate II obtained in the aforementioned step (6-1) by the same method as in step (3-2) of Example 3, thereby obtaining an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0623] (6-3. Formation of Upper Cladding Layer)
[0624] By the same method as step (1-3) of Example 1, an upper cladding layer is formed on the core layer of the intermediate stack IV obtained in the aforementioned step (6-2), thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0625] [Example 7]
[0626] (7-1. Formation of Lower Cladding Layer)
[0627] By the same method as step (1-1) of Example 1, an intermediate laminate II including a silicon wafer and a lower cladding layer was produced.
[0628] (7-2. Formation of Core Layer)
[0629] The coating thickness of the resin varnish was changed to 3 μm, and the thickness of the core layer was changed to 3 μm. Furthermore, the quartz glass mask was replaced with a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at an L / S (line / space) ratio of 4.5 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at an L / S (line / space) ratio of 4.5 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at an L / S (line / space) ratio of 4.5 μm / 100 μm. Except for the above, a core layer was formed on the surface of the lower cladding layer of the intermediate laminate II obtained in the aforementioned step (7-1) by the same method as in step (3-2) of Example 3, thereby obtaining an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0630] (7-3. Formation of Upper Cladding Layer)
[0631] By the same method as step (1-3) of Example 1, an upper cladding layer is formed on the core layer of the intermediate stack IV obtained in the aforementioned step (7-2), thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0632] [Example 8]
[0633] (8-1. Formation of Lower Cladding Layer)
[0634] An intermediate laminate II including a silicon wafer and a lower cladding layer was manufactured by the same method as step (1-1) of Example 1 except that the resin sheet having a 10 μm thick resin composition layer manufactured in Manufacturing Example 6 was used as the resin sheet for forming the lower cladding layer.
[0635] (8-2. Formation of Core Layer)
[0636] The coating thickness of the resin varnish was changed to 3 μm, and the thickness of the core layer was changed to 3 μm. Furthermore, the quartz glass mask was replaced with a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at an L / S (line / space) ratio of 4.5 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at an L / S (line / space) ratio of 4.5 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at an L / S (line / space) ratio of 4.5 μm / 100 μm. Except for the above, a core layer was formed on the surface of the lower cladding layer of the intermediate laminate II obtained in the above step (8-1) by the same method as step (3-2) of Example 3, thereby obtaining an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0637] (8-3. Formation of Upper Cladding Layer)
[0638] As a resin sheet for forming the upper cladding layer, the resin sheet having a resin composition layer with a thickness of 20 μm manufactured in Manufacturing Example 6 was used. In addition, an upper cladding layer was formed on the core layer of the intermediate stack IV obtained in the aforementioned step (8-2) by the same method as step (1-3) of Example 1, thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0639] [Example 9]
[0640] (9-1. Formation of Lower Cladding Layer)
[0641] By the same method as step (1-1) of Example 1, an intermediate laminate II including a silicon wafer and a lower cladding layer was produced.
[0642] (9-2. Formation of Core Layer)
[0643] As the resin sheet for forming the core layer, the resin sheet having a 15 μm thick resin composition layer produced in Production Example 1 was used. Furthermore, the quartz glass mask was replaced with a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at an L / S (line / space) ratio of 15 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at an L / S (line / space) ratio of 15 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at an L / S (line / space) ratio of 15 μm / 100 μm. Except for the above, a core layer was formed on the surface of the lower cladding layer of the intermediate laminate II obtained in the aforementioned step (9-1) by the same method as in step (1-2) of Example 1, thereby obtaining an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0644] (9-3. Formation of Upper Cladding Layer)
[0645] By the same method as step (1-3) of Example 1, an upper cladding layer is formed on the core layer of the intermediate stack IV obtained in the aforementioned step (9-2), thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0646] [Example 10]
[0647] (10-1. Formation of Lower Cladding Layer)
[0648] An intermediate laminate II including a silicon wafer and a lower cladding layer was produced by the same method as step (1-1) of Example 1 except that the resin sheet having a 10 μm thick resin composition layer produced in Production Example 12 was used as the resin sheet for forming the lower cladding layer.
[0649] (10-2. Formation of Core Layer)
[0650] As a resin sheet for forming the core layer, the resin sheet having a resin composition layer with a thickness of 5 μm manufactured in Manufacturing Example 10 is used. In addition, a core layer is formed on the surface of the lower cladding layer of the intermediate stack II obtained in the aforementioned step (10-1) by the same method as the step (1-2) of Example 1, thereby obtaining an intermediate stack IV having a silicon wafer, a lower cladding layer and a core layer in sequence.
[0651] (10-3. Formation of Upper Cladding Layer)
[0652] As a resin sheet for forming the upper cladding layer, the resin sheet having a resin composition layer with a thickness of 20 μm manufactured in Manufacturing Example 12 was used. In addition, an upper cladding layer was formed on the core layer of the intermediate stack IV obtained in the aforementioned step (10-2) by the same method as in step (1-3) of Example 1, thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0653] [Example 11]
[0654] (11-1. Formation of Lower Cladding Layer)
[0655] An intermediate laminate II including a silicon wafer and a lower cladding layer was produced by the same method as step (1-1) of Example 1 except that the resin sheet having a 10 μm thick resin composition layer produced in Production Example 12 was used as the resin sheet for forming the lower cladding layer.
[0656] (11-2. Formation of Core Layer)
[0657] As a resin sheet for forming the core layer, a resin sheet having a resin composition layer with a thickness of 5 μm manufactured in Manufacturing Example 11 is used. In addition, a core layer is formed on the surface of the lower cladding layer of the intermediate stack II obtained in the aforementioned step (11-1) by the same method as the step (1-2) of Example 1, thereby obtaining an intermediate stack IV having a silicon wafer, a lower cladding layer and a core layer in sequence.
[0658] (11-3. Formation of Upper Cladding Layer)
[0659] As a resin sheet for forming the upper cladding layer, the resin sheet having a resin composition layer with a thickness of 20 μm manufactured in Manufacturing Example 12 was used. In addition, an upper cladding layer was formed on the core layer of the intermediate stack IV obtained in the aforementioned step (11-2) by the same method as in step (1-3) of Example 1, thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0660] [Example 12]
[0661] (12-1. Formation of Lower Cladding Layer)
[0662] By the same method as step (1-1) of Example 1, an intermediate laminate II including a silicon wafer and a lower cladding layer was produced.
[0663] (12-2. Formation of Core Layer)
[0664] As a support, a polyethylene terephthalate film ("PTH-25" manufactured by Unichika Co., Ltd., with a thickness of 25 μm) having a rough surface was prepared. The resin varnish manufactured in Manufacturing Example 1 was evenly applied to the rough surface of the support using a die coater so that the thickness of the resin composition layer after drying became 10 μm, and dried at 80°C to 110°C (maximum temperature of 110°C) for 7 minutes to form a resin composition layer. Subsequently, a covering film (biaxially stretched polypropylene film, "MA-411" manufactured by Prince Eptex Co., Ltd.) was placed on the surface of the resin composition layer and laminated at 80°C to manufacture a resin sheet having a three-layer structure of a support / resin composition layer / covering film. The surface of the support side of the resin composition layer of the resin sheet manufactured in this manner is made rougher by being pressed against the rough surface of the support. Therefore, the aforementioned resin sheet is sometimes referred to as a "roughened resin sheet" hereinafter.
[0665] The aforementioned roughened resin sheet was used as the resin sheet for forming the core layer. Furthermore, the quartz glass mask was replaced with a quartz glass mask having a mask pattern capable of drawing multiple straight lines with a length of 1 cm at an L / S (line / space) ratio of 10 μm / 100 μm, a mask pattern capable of drawing multiple straight lines with a length of 2 cm at an L / S (line / space) ratio of 10 μm / 100 μm, and a mask pattern capable of drawing multiple straight lines with a length of 3 cm at an L / S (line / space) ratio of 10 μm / 100 μm. With the exception of the above, a core layer was formed on the surface of the lower cladding layer of the intermediate laminate II obtained in the aforementioned step (12-1) by the same method as in step (1-2) of Example 1, yielding an intermediate laminate IV comprising a silicon wafer, a lower cladding layer, and a core layer in this order.
[0666] (12-3. Formation of Upper Cladding Layer)
[0667] By the same method as step (1-3) of Example 1, an upper cladding layer is formed on the core layer of the intermediate stack IV obtained in the aforementioned step (12-2), thereby obtaining a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0668] [Example 13]
[0669] In the formation of the lower cladding layer, the formation of the core layer, and the formation of the upper cladding layer, when the resin composition layer is cured in a clean oven, the heat treatment conditions are changed as described below. That is, the temperature is raised from room temperature to 100°C, and after reaching 100°C, the temperature is heated for 60 minutes, then raised to 190°C, and after reaching 190°C, the temperature is heated for 90 minutes under a nitrogen atmosphere to cure the resin composition layer. Except for the above matters, the same operation as in Example 12 is performed to obtain a sample stack having a silicon wafer, a lower cladding layer, a core layer, and an upper cladding layer in sequence. In this Example 13, by changing the curing conditions of the resin composition based on the heat treatment, the shape of the rough surface of the support is more clearly reflected on the surface of the core layer. Therefore, the surface roughness of the core layer is greater than that of Example 12.
[0670] [Comparative Example 1]
[0671] (C1-1. Formation of Lower Cladding Layer)
[0672] An intermediate laminate II including a silicon wafer and a lower cladding layer was manufactured by the same method as step (1-1) of Example 1 except that the resin sheet having a 10 μm thick resin composition layer manufactured in Manufacturing Example 3 was used as the resin sheet for forming the lower cladding layer.
[0673] (C1-2. Formation of Core Layer)
[0674] By the same method as step (1-2) of Example 1, a core layer was formed on the lower cladding layer of the intermediate laminate II obtained in the above step (C2-1) to obtain an intermediate laminate IV having a silicon wafer, a lower cladding layer and a core layer in this order.
[0675] (C1-3. Formation of Upper Cladding Layer)
[0676] As a resin sheet for forming the upper cladding layer, the resin sheet having a resin composition layer with a thickness of 20 μm manufactured in Manufacturing Example 3 was used. In addition, an upper cladding layer was formed on the core layer of the aforementioned intermediate stack IV obtained in the aforementioned step (C1-2) by the same method as step (1-3) of Example 1, thereby manufacturing a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0677] [Comparative Example 2]
[0678] (C2-1. Formation of Lower Cladding Layer)
[0679] An intermediate laminate II including a silicon wafer and a lower cladding layer was manufactured by the same method as step (1-1) of Example 1 except that the resin sheet having a 10 μm thick resin composition layer manufactured in Manufacturing Example 7 was used as the resin sheet for forming the lower cladding layer.
[0680] (C2-2. Formation of Core Layer)
[0681] As a resin sheet for forming the core layer, a resin sheet having a resin composition layer with a thickness of 5 μm manufactured in Manufacturing Example 8 is used. In addition, a core layer is formed on the lower cladding layer of the intermediate stack II obtained in the aforementioned step (C2-1) by the same method as step (1-2) of Example 1, thereby obtaining an intermediate stack IV having a silicon wafer, a lower cladding layer and a core layer in sequence.
[0682] (C2-3. Formation of Upper Cladding Layer)
[0683] As a resin sheet for forming the upper cladding layer, the resin sheet having a resin composition layer with a thickness of 20 μm manufactured in Manufacturing Example 7 was used. In addition, an upper cladding layer was formed on the core layer of the aforementioned intermediate stack IV obtained in the aforementioned step (C2-2) by the same method as step (1-3) of Example 1, thereby manufacturing a sample stack having a silicon wafer, a lower cladding layer, a core layer and an upper cladding layer in sequence.
[0684] [Comparative Example 3]
[0685] As the resin sheet for forming the lower cladding layer, the resin sheet having a 10 μm thick resin composition layer produced in Production Example 13 was used. Furthermore, as the resin sheet for forming the upper cladding layer, the resin sheet having a 20 μm thick resin composition layer produced in Production Example 13 was used. A sample laminate comprising a silicon wafer, a lower cladding layer, a core layer, and an upper cladding layer in this order was produced by the same method as in Example 1, except for the above-mentioned matters.
[0686] [Measurement of Surface Roughness of Core Layer]
[0687] In the above-described Examples and Comparative Examples, the arithmetic mean roughness (Ra) of the core layer's surface roughness was measured after forming the core layer and before forming the upper cladding layer. This measurement was performed using a surface roughness meter (WYKONT3300, manufactured by Vicontest Corporation) in VSI mode with a 50x lens, and a measurement range of 121 μm x 92 μm. The Ra value was calculated from the obtained values. For each sample, the average value of 10 randomly selected points was calculated.
[0688] [Evaluation of optical waveguide]
[0689] (Measurement of Light Transmission Loss in Calibration Optical Systems)
[0690] The transmission loss of an optical system constructed by removing the test substrate and focusing module from the optical system for measuring transmission loss of the test substrate described later was measured. Specifically, a light source (a 1310 nm light source, "LPSC-1310-FC" manufactured by THORLABS) and a light receiver (an optical power meter "N7742" manufactured by Keysite) were connected via an optical fiber (incident fiber) on a vibration-isolating table covered with a black curtain, creating a calibration optical system. The light source was illuminated, and the intensity of the light entering the light receiver was measured using the light receiver to measure the loss of the calibration optical system.
[0691] (Preparation of test substrate)
[0692] From the sample laminates produced in Examples and Comparative Examples, the core layer and the surrounding cladding layers were cut out at the portion where the core layer was formed, thereby obtaining test substrates having an optical transmission path.
[0693] (Measurement of optical transmission loss)
[0694] A test substrate is set up on a vibration removal table covered with a black curtain. One end (incident end) of the optical waveguide of the test substrate is connected to a focusing module (with an aperture of 0.18), and then the focusing module is connected to a light source (1310nm light source, "LPSC-1310-FC" manufactured by THORLABS) via an optical fiber (incident fiber). In addition, the other end (emission end) of the optical waveguide of the test substrate is connected to another focusing module (with an aperture of 0.18), and then the focusing module is connected to an optical receiver (optical power meter "N7742" manufactured by Keysite Corporation) via an optical fiber (emission fiber). Through the above operation, an optical system is obtained in which the light emitted by the light source passes through the optical fiber (incident fiber), focusing module, optical waveguide, focusing module and optical fiber (emission fiber) in sequence, and then enters the optical receiver. Hereinafter, this optical system may sometimes be referred to as the sample optical system. The light source is made to emit light, and the intensity of the light entering the optical receiver is measured using the optical receiver to measure the loss of the sample optical system.
[0695] The loss of the optical system for correction is subtracted from the loss of the sample optical system to determine the loss of the optical waveguide included in the test substrate.
[0696] (Measurement of Transmission Loss (dB / cm) of an Optical Waveguide)
[0697] The optical waveguide loss was measured for each of the 1 cm, 2 cm, and 3 cm optical waveguide lengths. The measurement results were plotted in a coordinate system with the optical waveguide length on the horizontal axis and the optical waveguide loss on the vertical axis, yielding the coordinates of three points representing the measurement results. An approximate straight line was calculated for these three points using the least squares method, and the slope of this approximate straight line was determined as the optical waveguide loss per unit distance (transmission loss).
[0698] (Confirmation of mode)
[0699] Remove the light receiver and replace it with an infrared camera (InGaAs camera with a 100x objective lens). Light the light source and use the infrared camera to capture the light emitted from the end of the optical fiber (output fiber). If only a single perfectly circular edge of light is observed, it is determined to be single-mode. If multiple edges are observed, it is determined to be multimode.
[0700] (Appearance observation after reflow)
[0701] Using a reflow apparatus ("HAS6116" manufactured by Antrum), the test substrates were subjected to five heat treatments (reflow temperature profile based on IPC / JEDEC J-STD-020C). The test substrates were observed after treatment. If there were no voids or peeling within the substrate, the reflow resistance was judged as "Excellent." Otherwise, if there were voids or peeling within the substrate, the reflow resistance was judged as "Poor."
[0702] [result]
[0703] The results of the above examples and comparative examples are shown in the following Tables 3 and 4. In the following Tables 3 and 4, the abbreviations have the following meanings.
[0704] NA: Number of openings of the optical waveguide
[0705] ΔCTE: The difference between the linear thermal expansion coefficient of the cured product of the core resin composition and the linear thermal expansion coefficient of the cured product of the covering resin composition.
[0706] In the Mode column it is written as "S": Single Mode.
[0707] In the Mode column it is written as "M": Multimode.
[0708] [Table 3]
[0709] [Table 3. Results of Examples 1 to 8]
[0710]
[0711] [Table 4]
[0712] [Table 4. Results of Examples 9 to 13 and Comparative Examples 1 to 3]
[0713]
[0714] [Research]
[0715] Single mode was confirmed in Examples 1 and 3 to 7, which have small core layers and small numerical apertures. It should be noted that, separately from the above examples and comparative examples, optical waveguides with numerical apertures less than 0.05 were produced. However, due to process variations, the refractive index within the waveguides changed, and light guidance could not be confirmed.
[0716] In Comparative Examples 1 and 2 where the numerical aperture NA was 0.4 or more, the transmission loss became significant and there was much noise, so that the transmission loss value could not be measured.
[0717] Description of Reference Numerals
[0718] 10 Optical waveguide
[0719] 100 core layer
[0720] 110 Second composition layer
[0721] 111 Exposure Department
[0722] 112 Non-exposure Department
[0723] 200 cladding
[0724] 210 first composition layer
[0725] 220 Cured first composition layer (lower coating layer)
[0726] 230 Third Composition Layer
[0727] 240 Cured third composition layer (upper coating layer)
[0728] 300 base material
[0729] 400 Mask
[0730] 410 light-transmitting part
[0731] 420 shading part
Claims
1. A photosensitive resin composition kit comprising a core resin composition and a coating resin composition, The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator and (C) a crosslinking agent, The coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator and (c) a crosslinking agent. The opening number NA shown in the following formula (1) is greater than 0.05 and less than 0.4, [Mathematical formula 1] In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad It represents the refractive index of the cured product of the coating resin composition.
2. The photosensitive resin composition kit according to claim 1, wherein (C) The cross-linking agent is an amino resin.
3. The photosensitive resin composition kit according to claim 1, wherein The core resin composition contains (D) a polymer having a weight average molecular weight of 2500 or more.
4. The photosensitive resin composition kit according to claim 1, wherein The core resin composition contains (E) a compound represented by the following formula (E-1), [Chemistry 1] In formula (E-1), R e1 , R e2 and R e3 Each independently represents a hydrogen atom or a hydrocarbon group, R e1 With R e2 They are optionally bonded to form a ring. 5 . The photosensitive resin composition kit according to claim 1 , which is a photosensitive resin composition kit for producing an optical waveguide. 6 . The photosensitive resin composition kit according to claim 1 , which is a photosensitive resin composition kit for producing an optical waveguide capable of transmitting light having a wavelength of 1300 nm to 1320 nm. 7 . The photosensitive resin composition kit according to claim 1 , which is a photosensitive resin composition kit for producing a single-mode optical waveguide.
8. An optical waveguide having a core layer and a cladding layer, The core layer comprises a cured product of a core resin composition, wherein the core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent. The coating layer comprises a cured product of a coating resin composition, wherein the coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent. The opening number NA shown in the following formula (1) is greater than 0.05 and less than 0.4, [Mathematical formula 2] In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad It represents the refractive index of the cured product of the coating resin composition.
9. The optical waveguide according to claim 8, which is capable of transmitting light having a wavelength of 1300 nm to 1320 nm.
10. The optical waveguide according to claim 8, which is a single-mode optical waveguide.
11. An optoelectronic hybrid substrate comprising the optical waveguide according to any one of claims 8 to 10.
12. A method for manufacturing an optical waveguide, comprising: A step of forming a first composition layer including a coating resin composition; A step of subjecting the first composition layer to an exposure treatment; a step of curing the first composition layer; forming a second composition layer including a core resin composition on the first composition layer; A step of subjecting the second composition layer to an exposure treatment; A step of developing the second composition layer; a step of curing the second composition layer; forming a third composition layer including a coating resin composition on the second composition layer; a step of subjecting the third composition layer to an exposure treatment; as well as a step of curing the third composition layer, The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator and (C) a crosslinking agent, The coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator and (c) a crosslinking agent. The opening number NA shown in the following formula (1) is greater than 0.05 and less than 0.4, [Mathematical formula 3] In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad It represents the refractive index of the cured product of the coating resin composition.
13. A sheet set comprising a core resin sheet and a covering resin sheet, The core resin sheet comprises a core resin composition layer including a core resin composition, wherein the core resin composition includes (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent. The coating resin sheet comprises a coating resin composition layer including a coating resin composition, wherein the coating resin composition includes (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent. The opening number NA shown in the following formula (1) is greater than 0.05 and less than 0.4, [Formula 4] In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad It represents the refractive index of the cured product of the coating resin composition.
14. A core resin composition for forming a core layer in a coating layer, wherein the coating layer comprises a cured product of the coating resin composition, wherein the coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator, and (c) a crosslinking agent, The core resin composition comprises (A) a phenolic resin, (B) a photoacid generator and (C) a crosslinking agent, The opening number NA shown in the following formula (1) is greater than 0.05 and less than 0.4, [Formula 5] In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad It represents the refractive index of the cured product of the coating resin composition. 15 . A resin sheet comprising a resin composition layer comprising the core resin composition according to claim 14 .
16. A coating resin composition for forming a coating layer covering a core layer, wherein the core layer comprises a cured product of the core resin composition, wherein the core resin composition comprises (A) a phenolic resin, (B) a photoacid generator, and (C) a crosslinking agent, The coating resin composition comprises (a) a phenolic resin, (b) a photoacid generator and (c) a crosslinking agent. The opening number NA shown in the following formula (1) is greater than 0.05 and less than 0.4, [Mathematical formula 6] In formula (1), n core represents the refractive index of the cured product of the core resin composition, n clad It represents the refractive index of the cured product of the coating resin composition. 17 . A resin sheet comprising a resin composition layer comprising the coating resin composition according to claim 16 .
Citation Information
Patent Citations
Silicone-containing polyimide resin, silicone-containing polyamic acid and their production
JP2000319386A
Polyimidesilicone resin, solution composition thereof, and polyimidesilicone resin coating film
JP2002012667A
Thermosetting resin composition containing modified polyimide resin
JP2006037083A
Photocurable thermosetting resin composition for forming optical waveguide, and cured product thereof and optical waveguide, and optoelectronic hybrid substrate, waveguide-type light splitter, and optical module including optical waveguide
JP2019211540A