Calcium-magnesium loaded biochar adsorbent as well as preparation method and application thereof
Through the preparation of calcium and magnesium loaded biochar adsorbents, the problems of poor phosphorus adsorption ability and environmental pollution of biochar in the existing technology are solved, the efficient removal of low concentration phosphorus and the application of slow-release fertilizers are achieved, and the resource utilization rate is improved. .
Patent Information
- Application Number
- CN202410839365.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-11
AI Technical Summary
Existing biochar modification technology is complex and may cause environmental pollution. It is difficult to effectively improve the adsorption capacity of phosphorus, and the original biochar has poor adsorption capacity for phosphorus.
Using the preparation method of calcium and magnesium loaded biochar adsorbent, the biomass material is mixed with a strong alkali and then stirred with an alcohol solution and a hydrochloric acid solution, adding calcium salt and magnesium salt, ultrasonic treatment and calcining under the protection of inert gas to prepare a biochar adsorbent with Calcium and magnesium loaded biochar adsorbent with excellent phosphorus adsorption performance.
It achieves excellent phosphorus adsorption performance at low concentrations and can be used for removal in actual wastewater. The adsorbed material can be used as a slow-release fertilizer to improve resource utilization and reduce environmental pollution.
Smart Images

Figure CN118751201A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste resource utilization and environmental protection, and specifically relates to a calcium-magnesium loaded biochar adsorbent and a preparation method and application thereof. Background Art
[0002] Biochar, a solid porous material with a large specific surface area and high porosity produced by high-temperature pyrolysis of agricultural waste, is widely used in environmental pollution remediation and soil improvement. Studies have found that adding biochar to soil can increase the soil cation exchange capacity and bacterial solubility, enhance the soil's repulsion of phosphorus, and thus reduce the soil's adsorption of available phosphorus. Therefore, it is of great significance to recover phosphorus from water bodies through biochar adsorption and use it in agricultural production. However, the negative charge characteristics of the original biochar surface lead to its poor adsorption capacity for phosphorus, and physical and chemical modifications are required to improve its adsorption capacity. The current modification method is mainly metal modification. By doping biochar with metal ions such as iron, lanthanum, calcium, and magnesium, the electrostatic attraction and ligand exchange capacity of biochar can be enhanced, greatly improving its adsorption capacity for phosphorus. For example, lanthanum-modified sycamore biochar was used to remove phosphorus from actual wastewater, and the adsorption capacity reached 116 mg / g. Iron-impregnated straw biochar showed an excellent phosphorus adsorption capacity of 39.2 mg / g compared with unmodified biochar. However, the above biochar modification technology preparation process is relatively complicated and may cause secondary pollution to the environment, which is not conducive to the resource utilization of phosphorus.
[0003] In recent years, biochar (BC) converted from waste has gradually become a research hotspot in the field of adsorption materials. It can not only realize waste utilization, alleviate environmental pressure, but also reduce cost investment. Based on this, the present invention provides a new type of biochar adsorbent, which provides a feasible way to control phosphorus pollution. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, one of the purposes of the present invention is to provide a method for preparing a calcium-magnesium loaded biochar adsorbent, which is simple, easy to operate and practice, green and environmentally friendly, and can save costs.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a calcium and magnesium loaded biochar adsorbent comprises the following steps:
[0007] (1) pre-treating the biomass material, mixing it with a strong base, and ball-milling it to obtain a biomass mixture;
[0008] (2) adding an alcohol solution and a hydrochloric acid solution to the biomass mixture of step (1), adding calcium salt and magnesium salt after ultrasonication, and stirring the reaction to obtain a calcium-magnesium loaded biomass mixture;
[0009] (3) Under the protection of inert gas, the calcium-magnesium-loaded biomass mixture of step (2) is calcined to obtain a calcium-magnesium-loaded biochar adsorbent.
[0010] Furthermore, in step (2), the mass ratio of the biomass mixture, calcium salt and magnesium salt is 1:(0.1-0.3):(0.1-0.3), the calcium salt is selected from one or more of calcium chloride, calcium sulfate and calcium hydroxide, and the magnesium salt is selected from one or more of magnesium chloride hexahydrate, magnesium sulfate and magnesium nitrate.
[0011] Furthermore, in step (2), the solid-liquid ratio of the biomass mixture to the alcohol solution and the hydrochloric acid solution is 1:(0.04-0.05):(0.5-1.5), the mass concentration of the hydrochloric acid is 28-35%, the alcohol solution is an anhydrous ethanol solution or a methanol solution, the solvent of the alcohol solution is water, and the volume ratio of anhydrous ethanol or methanol to water in the alcohol solution is 1:(0.05-0.5).
[0012] Furthermore, the alcohol solution is an anhydrous ethanol solution.
[0013] Furthermore, the stirring reaction temperature in step (2) is 30-50° C., and the stirring reaction time is 5-10 h.
[0014] Furthermore, the pretreatment in step (1) is to screen the biomass material, the biomass material is selected from one of coffee grounds, wheat straw, and peanut shells, the mesh size of the screening is 80-100 mesh, the mass ratio of the biomass material to the strong alkali is 1:(0.5-2), and the ball milling time is 1.5-3h.
[0015] Furthermore, in step (1), the mass ratio of the biomass material to the strong base is 1:1.
[0016] Furthermore, the calcination temperature in step (3) is to increase the temperature to 550-650°C at a heating rate of 5-10°C / min, and the calcination time is 2-3h.
[0017] A second object of the present invention is to provide a calcium-magnesium loaded biochar adsorbent having excellent adsorption performance.
[0018] To achieve the above object, the present invention adopts the following technical solutions:
[0019] A calcium-magnesium loaded biochar adsorbent is prepared by adopting the preparation method of the calcium-magnesium loaded biochar adsorbent.
[0020] The third object of the present invention is to provide an application of a calcium and magnesium loaded biochar adsorbent, which has broad application prospects.
[0021] To achieve the above object, the present invention adopts the following technical solutions:
[0022] An application of a calcium-magnesium loaded biochar adsorbent, and the application of the calcium-magnesium loaded biochar adsorbent as a phosphorus adsorbent.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The present invention uses waste biomass materials as raw materials, strictly controls the calcium and magnesium loading, and obtains a calcium and magnesium loaded biochar adsorbent with excellent phosphorus adsorption performance by closely coordinating each step.
[0025] (2) The biochar adsorbent of the present invention has excellent adsorption performance even at low concentrations and can be used to remove phosphorus from actual wastewater.
[0026] (3) The preparation method of the present invention has the advantages of easy availability of raw materials, low cost, and environmental protection.
[0027] (4) The calcium-magnesium loaded biochar adsorbent of the present invention has excellent phosphorus adsorption performance and can be used as a slow-release fertilizer after adsorption, which can improve resource utilization and reduce environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is the XRD diagram of the biochar adsorbent prepared in Example 1 and Comparative Example 1;
[0029] Figure 2 is a morphological characteristic diagram of the biochar adsorbent prepared in Example 1;
[0030] Figure 3 This is a morphological characteristic diagram of the biochar adsorbent prepared in Comparative Example 1;
[0031] Figure 4 It is a result diagram of the equilibrium adsorption amount of phosphorus by the biochar adsorbent of Examples 1-6 and Comparative Examples 1-3;
[0032] Figure 5 is a graph showing the adsorption performance of the biochar adsorbent of Example 1 for low concentration phosphorus;
[0033] Figure 6 This is a graph of crop growth after adding calcium and magnesium loaded biochar adsorbent after phosphorus adsorption to the soil. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further explained below in conjunction with specific embodiments, comparative examples, test examples and drawings.
[0035] In the following examples, comparative examples and test examples, the raw materials and preparation methods used are conventional materials and techniques in the art unless otherwise specified.
[0036] Example 1
[0037] Example 1 provides a method for preparing a calcium and magnesium loaded biochar adsorbent, comprising the following steps:
[0038] (1) Passing the collected coffee grounds through a 100-mesh sieve, mixing the coffee grounds with sodium hydroxide in a mass ratio of 1:1, and ball milling the mixture using a ball mill. The ball milling beads used in the ball milling are zirconia balls, and the zirconia balls include a first zirconia ball, a second zirconia ball, and a third zirconia ball. The diameter of the first zirconia ball is 15 mm, the diameter of the second zirconia ball is 5 mm, and the diameter of the third zirconia ball is 3 mm. The mass ratio of the first zirconia ball, the second zirconia ball, and the third zirconia ball is 2:5:3. The mixture is ball milled for 2 h to obtain a coffee ground mixture.
[0039] (2) Take 10 g of the coffee grounds mixture of step (1), add anhydrous ethanol solution (composed of 200 mL of water and 20 mL of anhydrous ethanol), add 10 mL of 30% hydrochloric acid solution, add 3 g of calcium chloride and 3 g of magnesium chloride hexahydrate after ultrasonic treatment for 20 min, stir and react at 40° C. for 5 h, and after the reaction is completed, separate and dry to obtain a calcium-magnesium loaded coffee grounds mixture;
[0040] (3) The calcium-magnesium-loaded coffee grounds mixture of step (2) was placed in a tubular furnace, heated to 600° C. at a heating rate of 5° C. / min under a nitrogen atmosphere, calcined for 2 h, cooled to room temperature, and ground through a 100-mesh sieve to obtain a calcium-magnesium-loaded biochar adsorbent, recorded as CMBC.
[0041] Example 1 also provides a calcium-magnesium-loaded biochar adsorbent, which is prepared using the above-mentioned preparation method of the calcium-magnesium-loaded biochar adsorbent.
[0042] Example 2
[0043] Example 2 provides a method for preparing a calcium and magnesium loaded biochar adsorbent, comprising the following steps:
[0044] (1) passing the collected coffee grounds through an 80-mesh sieve, mixing the coffee grounds with sodium hydroxide in a mass ratio of 1:0.5, and ball milling the mixture using a ball mill. The ball milling beads used in the ball milling are zirconia balls, and the zirconia balls include a first zirconia ball, a second zirconia ball, and a third zirconia ball. The diameter of the first zirconia ball is 15 mm, the diameter of the second zirconia ball is 5 mm, and the diameter of the third zirconia ball is 3 mm. The mass ratio of the first zirconia ball, the second zirconia ball, and the third zirconia ball is 1:4:2. The mixture is ball milled for 1.5 hours to obtain a coffee ground mixture.
[0045] (2) Take 10 g of the coffee grounds mixture of step (1), add anhydrous ethanol solution (composed of 238 mL of water and 12 mL of anhydrous ethanol), add 20 mL of 28% hydrochloric acid solution, add 1 g of a mixture of calcium chloride and calcium sulfate, and 1 g of a mixture of magnesium chloride hexahydrate and magnesium sulfate, and stir at 50° C. for 6 h. After the reaction is completed, separate and dry to obtain a calcium-magnesium loaded coffee grounds mixture;
[0046] (3) The calcium-magnesium-loaded coffee grounds mixture of step (2) was placed in a tubular furnace, heated to 550°C at a heating rate of 8°C / min under a nitrogen atmosphere, calcined for 3 hours, cooled to room temperature, and then ground through a 100-mesh sieve to obtain a calcium-magnesium-loaded biochar adsorbent, recorded as C1M1BC.
[0047] Example 2 also provides a calcium-magnesium-loaded biochar adsorbent, which is prepared using the above-mentioned preparation method of the calcium-magnesium-loaded biochar adsorbent.
[0048] Example 3
[0049] Example 3 provides a method for preparing a calcium and magnesium loaded biochar adsorbent, comprising the following steps:
[0050] (1) passing the collected coffee grounds through a 90-mesh sieve, mixing the coffee grounds with sodium hydroxide in a mass ratio of 1:2, and ball milling using a ball mill. The ball milling beads used in the ball milling are zirconia balls, and the zirconia balls include a first zirconia ball, a second zirconia ball, and a third zirconia ball. The diameter of the first zirconia ball is 15 mm, the diameter of the second zirconia ball is 5 mm, and the diameter of the third zirconia ball is 3 mm. The mass ratio of the first zirconia ball, the second zirconia ball, and the third zirconia ball is 3:6:4. The ball milling is performed for 3 hours to obtain a coffee ground mixture.
[0051] (2) Take 10 g of the coffee grounds mixture of step (1), add a methanol solution (composed of 133 mL of water and 67 mL of methanol), add 6.7 mL of a 35% hydrochloric acid solution, add 3 g of calcium chloride, a mixture of calcium sulfate and calcium hydroxide, 3 g of magnesium chloride hexahydrate, a mixture of magnesium sulfate and magnesium nitrate, and stir at 30° C. for 10 h. After the reaction is completed, separate and dry to obtain a calcium-magnesium loaded coffee grounds mixture;
[0052] (3) The calcium-magnesium-loaded coffee grounds mixture of step (2) was placed in a tubular furnace, heated to 650°C at a heating rate of 10°C / min under a nitrogen atmosphere, calcined for 2.5 hours, cooled to room temperature, and then ground through a 100-mesh sieve to obtain a calcium-magnesium-loaded biochar adsorbent, recorded as C3M1BC.
[0053] Example 3 also provides a calcium-magnesium-loaded biochar adsorbent, which is prepared using the above-mentioned preparation method of the calcium-magnesium-loaded biochar adsorbent.
[0054] Example 4
[0055] Example 4 provides a method for preparing a calcium and magnesium loaded biochar adsorbent, comprising the following steps:
[0056] (1) Passing the collected coffee grounds through a 100-mesh sieve, mixing the coffee grounds with sodium hydroxide in a mass ratio of 1:1, and ball milling the mixture using a ball mill. The ball milling beads used in the ball milling are zirconia balls, and the zirconia balls include a first zirconia ball, a second zirconia ball, and a third zirconia ball. The diameter of the first zirconia ball is 15 mm, the diameter of the second zirconia ball is 5 mm, and the diameter of the third zirconia ball is 3 mm. The mass ratio of the first zirconia ball, the second zirconia ball, and the third zirconia ball is 2:5:3. The mixture is ball milled for 2 h to obtain a coffee ground mixture.
[0057] (2) Take 10 g of the coffee grounds mixture of step (1), add anhydrous ethanol solution (composed of 200 mL of water and 20 mL of anhydrous ethanol), add 10 mL of 30% hydrochloric acid solution, add 1 g of calcium chloride and 3 g of magnesium chloride hexahydrate after ultrasonic treatment for 20 min, stir and react at 40° C. for 5 h, and after the reaction is completed, separate and dry to obtain a calcium-magnesium loaded coffee grounds mixture;
[0058] (3) The calcium-magnesium-loaded coffee grounds mixture of step (2) was placed in a tubular furnace, heated to 600°C at a heating rate of 5°C / min under a nitrogen atmosphere, calcined for 2 hours, cooled to room temperature, and ground through a 100-mesh sieve to obtain a calcium-magnesium-loaded biochar adsorbent, recorded as C1M3BC.
[0059] Example 4 also provides a calcium-magnesium-loaded biochar adsorbent, which is prepared using the above-mentioned preparation method of the calcium-magnesium-loaded biochar adsorbent.
[0060] Example 5
[0061] The difference between Example 5 and Example 1 is that the biomass material is wheat straw, and the rest is the same as Example 1, forming Example 5.
[0062] Example 6
[0063] The difference between Example 6 and Example 1 is that the biomass material is peanut shells, and the rest is the same as Example 1, forming Example 6.
[0064] Comparative Example 1
[0065] Comparative Example 1 provides a method for preparing a biochar adsorbent, comprising the following steps:
[0066] After the collected coffee grounds were passed through a 100-mesh sieve, 10 g was weighed and placed in a tubular furnace. Under a nitrogen atmosphere, the temperature was raised to 600 °C at a heating rate of 5 °C / min and calcined for 2 h. After cooling to room temperature, the ground coffee grounds were ground through a 100-mesh sieve to obtain a biochar adsorbent, recorded as BC.
[0067] Comparative Example 2
[0068] Comparative Example 2 provides a method for preparing a calcium-loaded biochar adsorbent, comprising the following steps:
[0069] (1) Obtaining a coffee grounds mixture: The preparation process of the coffee grounds mixture is the same as step (1) of Example 1;
[0070] (2) Take 10 g of the coffee grounds mixture of step (1), add anhydrous ethanol solution (composed of 200 mL of water and 20 mL of anhydrous ethanol), add 10 mL of 30% hydrochloric acid solution, add 3 g of calcium chloride after ultrasonic treatment for 20 min, stir and react at 40° C. for 5 h, and after the reaction is completed, separate and dry to obtain a calcium-loaded coffee grounds mixture;
[0071] (3) The calcium-loaded coffee grounds mixture of step (2) was placed in a tubular furnace, heated to 600° C. at a heating rate of 5° C. / min under a nitrogen atmosphere, calcined for 2 h, cooled to room temperature, and then ground through a 100-mesh sieve to obtain a calcium-loaded biochar adsorbent, recorded as CBC.
[0072] Comparative Example 3
[0073] Comparative Example 3 provides a method for preparing a magnesium-loaded biochar adsorbent, comprising the following steps:
[0074] (1) Obtaining a coffee grounds mixture: The preparation process of the coffee grounds mixture is the same as step (1) of Example 1;
[0075] (2) Take 10 g of the coffee grounds mixture of step (1), add anhydrous ethanol solution (composed of 200 mL of water and 20 mL of anhydrous ethanol), add 10 mL of 30% hydrochloric acid solution, add 3 g of magnesium chloride hexahydrate after ultrasonic treatment for 20 min, stir and react at 40° C. for 5 h, and after the reaction is completed, separate and dry to obtain a magnesium-loaded coffee grounds mixture;
[0076] (3) The magnesium-loaded coffee grounds mixture of step (2) was placed in a tubular furnace, heated to 600° C. at a heating rate of 5° C. / min under a nitrogen atmosphere, calcined for 2 h, cooled to room temperature, and then ground through a 100-mesh sieve to obtain a magnesium-loaded biochar adsorbent, recorded as MBC.
[0077] The performance of the calcium-magnesium loaded biochar adsorbent prepared by the present invention was tested as follows.
[0078] 1. X-ray diffraction detection of calcium and magnesium loaded biochar adsorbent
[0079] The biochar adsorbents prepared in Example 1 and Comparative Example 1 were subjected to X-ray diffraction testing, and the results are shown in Figure 1 .
[0080] Figure 1 The XRD diagrams of the biochar adsorbents prepared in Example 1 and Comparative Example 1 are shown in FIG. Figure 1 It is known that MgO (JCPDF: 71-1176), CaCO3 (JCPDF: 72-1616), and CaO (JCPDF: 77-2376) appear on the biochar adsorbent of Example 1, while no peak of the relevant intensity diffraction band appears on the biochar adsorbent of Comparative Example 1. This shows that Example 1 successfully prepared the calcium and magnesium loaded biochar adsorbent.
[0081] 2. Detection of the morphological characteristics of calcium and magnesium loaded biochar adsorbent
[0082] The morphology of the biochar adsorbents prepared in Example 1 and Comparative Example 1 was observed using a field emission scanning electron microscope. The results are as follows: Figure 2-3 shown.
[0083] Figure 2 This is a morphological characteristic diagram of the biochar adsorbent prepared in Example 1. Figure 3 This is the morphological characteristics of the biochar adsorbent prepared in Example 1. Figure 3 It is known that the biochar adsorbent of Comparative Example 1 is a porous sheet structure with a rough and irregular surface, which provides an advantage for the use of calcium and magnesium loading. Figure 2 It is known that, compared with Comparative Example 1, the surface of the calcium and magnesium loaded biochar adsorbent of Example 1 has randomly opened pores, and a large amount of granular calcium and magnesium are accumulated on the surface.
[0084] 3. Detection of the relative content of elements in calcium and magnesium loaded biochar adsorbent
[0085] The relative contents of elements in the biochar adsorbents prepared in Examples 1-6 and Comparative Examples 1-3 were detected by energy dispersive spectroscopy. The results are shown in Table 1.
[0086] Table 1
[0087] Group / Element (wt%) C O Ca Mg Example 1 53.71 25.08 4.10 17.10 Example 2 74.84 18.58 1.21 5.37 Example 3 73.49 17.26 5.83 3.42 Example 4 60.66 22.11 2.30 14.93 Example 5 53.60 24.08 4.10 18.22 Example 6 59.33 23.41 3.15 14.11 Comparative Example 1 84.22 15.78 / / Comparative Example 2 80.51 16.25 3.24 / Comparative Example 3 72.83 19.31 / 7.86
[0088] It can be seen from Table 1 that calcium and magnesium elements appeared in the biochar adsorbents prepared in Examples 1-6, which once again proves that calcium and magnesium are successfully loaded on biochar. Further analysis shows that the content of calcium and magnesium in the calcium and magnesium loaded biochar adsorbent is positively correlated with the amount of calcium and magnesium added. When the mass ratio of biomass mixture, calcium salt and magnesium salt is 1:0.3:0.3, the content of calcium and magnesium in the calcium and magnesium loaded biochar adsorbent is relatively high, which is 4.10% and 18.22% respectively. This structure also provides a large number of active sites for the adsorption of phosphorus.
[0089] 4. Detection of the specific surface area of calcium and magnesium loaded biochar adsorbent
[0090] The specific surface areas of the biochar adsorbents prepared in Examples 1-6 and Comparative Examples 1-3 were tested using a fully automatic specific surface area analyzer. The results are shown in Table 2.
[0091] Table 2
[0092] Grouping <![CDATA[Specific surface area (m 2 / g)]]> Example 1 141.74 Example 2 170.78 Example 3 151.32 Example 4 180.23 Example 5 135.37 Example 6 127.28 Comparative Example 1 129.56 Comparative Example 2 135.14 Comparative Example 3 175.81
[0093] It can be seen from Table 2 that different calcium and magnesium loadings lead to differences in the specific surface area of the adsorbent.
[0094] 5. Testing the adsorption performance of calcium and magnesium loaded biochar adsorbent on phosphorus
[0095] Prepare phosphate solution: dissolve 878.8 mg potassium dihydrogen phosphate in 1 L water to obtain a phosphate solution with a concentration of 200 mg / L, and set aside;
[0096] 0.02 g of the biochar adsorbent of Examples 1-6 and Comparative Examples 1-3 was added to 40 mL of a phosphate solution with a pH of 7 and a concentration of 200 mg / L, and the solution was shaken at a speed of 220 r / min for 12 h in a constant temperature shaker, and then taken out and filtered. The phosphate concentration in the supernatant was determined by ammonium molybdate spectrophotometry, and the phosphorus equilibrium adsorption capacity of the biochar adsorbent of Examples 1-6 and Comparative Examples 1-3 was calculated. The results are shown in FIG. Figure 4 .
[0097] Figure 4 The following is a graph showing the equilibrium adsorption of phosphorus by the biochar adsorbents of Examples 1-6 and Comparative Examples 1-3. Figure 4It is known that the equilibrium adsorption amount of phosphorus in Example 1 (CMBC) is about 98.6 mg / g, the equilibrium adsorption amount of phosphorus in Example 2 (C1M1BC) is about 61.78 mg / g, the equilibrium adsorption amount of phosphorus in Example 3 (C3M1BC) is about 71.83 mg / g, the equilibrium adsorption amount of phosphorus in Example 4 (C1M3BC) is about 76.66 mg / g, the equilibrium adsorption amount of phosphorus in Example 5 is about 83.58 mg / g, and the equilibrium adsorption amount of phosphorus in Example 6 is about 78.22 mg / g, which is significantly higher than that in Comparative Example 1 (BC, the equilibrium adsorption amount of phosphorus is about 5.80 mg / g), Comparative Example 2 (CBC, the equilibrium adsorption amount of phosphorus is about 34.88 mg / g) and Comparative Example 3 (MBC, the equilibrium adsorption amount of phosphorus is about 46.16 mg / g). It can be seen from the above that calcium and magnesium active sites can improve the affinity of biochar to phosphate.
[0098] 6. Test the adsorption performance of calcium and magnesium loaded biochar adsorbent on low concentration phosphorus
[0099] 0.5 g of the biochar adsorbent of Example 1 was added to 500 mL of phosphate solution with a pH of 7 and concentrations of 1, 3, 5, and 10 mg / L, respectively. The solution was shaken at a speed of 220 r / min for 24 h in a constant temperature shaker, taken out and filtered, and the phosphorus concentration in the supernatant was determined by ammonium molybdate spectrophotometry to simulate the adsorption effect of the adsorbent in the actual treatment of phosphorus-containing wastewater. The results are shown in Table 1. Figure 5 .
[0100] Figure 5 This is a graph showing the adsorption performance of the biochar adsorbent of Example 1 for low concentration phosphorus. Figure 5 It is known that when the initial phosphorus concentration is low (1-5 mg / L), the adsorption equilibrium concentration of the biochar adsorbent of Example 1 is 0.08-0.36 mg / L. GB18918-2002 stipulates that the primary discharge standard of urban sewage treatment plants is 0.5 mg / L. Therefore, the biochar adsorbent of the present invention can be used to remove low-concentration phosphorus.
[0101] When the initial phosphorus concentration is high (10 mg / L), the adsorption equilibrium concentration of the biochar adsorbent of Example 1 is 1.23 mg / L, which is much lower than the secondary discharge standard of urban sewage treatment plants (3 mg / L, GB18918-2002).
[0102] In summary, the biochar adsorbent of the present invention has excellent adsorption performance even at low concentrations and can be used to remove phosphorus in actual wastewater.
[0103] 7. Add calcium and magnesium loaded biochar adsorbent (CMBC-P) after phosphorus adsorption to the soil to explore its effect on crop growth
[0104] The calcium and magnesium loaded biochar adsorbent of Example 1 (CMBC) after the adsorption performance test in Experiment 5 above was dried for later use and recorded as CMBC-P;
[0105] The seeds of Chinese cabbage were sown in soil supplemented with 1% CMBC-P and 1% phosphorus fertilizer. Three repeated experiments were set for each pot test. The germination rate of each group of seeds was counted after germination. After 40 days of cultivation, plant samples were harvested and root morphology was tested. The results are shown in Table 3. Figure 6 .
[0106] Table 3
[0107] Grouping / Indicators Seedling rate (%) Root-shoot ratio Root length (m / g) <![CDATA[Specific surface area per root (cm 2 / g)]]> 1%CMBC-P 93.0±5.77 0.09±0.004 9.66±0.3 43.54±2.2 1% Phosphate Fertilizer 56.3±6.07 0.08±0.007 5.45±0.7 62.0±4.3
[0108] Figure 6 This is a graph showing crop growth after adding calcium and magnesium loaded biochar adsorbent after phosphorus adsorption to the soil. Figure 6 It is known that the growth of pakchoi with CMBC-P is significantly better than that with phosphate fertilizer. It can be seen from Table 3 that the pakchoi with 1% CMBC-P has much higher growth indicators such as germination rate (93%), root-crown ratio (0.09), and specific root length (9.66m / g) than those with 1% phosphate fertilizer. From the above, it can be seen that CMBC-P has good phosphorus slow-release performance, thereby providing more sufficient nutrition for plants. And CMBC-P has high phosphorus utilization efficiency, which may be due to the presence of non-permanent precipitates such as Ca(H2PO4)2, Mg(H2PO4)2, and Mg3(PO4)2, which contributes to better slow-release performance of phosphorus. The above results show that calcium-magnesium loaded biochar adsorbent after phosphorus adsorption can be used as a slow-release phosphorus fertilizer to effectively promote crop growth.
[0109] The above are only preferred embodiments of the present invention, and are not limited to the above examples. For those skilled in the art, various changes and variations are possible under the principle of the present invention. Any modifications and improvements made should be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a calcium and magnesium loaded biochar adsorbent, characterized in that: The following steps are involved: (1) pre-treating the biomass material, mixing it with a strong base, and ball-milling it to obtain a biomass mixture; (2) adding an alcohol solution and a hydrochloric acid solution to the biomass mixture of step (1), adding calcium salt and magnesium salt after ultrasonication, and stirring the reaction to obtain a calcium-magnesium loaded biomass mixture; (3) Under the protection of inert gas, the calcium-magnesium-loaded biomass mixture of step (2) is calcined to obtain a calcium-magnesium-loaded biochar adsorbent.
2. The method for preparing the calcium and magnesium loaded biochar adsorbent according to claim 1, characterized in that: The mass ratio of the biomass mixture, calcium salt and magnesium salt in step (2) is 1:(0.1-0.3):(0.1-0.3), the calcium salt is selected from one or more of calcium chloride, calcium sulfate and calcium hydroxide, and the magnesium salt is selected from one or more of magnesium chloride hexahydrate, magnesium sulfate and magnesium nitrate.
3. The method for preparing the calcium and magnesium loaded biochar adsorbent according to claim 1, characterized in that: The solid-to-liquid ratio of the biomass mixture to the alcohol solution and the hydrochloric acid solution in step (2) is 1:(0.04-0.05):(0.5-1.5), the mass concentration of the hydrochloric acid is 28-35%, the alcohol solution is an anhydrous ethanol solution or a methanol solution, the solvent of the alcohol solution is water, and the volume ratio of anhydrous ethanol or methanol to water in the alcohol solution is 1:(0.05-0.5).
4. The method for preparing the calcium and magnesium loaded biochar adsorbent according to claim 1, characterized in that: The stirring reaction temperature in step (2) is 30-50° C., and the stirring reaction time is 5-10 h.
5. The method for preparing the calcium and magnesium loaded biochar adsorbent according to claim 1, characterized in that: The pretreatment in step (1) is to screen the biomass material, the biomass material is selected from one of coffee grounds, wheat straw, and peanut shells, the mesh size of the screening is 80-100 mesh, the mass ratio of the biomass material to the strong alkali is 1: (0.5-2), and the ball milling time is 1.5-3h.
6. The method for preparing the calcium and magnesium loaded biochar adsorbent according to claim 1, characterized in that: The calcination temperature program in step (3) is to increase the temperature to 550-650°C at a heating rate of 5-10°C / min, and the calcination time is 2-3h.
7. A calcium and magnesium loaded biochar adsorbent, characterized in that: The biochar adsorbent is prepared by the method for preparing the calcium-magnesium loaded biochar adsorbent according to any one of claims 1 to 6.
8. The use of the calcium and magnesium loaded biochar adsorbent as claimed in claim 7, characterized in that: The calcium-magnesium loaded biochar adsorbent is used as a phosphorus adsorbent.
Citation Information
Patent Citations
Calcium-magnesium mineralized biocarbon, and preparation method and application thereof
CN103406099A
Modified biochar s well as preparation method and application thereof
CN110559991A
Modified biochar as well as preparation method and application thereof
CN117416941A