Preparation method of adsorbent and method for adsorbing and removing chloride ions in water
The adsorbent is prepared by roasting and modifying magnesium-aluminum layered hydroxide, which solves the problems of high cost, low efficiency and pollution of chloride ion removal in water in the existing technology, and achieves efficient and environmentally friendly chloride ion removal effect and adsorbent quality. Cycle regeneration.
Patent Information
- Application Number
- CN202410741825.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for removing chloride ions from water are high in cost, low in efficiency, and prone to pollution. In particular, precipitation methods and ion exchange methods have limited chloride ion removal effects and high equipment investment, accompanied by secondary pollution problems.
Using magnesium-aluminum layered hydroxide as the adsorbent, a mixed metal salt solution containing magnesium and aluminum is mixed with an alkali solution, left to stand for aging, and then roasted and modified to prepare magnesium with rich pore structure and high specific surface area. Aluminum oxide adsorbent is used to efficiently adsorb chloride ions in water, and the adsorbent can be recycled through roasting and regeneration.
It achieves efficient removal of chloride ions in water, reduces the cost of removing chlorine ions, avoids pollution problems through a simple preparation method and excellent recycling performance, and significantly improves the removal effect of chloride ions.
Smart Images

Figure CN118751192A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water treatment, and in particular to a method for preparing an adsorbent and a method for removing chloride ions in water by adsorption. Background Art
[0002] High concentration of Cl in water - It will seriously harm the natural environment, production and life, and human health, such as: Cl - The high mobility and high stability make it difficult to remove and accumulate. Once it enters the soil, it will cause soil compaction, soil salinization, and reduce the arable land area. - The corrosiveness of the water will eventually lead to the rupture of metal pipes. According to the requirements of the current national relevant industry standards, Cl in water - The content must be controlled below 300 mg / L. Therefore, it is urgent to control the Cl - Remove it to reduce its harm to production and life.
[0003] At present, the commonly used methods for removing chloride ions from wastewater include precipitation, evaporation concentration, ion exchange and membrane separation. Among them, precipitation is to add a certain amount of reagents that can combine with chloride ions to form slightly soluble, insoluble or insoluble compounds to the chlorine-containing wastewater. - It is removed in the form of precipitation. The precipitation method can be divided into ultra-high lime aluminum method, silver method, and bismuth oxide method according to the type of reagent added. The silver method and bismuth oxide method are relatively expensive and have a limited scope of application. The ion exchange method uses the fixed anions and cations in the ion exchange resin to exchange with the ions in the wastewater to achieve the purpose of removing the target ions; this method has limited effect on the removal of chloride ions, and is usually accompanied by a regeneration process. The equipment investment is high and it is easy to generate a large amount of waste liquid again, causing secondary pollution. Summary of the invention
[0004] In view of the above analysis, the embodiments of the present invention aim to provide a method for preparing an adsorbent and a method for removing chloride ions from water by adsorption, so as to solve at least one of the problems of existing removal methods, such as high cost, low efficiency, and easy pollution.
[0005] On the one hand, an embodiment of the present invention provides a method for preparing an adsorbent, which includes: mixing a mixed metal salt solution containing magnesium and aluminum with an alkaline solution, and standing and aging to obtain a magnesium-aluminum layered hydroxide; and calcining the magnesium-aluminum layered hydroxide to obtain an adsorbent.
[0006] Furthermore, the temperature of the static aging is 25°C to 70°C.
[0007] Furthermore, the standing aging time is 12 to 36 hours.
[0008] Furthermore, when the magnesium aluminum layered hydroxide is calcined, the calcination temperature is 120° C. to 600° C., and the calcination time is 1 to 5 hours.
[0009] Furthermore, the method also includes: after crushing and screening the magnesium-aluminum layered hydroxide, roasting the magnesium-aluminum layered hydroxide.
[0010] On the other hand, an embodiment of the present invention provides a method for removing chloride ions from water by adsorption, which is implemented using an adsorbent obtained by the preparation method according to the above embodiment, and includes: placing the adsorbent in a chlorine-containing solution to be treated, so that the chloride ions in the chlorine-containing solution are adsorbed on the adsorbent; separating the adsorbent and the solution adsorbed with chloride ions; and regenerating the separated adsorbent to recycle the adsorbent.
[0011] Furthermore, the separated adsorbent is regenerated, including: roasting and regenerating the adsorbent.
[0012] Furthermore, when the adsorbent is calcined for regeneration, the calcination temperature is 450° C. to 500° C., and the calcination time is 3 to 4 hours.
[0013] Furthermore, the amount of the adsorbent added to the chlorine-containing solution is 40 to 200 g / L.
[0014] Furthermore, the contact time of the adsorbent in the chlorine-containing solution is 3 to 15 hours.
[0015] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0016] 1. The present invention obtains magnesium aluminum oxide with a layered structure by calcining and modifying magnesium aluminum layered hydroxide, which gives the material a richer pore structure and a larger specific surface area, exposing more active sites, so that it can be used as an adsorbent with rich active sites and high reactivity for efficiently adsorbing chloride ions in water;
[0017] 2. When synthesizing magnesium aluminum layered hydroxide by coprecipitation, the mixed solution of metal solution and alkaline solution is left to stand for aging, thus eliminating the mechanical dripping and stirring operations in the traditional coprecipitation method. The method is simpler and easier to operate.
[0018] 3. The magnesium aluminum oxide adsorbent prepared by the present invention has excellent chloride ion removal effect and recycling regeneration performance.
[0019] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings are only for the purpose of illustrating specific embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0021] Figure 1 (a) is a scanning electron microscope photo of MgAl-LDH according to one embodiment of the present invention; Figure 1 (b) is a scanning electron microscope photograph of MgAl-LDO according to an embodiment of the present invention.
[0022] Figure 2 FIG. 5 is a particle size distribution curve of MgAl-LDH and MgAl-LDO according to an embodiment of the present invention.
[0023] Figure 3 (a) and (b) are respectively the pseudo-first-order adsorption kinetics and pseudo-second-order adsorption kinetics fitting diagrams of chloride ion adsorption by MgAl-LDO according to one embodiment of the present invention.
[0024] Figure 4 This is a fitting curve diagram of intra-particle diffusion of chloride ions adsorbed by MgAl-LDH according to one embodiment of the present invention.
[0025] Figure 5 (a) and (b) are respectively the adsorption of Cl by MgAl-LDO according to an embodiment of the present invention. - Fitting curve diagram of Langmuir model and Freundlich model.
[0026] Figure 6 2 are XRD patterns of MgAl-LDH and MgAl-LDO of Example 1.
[0027] Figure 7 This is a statistical graph of chloride ion removal rate and adsorption capacity of the adsorbent at different ion molar ratios in Example 2.
[0028] Figure 8 This is a statistical graph of chloride ion removal rate and adsorption capacity of the adsorbent at different calcination temperatures in Example 3.
[0029] Fig. 9 This is a statistical chart of chloride ion removal rate and adsorption capacity of the adsorbent at different calcination times in Example 4.
[0030] Fig.10 This is a statistical chart of chloride ion removal rate and adsorption capacity of the adsorbent at different adsorbent dosages in Example 5.
[0031] Fig.11 This is a statistical graph of chloride ion removal rate and adsorption capacity of the adsorbent at different initial chloride ion concentrations in Example 6.
[0032] Fig.12 This is a statistical graph of chloride ion removal rate and adsorption capacity of the adsorbent at different contact times in Example 7.
[0033] Fig.13 This is a statistical chart of the chloride ion removal rate of the adsorbent at different adsorption temperatures in Example 8.
[0034] Fig.14 This is a statistical graph of the chloride ion removal rate of the adsorbent under different coexisting anions in Example 9.
[0035] Fig.15 This is a statistical chart of the chloride ion removal rate of the adsorbent at different cycle numbers in Example 10. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solutions and advantages of the present invention clearer, exemplary embodiments of the present invention will be described below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. For the sake of clarity and conciseness, not all features of the actual implementation are described in the specification.
[0037] It is also necessary to explain here that, in order to avoid obscuring the present invention due to unnecessary details, only the device structure and / or processing steps closely related to the solution according to the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.
[0038] An embodiment of the present invention provides a method for preparing an adsorbent, and the preparation method specifically comprises the following steps:
[0039] Step S1, mixing a mixed metal salt solution containing magnesium and aluminum with an alkali solution, and allowing the mixture to stand for aging to obtain a magnesium-aluminum layered hydroxide;
[0040] Step S2, calcining the magnesium aluminum layered hydroxide to obtain an adsorbent.
[0041] The embodiment of the present invention obtains magnesium aluminum oxide with a layered structure by roasting and modifying magnesium aluminum layered hydroxide, which gives the material a richer pore structure and a larger specific surface area, exposing more active sites, so that it can be used as an adsorbent with rich active sites and high reactivity for efficient adsorption of chloride ions in water, solving the problem of limited removal effect of chloride ions by traditional methods. In addition, the preparation method of the embodiment of the present invention is simple and low in cost.
[0042] In addition, when synthesizing magnesium aluminum layered hydroxide in the embodiment of the present invention, the mixed solution of metal solution and alkaline solution is left to stand for aging, thus getting rid of the mechanical dripping and stirring operations in the traditional coprecipitation method, and the method is simpler and easier to operate and implement.
[0043] In some embodiments of the present invention, in the mixed metal salt solution of step S1, the molar ratio of magnesium ions to aluminum ions is 2:1 to 6:1, so as to prepare magnesium-aluminum bimetallic layered hydroxides of different molar ratios. The larger the molar ratio of magnesium ions to aluminum ions within the molar ratio range, the greater the adsorption amount of chloride ions in water, and the better the dechlorination effect; when the molar ratio is too large, the stability of the layered structure of the adsorbent may be destroyed and the adsorption performance of the adsorbent may be affected.
[0044] In some embodiments, in step S1, a mixed metal salt solution may be prepared using a magnesium salt and an aluminum salt, wherein the magnesium salt may be magnesium nitrate, and the aluminum salt may be aluminum nitrate.
[0045] In some embodiments of the present invention, the alkali solution used in step S1 can be a sodium hydroxide solution. Preferably, the concentration of sodium hydroxide is 3 mol / L, and the volume of the mixed metal salt solution is equal to the volume of the alkali solution, for example, both can be 250 mL. The embodiment of the present invention uses an equal volume of sodium hydroxide solution of this concentration to adjust the pH value of the salt solution so that the magnesium ions and aluminum ions in the solution are co-precipitated, which can ensure the complete precipitation of the two ions.
[0046] In some embodiments of the present invention, in step S1, the mixed solution can be left to stand and age at 25°C to 70°C. In this embodiment, the heating temperature is relatively low during the standing and aging, or even no heating is required, thus avoiding high-temperature heating during the aging process and simplifying the operation.
[0047] In some embodiments of the present invention, the static aging time can be 12 to 36 hours, so that the magnesium ions and chloride ions can fully react, and the precipitate can further grow and crystallize to obtain crystals with stable crystal structure and high crystallinity.
[0048] Within a certain range of static aging temperature and static aging time, increasing the temperature and / or time is helpful to improve the crystallinity of the adsorbent material, which is beneficial to improving the adsorption effect of the adsorbent material on chloride ions and the "structural memory effect" of the material.
[0049] In some embodiments of the present invention, after the static aging is completed, the generated crystals and the solution are separated, and the crystals are washed to neutrality to remove the alkali solution remaining on the surface. Then, the crystals are dried to obtain magnesium aluminum layered hydroxide. The drying temperature can be 70° C. and the drying time can be 10 hours.
[0050] In some embodiments of the present invention, when the magnesium aluminum layered hydroxide is calcined in step S2, the calcination temperature may be 120°C to 600°C, and the calcination time may be 1 to 5 hours; preferably, the calcination temperature is 400 to 500°C, and the calcination time is 3 to 4 hours.
[0051] More preferably, the calcination temperature is 480° C. and the calcination time is 4 hours.
[0052] In addition, during the calcination process, the heating rate may be 5 to 15° C. / min, for example, 10° C. / min.
[0053] In some embodiments, the magnesium-aluminum layered hydroxide is crushed and screened, and then the magnesium-aluminum layered hydroxide is calcined. In this embodiment, the particle size of the MgAl-LDH powder can be ensured to be small by crushing and screening, which is conducive to sufficient calcination modification. Exemplarily, the MgAl-LDH powder with a particle size of less than 74 μm is selected by crushing and screening, and calcination modification is performed.
[0054] Among them, magnesium aluminum layered hydroxide, also known as magnesium aluminum hydrotalcite (MgAl-LDH), as a two-dimensional anion intercalation material, has magnesium aluminum double hydroxide layers and exchangeable intercalation anions. Since the layer elements of MgAl-LDH can have different proportions, variable interlayer anions and controllable sizes, it brings more possibilities for the application of materials. The calcined and modified MgAl-LDH can undergo structural transformation and be converted into magnesium aluminum oxide (MgAl-LDO) with thermal and chemical stability.
[0055] In the embodiment of the present invention, the MgAl-LDO prepared under the above calcination conditions has a significant layered structure and a higher specific surface area and pore structure, so that it exhibits a good adsorption effect on chloride ions. Figure 1 (a) shows a scanning electron microscope photo of MgAl-LDH according to an embodiment of the present invention, Figure 1(b) shows a scanning electron microscope photo of MgAl-LDO according to an embodiment of the present invention. Figure 1 , MgAl-LDO exhibits richer pore structure and larger specific surface area than MgAl-LDH. Figure 2 FIG. 4 shows a particle size distribution curve of MgAl-LDH and MgAl-LDO according to an embodiment of the present invention. Figure 2 As shown, the particle size of MgAl-LDO is smaller than that of MgAl-LDH, indicating that the specific surface area of MgAl-LDO is larger.
[0056] Through the adsorption test analysis of the materials, MgAl-LDH, MgAl-LDO and MgAl-LDO-Cl after adsorption of chloride ions were obtained. - The specific surface area, total pore volume, average pore diameter and other data are shown in Table 1.
[0057] Table 1 MgAl-LDH, MgAl-LDO and MgAl-LDO-Cl - Specific surface area data table
[0058]
[0059] As shown in Table 1, the specific surface area and total pore volume of MgAl-LDO are much larger than those of MgAl-LDH, indicating that the calcination modification gives MgAl-LDO a larger specific surface area and rich pore structure, making it more conducive to the adsorption of chloride ions. - It exhibits smaller specific surface area and pore volume than MgAl-LDH.
[0060] The MgAl-LDO prepared in the embodiment of the present invention also has excellent chloride ion removal effect and recycling performance. When MgAl-LDH is calcined, most of its interlayer anions are eliminated to form MgAl-LDO. MgAl-LDO has a structural memory effect. When it comes into contact with water, it can recombine water and anions during the rehydration process, so that MgAl-LDO restores its original layered structure, thereby achieving the purpose of removing chloride ions from water. In addition, the exchange of negative ions in the aqueous solution with the remaining anions between the MgAl-LDO layers can further improve the removal efficiency of chloride ions.
[0061] When the MgAl-LDO adsorbed with chloride ions is calcined and regenerated again, most of the adsorbed anions are eliminated, so that the anions can be adsorbed again, so that it can be recycled and reused to adsorb chloride ions.
[0062] An embodiment of the present invention further provides a method for removing chloride ions from water by adsorption. The method can be implemented using the adsorbent prepared in the above embodiment, and specifically comprises the following steps:
[0063] Step S10, placing an adsorbent in the chlorine-containing solution to be treated, so that the chloride ions in the chlorine-containing solution are adsorbed on the adsorbent;
[0064] Step S20, separating the adsorbent adsorbed with chloride ions and the solution;
[0065] Step S30, regenerating the separated adsorbent to recycle the adsorbent.
[0066] In the embodiment of the present invention, since MgAl-LDO has a certain layer plate structure and a rich pore structure, it can adsorb a large amount of chloride ions in water, and can effectively remove chloride ions in water with high removal efficiency. In addition, the MgAl-LDO material itself is easy to prepare, has good recycling performance, and can be reused, thereby reducing the cost of removing chloride ions.
[0067] In order to make MgAl-LDO fully contact with the solution, in step S10, after the MgAl-LDO adsorbent is placed in the chlorine-containing solution, the solution can be stirred so that MgAl-LDO is fully contacted with the chloride ions in the solution to adsorb the chloride ions to the maximum extent.
[0068] In some embodiments, in step S10, the amount of adsorbent added to the chlorine-containing solution is 40 to 200 g / L. Within a certain range, the increase in the amount of adsorbent can improve the removal rate of chloride ions. As the amount increases, the removal rate of chloride ions will gradually reach saturation, and the adsorption capacity of the adsorbent will decrease. In this embodiment, the chloride ion removal rate and the cost of the agent are comprehensively considered, and the above-mentioned low-dosage adsorbent is used to achieve effective removal of chloride ions in water.
[0069] When MgAl-LDO is used to remove chloride ions from water, the electrostatic attraction of the positively charged layers in MgAl-LDO to chloride ions and the recovery of the unique layered structure of hydroxide promote the adsorption process, which is more conducive to the adsorption of chloride ions, thereby improving the removal rate and efficiency of chloride ions.
[0070] In the embodiment of the present invention, chloride ions are adsorbed on MgAl-LDO by chemical adsorption and physical adsorption, thereby increasing the adsorption amount of chloride ions by MgAl-LDO. The adsorption process of MgAl-LDO in the embodiment of the present invention conforms to the pseudo-secondary adsorption kinetic model and the Freundlich isotherm adsorption model, indicating that chemical adsorption and physical adsorption exist simultaneously in the adsorption process of MgAl-LDO.
[0071] Specifically, in order to study the intrinsic relationship between the adsorption capacity and contact time of the adsorbent material, MgAl-LDO was placed in a chlorine-containing solution under the conditions of a constant initial chloride ion concentration of 2000 mg / L and different contact times, and a chloride ion adsorption test was conducted on MgAl-LDO and a fitting analysis of the adsorption kinetic model was performed to analyze and study the adsorption kinetics of MgAl-LDO on chloride ions. Among them, the adsorption kinetic model includes a pseudo-first-order kinetic model, a pseudo-second-order kinetic model, and an intra-particle diffusion model, which are respectively expressed by the following expressions:
[0072] ln(q e -q t )=lnq e -k1×t (1)
[0073]
[0074] In the formula, q t (mg·g -1 ) and q e (mg·g -1 ) represent the adsorption amount of chloride ions at time t and equilibrium time respectively; k1(min -1 ) is the rate constant of the pseudo-first-order kinetic model; t (min) represents the contact time between MgAl-LDO and the chlorine-containing solution; k2 (g·mg -1 ·min -1 ) is the rate constant of the pseudo-second-order kinetic model; k p (g·mg -1 ·min 1 / 2 ) is the distribution coefficient that responds to the diffusion rate within the particle; C is the particle diffusion constant corresponding to the boundary layer thickness.
[0075] The fitting results of pseudo-first-order kinetic model and pseudo-second-order kinetic model at adsorption temperature of 20℃ are shown in Figure 3 The test results and fitting parameters are shown in Table 2. Figure 3 As shown in Table 2, the pseudo-first-order kinetic model (R 2 =0.98), the correlation coefficient (R 2 =0.99) is higher, and the theoretically calculated adsorption capacity (q e , cal) size is 34.14 mg·g -1 Closer to the experimental value (q e , exp)24.94mg·g -1 That is, the pseudo-second-order kinetic model is more suitable for describing Cl -The adsorption process of MgAl-LDO conforms to the pseudo-second-order adsorption kinetic model, indicating that the adsorption process of MgAl-LDO involves chemical adsorption, which is consistent with the adsorption of Cl - It is related to the interaction between MgAl-LDO layers.
[0076] Table 2 Fitting parameters of pseudo-first-order and pseudo-second-order adsorption kinetic models of MgAl-LDO
[0077]
[0078] The intraparticle diffusion was fitted for the adsorption structure under different contact times. When the fitting curve was linear, it showed that the intraparticle diffusion controlled the speed of the adsorption process. Figure 4 Shows q t With t 1 / 2 The fitting diagram of the intra-particle diffusion model is shown in Table 3.
[0079] Table 3 Fitting parameters of the intra-particle diffusion model of MgAl-LDO
[0080]
[0081] like Figure 4 As shown in the figure, the fitted linear curve does not pass through the origin, indicating that the effect of MgAl-LDO on Cl - The adsorption of is a complex process. p1 It can be seen that the diffusion speed in the first stage is relatively fast. The first stage involves Cl - The adsorption and diffusion on the surface of MgAl-LDO materials, the second stage is related to the intra-particle diffusion process. Considering the rate constant, it can be determined that the second stage is the rate-controlling step in the adsorption process, which is caused by the reduction of effective active sites of MgAl-LDO and the generation of a thicker boundary layer during the adsorption process.
[0082] Furthermore, the present invention uses the Langmuir isotherm model and the Freundlich isotherm model to simulate the experimental data to further analyze Cl - The Langmuir isotherm assumes that the adsorption of the adsorbate on the active site is uniform based on the monolayer adsorption; the Freundlich isotherm assumes that the adsorption is multilayer and non-uniform. The expressions of the above models can be expressed as follows:
[0083]
[0084] Among them, q e (mg·g -1 ) and q m (mg·g -1) represent the equilibrium adsorption capacity and the maximum adsorption capacity respectively; c e (mg·L -1 ) is Cl - The equilibrium concentration. Langmuir equilibrium adsorption constant K L (L mg -1 ) represents the affinity of the anion to the binding site, and the Freundlich constant K F is related to the adsorption capacity, and n is the heterogeneity factor. In this embodiment, the Langmuir and Freundlich isotherm fitting results of MgAl-LDO are as follows Figure 5 The fitting parameters are shown in Table 4.
[0085] Table 4 Langmuir and Freundlich isotherm model fitting parameters of MgAl-LDO
[0086]
[0087] Comparing the fitting results of the two models, we can observe that Cl - The adsorption on MgAl-LDO material is more consistent with the Freundlich model (R 2 =0.96), indicating that MgAl-LDO has a significant effect on Cl - There are multiple layers of adsorption in the removal process, which is usually caused by the existence of physical adsorption in the adsorption process.
[0088] The positive and negative values and magnitude of the adsorption thermodynamic parameters can determine whether the adsorption process can proceed spontaneously and the magnitude of the thermodynamic trend of spontaneous proceeding. The embodiments of the present invention further understand the influence of various factors on the adsorption process by analyzing the thermodynamic parameters. The adsorption thermodynamic parameters generally include the Gibbs free energy (ΔG 0 ), adsorption enthalpy change (ΔH 0 ), adsorption entropy change (ΔS 0 ) etc. For the solid-liquid system, the calculation formulas of the three are as follows:
[0089]
[0090] ΔG 0 =-RTlnK (8)
[0091] In the formula, c0(mg·L -1 ) is Cl - The initial concentration; K is the process equilibrium constant; R (J·mol·K -1 ) is the universal gas constant, which is 8.314; ΔG 0 (kJ·mol -1 ) represents the Gibbs free energy change; ΔS0 (J.mol.K -1 ) is the entropy change; ΔH 0 (kJ·mol -1 ) is the enthalpy change. After calculation of experimental data, MgAl-LDO has a great influence on Cl - The thermodynamic parameters of the adsorption process are shown in Table 5.
[0092] Table 5 Effect of MgAl-LDO on Cl at different temperatures - Table of thermodynamic parameters of the adsorption process
[0093]
[0094] As shown in Table 5, ΔG 0 All of them are negative, indicating that MgAl-LDO has a strong effect on Cl - The adsorption process is spontaneous; ΔH 0 and ΔS 0 is greater than zero, indicating that MgAl-LDO has a - The adsorption process is endothermic and the disorder increases. Increasing the temperature is conducive to the adsorption reaction, which indicates that physical adsorption exists in the adsorption process.
[0095] In some embodiments, in step S10, the contact time of the adsorbent in the chlorine-containing solution is set to 3 to 15 hours. As the contact time increases, the removal rate of chloride ions and the adsorption capacity of the adsorbent for chloride ions are increased, and eventually gradually reach saturation. In this embodiment, taking into account the removal effect and removal efficiency of chloride ions, the contact time is set to 3 to 15 hours, which can effectively achieve effective removal of chloride ions.
[0096] In some embodiments, in step S10, when the adsorbent adsorbs chloride ions in a chlorine-containing solution, the adsorption temperature is set to 20°C to 60°C. In this embodiment, the heating temperature during the adsorption process is relatively low or even no heating is required, thereby avoiding high-temperature heating during the adsorption process, and effective adsorption and removal of chloride ions can be achieved at a relatively low temperature.
[0097] In some embodiments of the present invention, the adsorbent is regenerated in step S30, including: calcining the adsorbent. According to the thermal stability of hydrotalcite, when the material is heated to different temperatures, water molecules and interlayer anions in the material will be removed and decomposed. Based on this characteristic of the material, the adsorbed MgAl-LDO-Cl - The calcination regeneration is carried out to eliminate most of the chloride ions between the middle plates of the MgAl-LDO adsorbent, so that it can be reused to adsorb chloride ions, thus achieving the purpose of recycling and regeneration.
[0098] In some embodiments of the present invention, when the adsorbent is calcined and regenerated, the calcination temperature is 450° C. to 500° C. and the calcination time is 3 to 5 hours. Preferably, the calcination temperature during regeneration is 480° C. and the calcination time is 4 hours.
[0099] After the adsorbent is calcined and regenerated, it can be used again to adsorb chloride ions in water. After the adsorption is completed, it is calcined and regenerated under the same conditions so that it can be used again to adsorb chloride ions in water, and so on, thereby realizing the recycling and regeneration of the adsorbent.
[0100] In the embodiment of the present invention, the removal rate of chloride ions by the adsorbent MgAl-LDO can reach more than 97%, and the removal rate of chloride ions by the adsorbent MgAl-LDO can still be maintained at more than 90% after 11 cycles of regeneration.
[0101] In order to illustrate the effects of the above embodiments of the present invention, the preparation method of the adsorbent provided by the present invention and the method of removing chloride ions in water by using the adsorbent are further described below in conjunction with the accompanying drawings and specific embodiments.
[0102] Example 1
[0103] Mg 2+ / Al 3+ Mg(NO3)2·6H2O and Al(NO3)3·9H2O in a molar ratio of 2:1 to 6:1 were mixed, and water was added to make the volume 250 mL to obtain a mixed metal nitrate solution. The mixed nitrate solution and a NaOH solution with a concentration of 3 mol / L were quickly mixed to form a white slurry.
[0104] The solution was allowed to stand at room temperature for 18 hours, and then the supernatant was removed by filtration, and the concentrated slurry was washed with deionized water until the filtrate was close to neutral, and the obtained white concentrated slurry was dried in an oven at 70°C for 10 hours to obtain a white solid. The white solid was crushed and screened to select a white powder with a particle size of less than 74 μm, i.e., MgAl-LDH powder. In this embodiment, the particle size of the MgAl-LDH powder can be ensured to be small by crushing and screening, which is conducive to sufficient calcination modification.
[0105] MgAl-LDH powder was heated in a muffle furnace at 10 °C min -1 The temperature was raised to 480°C at a heating rate of 1.5°C and calcined for 3 hours to obtain MgAl-LDO adsorbent powder. Figure 6 As shown, the XRD pattern shows that the above method successfully prepared MgAl-LDH and MgAl-LDO.
[0106] Example 2
[0107] The NaCl solution with an initial chloride ion concentration of 2000 mg / L was used as a simulated chlorine-containing solution for the chloride ion removal experiment.
[0108] Take multiple 25mL of the above NaCl solution and transfer it to a 100mL conical flask. In order to explore the effect of the magnesium-aluminum molar ratio on the chloride ion removal effect, the Mg in Example 1 2+ / Al 3+ MgAl-LDO with a molar ratio of 2:1, 3:1, 4:1, 5:1, and 6:1 was added to the above NaCl solution in an amount of 2 g. After magnetic stirring at 300-320 r / min for 2 h at a temperature of 20°C, the mixture was allowed to settle to ensure a contact time of 13 h, and the supernatant was obtained by centrifugation.
[0109] Ion chromatography was used to detect Cl in the supernatant. - concentration, and calculate the effect of MgAl-LDO on Cl - The adsorption capacity and chloride ion removal rate are shown in Table 6 and Figure 7 As shown. Among them, with Mg 2+ / Al 3+ With the increase of molar ratio, MgAl-LDO has a significant effect on Cl - The adsorption amount and chloride ion removal rate gradually increased.
[0110] Table 6 Chloride ion removal rate and adsorption capacity at different molar ratios
[0111]
[0112] Example 3
[0113] In order to explore the effect of calcination temperature on the removal of chloride ions, Mg 2+ / Al 3+ MgAl-LDH with a molar ratio of 6 was calcined at different calcination temperatures (120°C, 240°C, 360°C, 480°C, 600°C) for 3 h to obtain MgAl-LDO adsorbent powder. The other conditions were the same as in Example 1.
[0114] Take multiple 25mL NaCl solutions with a chloride ion concentration of 2000mg / L and transfer them to a conical flask, add 2g of MgAl-LDO calcined at different calcination temperatures, stir magnetically at 300-320r / min for 2h at an ambient temperature of 20°C, let it stand for sedimentation, ensure the contact time is 13h, and centrifuge to obtain the supernatant.
[0115] Ion chromatography was used to detect Cl in the supernatant. - concentration, and calculate the effect of MgAl-LDO on Cl at different calcination temperatures -The adsorption capacity and chloride ion removal rate are shown in Table 7 and Figure 8 shown.
[0116] Table 7 Chloride ion removal rate and adsorption capacity at different calcination temperatures
[0117]
[0118] Among them, with the increase of calcination temperature, MgAl-LDO has a great influence on Cl - The adsorption capacity of MgAl-LDO for Cl - The adsorption capacity of Cl is the largest. - The removal rate reached the highest level, which was 98.16%. When the calcination temperature was greater than 480℃, the removal rate of MgAl-LDO to Cl - The adsorption capacity decreased.
[0119] Example 4
[0120] In order to explore the effect of calcination time on the removal of chloride ions, Mg 2+ / Al 3+ MgAl-LDH with a molar ratio of 6 was calcined at a calcination temperature of 480° C. for different times (1 h, 2 h, 3 h, 4 h, 5 h) to obtain MgAl-LDO adsorbent powder. The other conditions were the same as those in Example 1.
[0121] Take multiple 25mL NaCl solutions with a concentration of 2000mg / L and transfer them to a conical flask, add 2g of MgAl-LDO obtained by roasting at different times, stir magnetically at 20℃ and 300-320r / min for 2h, let it stand for sedimentation, ensure the contact time is 13h, and centrifuge to take the supernatant.
[0122] Ion chromatography was used to detect Cl in the supernatant. - concentration, and calculate the effect of MgAl-LDO on Cl under different calcination times - The adsorption capacity and chloride ion removal rate are shown in Table 8 and Fig. 9 shown.
[0123] Table 8 Chloride ion removal rate and adsorption capacity at different calcination times
[0124]
[0125] Among them, as the calcination time increases, MgAl-LDO has a greater influence on Cl - The adsorption capacity of MgAl-LDO increased first and then decreased. - The adsorption capacity is the largest, and the chloride ion removal rate reaches the maximum, which is 95.45%.
[0126] Example 5
[0127] In order to explore the effect of adsorbent addition on chloride ion removal, several 25mL NaCl solutions with a chloride ion concentration of 2000mg / L were taken and transferred to conical flasks, and MgAl-LDO obtained by roasting at 480℃ for 3h was added thereto in amounts of 1g, 2g, 3g, 4g, and 5g, respectively. After magnetic stirring at 20℃ and 300-320r / min for 2h, the mixture was allowed to settle to ensure a contact time of 13h, and the supernatant was obtained by centrifugation.
[0128] Ion chromatography was used to detect Cl in the supernatant. - concentration, and calculate the effect of MgAl-LDO on Cl - The adsorption capacity and chloride ion removal rate are shown in Table 9 and Fig.10 As shown in the figure, with the increase of MgAl-LDO addition, the removal rate of chloride ions in the solution gradually increased. However, MgAl-LDO had a - The adsorption capacity of MgAl-LDO gradually decreased, resulting in the fact that MgAl-LDO was not fully utilized.
[0129] Table 9 Chloride ion removal rate and adsorption capacity at different adsorbent dosages
[0130]
[0131] Example 6
[0132] In order to explore the effect of the initial chloride ion concentration of the chloride-containing solution on the chloride ion removal effect of the adsorbent, 25 mL of the solution with an initial concentration of 500 mg·L -1 、1250mg·L -1 , 2000mg·L -1 、2750mg·L -1 、3500mg·L -1 、4250mg·L -1 2g of MgAl-LDO calcined at 480℃ for 3h was added to the NaCl solution. After magnetic stirring at 20℃ and 300-320r / min for 2h, the mixture was allowed to settle to ensure a contact time of 13h, and the supernatant was collected by centrifugation.
[0133] Ion chromatography was used to detect Cl in the supernatant. - concentration, and calculate the effect of MgAl-LDO on Cl - The adsorption capacity and chloride ion removal rate are shown in Table 10 and Fig.11 As shown. Among them, as Cl in the solution - With the increase of initial concentration, MgAl-LDO has a significant effect on Cl -The adsorption capacity increased, reaching a maximum of 40.50 mg / g; however, the chloride ion removal rate gradually decreased.
[0134] Table 10 Chloride ion removal rate and adsorption capacity at different initial chloride ion concentrations
[0135]
[0136] Example 7
[0137] In order to explore the effect of the contact time of the adsorbent on the removal of chloride ions, 25 mL of the adsorbent with an initial concentration of 2000 mg·L -1 2g of MgAl-LDO calcined at 480℃ for 3h was added to the NaCl solution. The mixture was stirred magnetically at 20℃ and 300-320r / min. Samples were taken within 1-15h. After the samples were allowed to settle, they were centrifuged to obtain the supernatant.
[0138] Ion chromatography was used to detect Cl in the supernatant. - concentration, and calculate the effect of MgAl-LDO on Cl - The adsorption capacity and chloride ion removal rate are shown in Table 11 and Fig.12 As shown in the figure, with the increase of contact time between MgAl-LDO and solution, the effect of MgAl-LDO on Cl - The adsorption capacity and chloride ion removal rate gradually increased.
[0139] Table 11 Chloride ion removal rate and adsorption capacity at different contact times
[0140]
[0141] Example 8
[0142] In order to explore the effect of adsorption temperature on the removal of chloride ions, 25 mL of the initial concentration of 2000 mg·L -1 2g of MgAl-LDO calcined at 480℃ for 3h was added to each of the NaCl solutions. The mixture was stirred magnetically for 2h at different adsorption temperatures (20℃, 40℃, 60℃) and 300-320r / min, and allowed to settle to ensure a contact time of 13h. The supernatant was separated by centrifugation.
[0143] Ion chromatography was used to detect Cl in the supernatant. - concentration, and calculate the effect of MgAl-LDO on Cl - The adsorption capacity and chloride ion removal rate are shown in Table 12 and Fig.13 As shown in the figure, the higher the adsorption temperature of MgAl-LDO and the solution, the higher the adsorption of MgAl-LDO to Cl -The higher the adsorption capacity and chloride ion removal rate, and the shorter the contact time required for chloride ion removal.
[0144] Table 12 Chloride ion removal rate and adsorption capacity at different adsorption temperatures
[0145]
[0146] Example 9
[0147] In order to explore the chloride ion removal effect of the adsorbent when other anions exist in the solution, Mg 2+ / Al 3+ MgAl-LDO with a molar ratio of 6:1, a calcination temperature of 480 °C, and a calcination time of 3 h was added to 25 mL of NO3 - 、SO4 - 、CO3 - The initial chloride ion concentration was 2000 mg / L, and the amount of MgAl-LDO added was 2 g. After magnetic stirring for 2 h at 20 ° C and 300-320 r / min, the mixture was allowed to settle for 13 h, and the supernatant was centrifuged. The Cl in the supernatant was detected using an ion chromatograph. - concentration, and calculated the chloride ion removal rate of MgAl-LDO.
[0148] like Fig.14 As shown, the coexisting NO3 - The effect on the removal of chloride ions is small. With the increase of the concentration of coexisting anions, the chloride ion removal rate of MgAl-LDO gradually decreases, indicating that MgAl-LDO can also adsorb and remove other coexisting anions.
[0149] Example 10
[0150] In order to explore the recycling performance of the adsorbent, Mg 2+ / Al 3+ MgAl-LDO with a molar ratio of 6:1, a calcination temperature of 480°C, and a calcination time of 3h was added to 25mL of NaCl solution with an initial concentration of 2000mg / L. The addition amount was 2g. After magnetic stirring for 2h at 20°C and 300-320r / min, it was allowed to settle and the contact time was ensured to be 13h. The supernatant was centrifuged and separated. The Cl in the supernatant was detected using an ion chromatograph. - concentration, and calculate the effect of MgAl-LDO on Cl - adsorption capacity and chloride ion removal rate.
[0151] The adsorbed Cl - The MgAl-LDO was calcined at 480 °C for 3 h to regenerate it and then added again to an initial concentration of 2000 mg·L-1 The reuse and recycling regeneration experiments were carried out in NaCl solution, and the adsorption reaction conditions were the same as the first adsorption.
[0152] Calculate the adsorption of Cl by MgAl-LDO during each regeneration cycle - The adsorption capacity and chloride ion removal rate are shown in Table 13 and Fig.15 Among them, after 11 cycles, the chloride ion removal rate of MgAl-LDO can still be maintained above 90%, indicating that it has excellent recycling performance.
[0153] Table 13 Chloride ion removal rate and adsorption capacity at different cycle times
[0154]
[0155] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing an adsorbent, characterized in that: include: Mixing a mixed metal salt solution containing magnesium and aluminum with an alkali solution and allowing the solution to stand for aging to obtain a magnesium-aluminum layered hydroxide; The magnesium aluminum layered hydroxide is calcined to obtain the adsorbent.
2. The method according to claim 1, characterized in that: The temperature of the static aging is 25°C to 70°C.
3. The method according to claim 2, characterized in that The static aging time is 12 to 36 hours.
4. The method according to claim 1, characterized in that The calcination temperature of the magnesium aluminum layered hydroxide is 120° C. to 600° C., and the calcination time is 1 to 5 hours.
5. The method according to any one of claims 1 to 4, characterized in that: Also includes: After the magnesium aluminum layered hydroxide is crushed and screened, the magnesium aluminum layered hydroxide is calcined.
6. A method for removing chloride ions from water by adsorption, characterized in that: The method is implemented using an adsorbent obtained by the preparation method according to any one of claims 1 to 5, and comprises: placing the adsorbent in a chlorine-containing solution to be treated, so that the chloride ions in the chlorine-containing solution are adsorbed on the adsorbent; separating the adsorbent adsorbed with the chloride ions and the solution; The separated adsorbent is regenerated to recycle the adsorbent.
7. The method according to claim 6, characterized in that The separated adsorbent is regenerated, comprising: calcining and regenerating the adsorbent.
8. The method according to claim 7, characterized in that When the adsorbent is calcined for regeneration, the calcination temperature is 450° C. to 500° C. and the calcination time is 3 to 4 hours.
9. The method according to claim 6, characterized in that The adsorbent is added in an amount of 40 to 200 g / L in the chlorine-containing solution.
10. The method according to claim 6, characterized in that The contact time of the adsorbent in the chlorine-containing solution is 3 to 15 hours.
Citation Information
Cited By
Preparation of roasted ternary layered double hydroxide with enhanced adsorption performance and application of roasted ternary layered double hydroxide in low-concentration bromide ion adsorption
CN119281290A
Method for modifying interlayer perchlorate radical intercalation of hydrotalcite
CN119752222A